A composite polymeric ferric sulfate and a method for producing the same

By preparing composite polyferric sulfate, the stability and corrosion problems of polyferric sulfate in water treatment were solved by combining ferrous sulfate (a byproduct of titanium dioxide) with modified graphene, phosphorus source and silicic acid, thus achieving a more efficient water treatment effect.

CN120328699BActive Publication Date: 2026-11-24SICHUAN LOMON TITANIUM IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510447646.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-10
Publication Date
2026-11-24
Estimated Expiration
2045-04-10

AI Technical Summary

Technical Problem

Existing polyferric sulfate is prone to precipitating solids during water treatment, exhibits poor stability, and causes severe equipment corrosion, leading to problems such as rusty odor in the water, which affects the actual industrial application effect.

Method used

Using ferrous sulfate, a byproduct of titanium dioxide, as raw material, polyphosphate ferric sulfate is generated by adding sulfuric acid, hydrochloric acid, phosphorus source, and modified graphene. The polyphosphate ferric sulfate is then cured in an ultrasonic environment to prepare composite polyphosphate ferric sulfate, avoiding the introduction of other metal ions into the reaction. Silicic acid and modified graphene are added to improve stability and adsorption capacity.

Benefits of technology

It effectively improves the stability of composite polyferric sulfate, prevents solid precipitation, reduces equipment corrosion, improves water quality, and enhances water treatment efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120328699B_ABST
    Figure CN120328699B_ABST
Patent Text Reader

Abstract

This invention relates to the field of polyferric sulfate technology, and discloses a composite polyferric sulfate and its production method, comprising the following steps: S1, taking ferrous sulfate, a byproduct of titanium dioxide, and preparing a ferrous sulfate solution; S2, adding sulfuric acid and hydrochloric acid to the ferrous sulfate solution, then adding a phosphorus source, stirring, adding hydrogen peroxide to react, generating polyphosphoric ferric sulfate; then adding silicic acid and modified graphene to the polyphosphoric ferric sulfate, placing it in an ultrasonic environment for aging, and obtaining the composite polyferric sulfate; and by mass fraction, the iron content in the composite polyferric sulfate is 9.5-12.5%, the sulfate ion content is 3-5.8%, and the modified graphene content is 2.5-5.5%. The composite polyferric sulfate of this invention, after phosphorus and silicon modification treatment and the introduction of modified graphene, can effectively solve the problem of poor stability caused by the precipitation of solid phases in the polyferric sulfate coagulant over time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyferric sulfate technology, and more specifically, to a composite polyferric sulfate and its production method. Background Technology

[0002] Common inorganic coagulants are mainly divided into traditional aluminum or iron salts, and polymeric coagulants developed based on traditional aluminum or iron salts, such as polyferric sulfate, polyferric chloride, polyaluminum sulfate, and polyaluminum chloride. Compared with traditional aluminum or iron salts, polymeric coagulants have a more outstanding water purification effect and are cheaper than organic polymeric coagulants. Therefore, they have gradually replaced traditional or organic polymeric coagulants and become the mainstream coagulants.

[0003] Among them, polyaluminum ferric chloride sulfate, polyaluminum ferric chloride, and polyaluminum ferric sulfate are all polymeric coagulants that are mainly composed of aluminum salts and supplemented with iron salts. Due to the residual Al in the water... 3+ However, it can cause certain toxic side effects to the environment, which is not conducive to long-term sustainable application and development, and has therefore attracted widespread attention. Polyferric coagulants have excellent coagulation performance, forming large and dense flocs with fast settling speed. They are applicable to a wide range of pH values ​​and water temperatures, and have good removal effects on COD, BOD, color, and heavy metals in various wastewaters. They have no toxic side effects on the environment, and therefore have become a research hotspot for inorganic polymer coagulants.

[0004] For example, patent CN115959756A provides a modified polyferric sulfate and its preparation method. By weight, the modified polyferric sulfate includes the following raw materials: 40-60 parts of pyrite slag, 15-25 parts of sulfuric acid, 1-5 parts of oxidant, 1-10 parts of acetic acid, 10-20 parts of sodium carboxymethyl cellulose and 1-5 parts of stabilizer. It has good removal efficiency and effect on pollutants, and has good basicity, decolorization rate and COD removal rate.

[0005] However, when operators used existing polyferric sulfate for water treatment, they found that as the usage time increased, the polyferric sulfate coagulant was prone to precipitating solids, indicating poor stability. Furthermore, after a period of operation, the equipment showed significant corrosion, back-mixing occurred in the water, and there was a noticeable rusty odor, indicating that the actual industrial water treatment effect was unsatisfactory. Summary of the Invention

[0006] The technical problem to be solved by this invention: In practical applications, it has been found that when using existing polyferric sulfate for water treatment, solid phases tend to precipitate out over time, indicating poor stability. Furthermore, after a period of operation, the equipment exhibits significant corrosion, back-mixing occurs in the water, and there is a noticeable rusty odor, meaning that the actual industrial water treatment effect is unsatisfactory.

[0007] The technical solution adopted in this invention is as follows: This invention provides a method for producing composite polyferric sulfate, comprising the following steps: S1 Take ferrous sulfate, a byproduct of titanium dioxide production, and prepare a ferrous sulfate solution. S2. Add sulfuric acid and hydrochloric acid to ferrous sulfate solution, then add phosphorus source, stir well, add hydrogen peroxide to react and generate polyphosphoric ferric sulfate; then add silicic acid and modified graphene to polyphosphoric ferric sulfate, place in an ultrasonic environment to mature, and obtain the composite polyphosphoric ferric sulfate.

[0008] Preferably, in step S1, the concentration of ferrous sulfate is 135-180 g / L; in step S2, the pH value of the slurry after adding sulfuric acid and hydrochloric acid is controlled to be 3-5.

[0009] Preferably, in step S2, ferrous sulfate solution, concentrated sulfuric acid and hydrochloric acid are used as reaction raw materials, the amount of phosphorus source added is controlled at a phosphorus-iron ratio of 1-1.3:1, the amount of silicic acid added is 3.5-5 times the total mass of the reaction raw materials, and the amount of modified graphene added is 2.5-8% of the total mass of the reaction raw materials.

[0010] Preferably, in step S2, the modified graphene is prepared by the following method: Graphene oxide was placed in ethanol and ultrasonically dispersed to obtain a graphene dispersion. Vinyl POSS and hydrogen peroxide were added to the graphene dispersion, and the mixture was heated under stirring. After cooling, the mixture was dried to obtain the modified graphene.

[0011] Preferably, during the heating reaction, the temperature is first raised to 120-150°C for 20-40 minutes, then raised to 180-250°C, and the reaction is carried out for 1-3 hours.

[0012] Preferably, during cooling, the cooling rate is controlled at 5-20℃ / min.

[0013] Preferably, the ratio of graphene oxide to vinyl POSS by mass is 1-3:1, and the amount of hydrogen peroxide is 0.5-5 wt% of the total mass of graphene oxide and vinyl POSS.

[0014] In the composite polyferric sulfate of this invention, the iron content is 9.5-12.5% ​​by mass fraction, the sulfate ion content is 3-5.8%, and the modified graphene content is 2.5-5.5%.

[0015] The beneficial effects of this invention are as follows: This invention has found that using a single ferric salt as a coagulant can easily cause corrosion to equipment during use. Due to the influence of ferrous ions, backmixing can easily occur at high dosages. Furthermore, water treated with a single ferric salt has a noticeable rusty taste, causing sensory discomfort. Therefore, this invention proposes a silicon- and phosphorus-modified composite polyferric sulfate, which, when used as a coagulant, can alleviate the problems associated with using a single ferric salt.

[0016] Specifically, the composite polyferric sulfate of this invention avoids the introduction of metal ions such as magnesium, sodium, or aluminum during the preparation process, thereby reducing the formation of solid precipitates due to further reactions with other impurity metal ions during use, thus maintaining the stability of the composite polyferric sulfate. Replacing part of the sulfuric acid with hydrochloric acid effectively improves the stability of the polyferric sulfate. By reducing the concentration of certain reaction raw materials, the formation of solid precipitates such as MgFe4(SO4)6(OH)2·20H2O can be prevented, thus avoiding chemical deterioration of the composite polyferric sulfate at the source. Furthermore, the introduction of phosphorus and silicon elements and the addition of modified graphene during the polymerization reaction effectively enhance the adsorption capacity of the composite polyferric sulfate as a water treatment additive, thereby improving its treatment effect and preventing the adsorption and flocculation effects from being affected by the reduction in raw material concentration. Attached Figure Description

[0017] Figure 1 The image shows the XRD pattern of the yellow solid phase precipitated in Comparative Example 1. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0019] This invention provides a composite polyferric sulfate, the production method of which includes the following steps: Ferrous sulfate, a byproduct of titanium dioxide production, is used as a raw material and dissolved in deionized water to prepare a ferrous sulfate solution of approximately 135-180 g / L. Concentrated sulfuric acid and hydrochloric acid are added to the ferrous sulfate solution, with the mass of sulfuric acid being 1.5-2 times the mass of ferrous sulfate. The pH is adjusted to 3-5, and a phosphorus source is added. The mixture is stirred until homogeneous, and then hydrogen peroxide is added. The mixture is stirred to undergo a series of reactions including oxidation, hydrolysis, and polymerization to generate polyphosphoric ferric sulfate. Then, silicic acid and modified graphene are added to the polyphosphoric ferric sulfate, and the mixture is placed in an ultrasonic environment for aging for 5-30 minutes to obtain composite polyferric sulfate. Ferrous sulfate solution, concentrated sulfuric acid, and hydrochloric acid are used as reaction raw materials. The amount of phosphorus source added is controlled at a phosphorus-iron molar ratio of 1-1.3:1. The amount of silicic acid added is 3.5-5 times the total mass of the reaction raw materials, and the amount of modified graphene added is 2.5-8% of the total mass of the reaction raw materials.

[0020] The method for preparing modified graphene in this invention includes the following steps: Take graphene oxide and place it in ethanol. After ultrasonic treatment, a graphene dispersion is formed. Take vinyl POSS and hydrogen peroxide and add them to the graphene dispersion. Under stirring, heat to 120-150℃ for preheating for 20-40 min, then raise the temperature to 180-250℃ and continue the reaction for 1-3 h. Cool slowly at a cooling rate of 5-20℃ / min and dry to obtain modified graphene. The ratio of graphene oxide to vinyl POSS by mass is 1-3:1, and the amount of hydrogen peroxide is 0.5-5 wt% of the total mass of graphene oxide and vinyl POSS.

[0021] The composite polyferric sulfate of the present invention can largely avoid the introduction of H during the preparation process. + Fe 3+ SO4 2 -、OH - The presence of other ions can reduce the further reaction between other metal ions and the polyferric sulfate product, thus reducing the precipitation. In other words, the composite polyferric sulfate in this invention can maintain material and performance stability for a longer period of time during water treatment.

[0022] In the composite polyferric sulfate of this invention, the iron content is 9.5-12.5% ​​by mass fraction, the sulfate ion content is 3-5.8%, and the modified graphene content is 2.5-5.5%.

[0023] Example 1 Step 1: Take about 150.3g of ferrous sulfate, a byproduct of titanium dioxide preparation, and place it in 1L of deionized water to prepare a ferrous sulfate solution with a concentration of 150.3g / L. Then add an equal volume of 98% concentrated sulfuric acid and 1M hydrochloric acid to the ferrous sulfate solution, and control the total mass of sulfuric acid and hydrochloric acid to be 1.6 times the mass of ferrous sulfate. At this time, the pH value of the slurry is measured to be 4.7, which meets the standard of reaction conditions. It can be used as the reaction stock solution for later use.

[0024] Step 2: Add phosphoric acid to the reaction stock solution, with the molar amount of phosphoric acid being 1.2 times that of iron ions. After stirring evenly, add an equal volume of hydrogen peroxide and stir at 120 rpm for 1 hour to allow the above raw materials to undergo a series of complex reactions to form polyphosphoric ferric sulfate.

[0025] Step 3: Add metasilicic acid and modified graphene to polyphosphoric ferric sulfate, with the amount of metasilicic acid being 4.2 times the total mass of the original reaction solution and the amount of modified graphene being 3.6 wt% of the original reaction solution; after mixing, place in an ultrasonic environment and mature for 15 minutes to obtain composite polyphosphoric ferric sulfate.

[0026] The composite polyferric sulfate prepared in this embodiment has a polyferric concentration of 10.5 wt%, and the concentrations of magnesium and sodium are both less than 2.0 wt%, and both are unavoidable impurities from the by-products of the raw material titanium dioxide.

[0027] Example 2 Step 1: Take approximately 151.9g of ferrous sulfate, a byproduct of titanium dioxide preparation, and place it in 1L of deionized water to prepare a ferrous sulfate solution with a concentration of 151.9g / L. Then, add an equal volume of 98% concentrated sulfuric acid and 1M hydrochloric acid to the ferrous sulfate solution, ensuring that the total mass of sulfuric acid and hydrochloric acid is 1.85 times the mass of ferrous sulfate. At this point, the pH value of the slurry is measured to be 3.9, which meets the standard for reaction conditions. This solution can then be used as the stock solution for future use.

[0028] Step 2: Add phosphoric acid to the reaction stock solution, with the molar amount of phosphoric acid being 1.27 times that of iron ions. After stirring evenly, add an equal volume of hydrogen peroxide and stir at 120 rpm for 1 hour to allow the above raw materials to undergo a series of complex reactions to form polyphosphoric ferric sulfate.

[0029] Step 3: Add metasilicic acid and modified graphene to polyphosphoric ferric sulfate, with the amount of metasilicic acid being 4.2 times the total mass of the original reaction solution and the amount of modified graphene being 3.2 wt% of the original reaction solution; after mixing, place in an ultrasonic environment and mature for 15 minutes to obtain composite polyphosphoric ferric sulfate.

[0030] The composite polyferric sulfate prepared in this embodiment has a polyferric concentration of 11.33 wt%, and the concentrations of magnesium and sodium are both less than 2.0 wt%, and both are unavoidable impurities from the by-products of the raw material titanium dioxide.

[0031] Example 3 Step 1: Take about 152.0g of ferrous sulfate, a byproduct of titanium dioxide preparation, and place it in 1L of deionized water to prepare a ferrous sulfate solution with a concentration of 152.0g / L. Then add an equal volume of 98% concentrated sulfuric acid and 1M hydrochloric acid to the ferrous sulfate solution, ensuring that the total mass of sulfuric acid and hydrochloric acid is twice the mass of ferrous sulfate. At this point, the pH value of the slurry is measured to be 3.4, which meets the standard for reaction conditions. This solution can then be used as the stock solution for later use.

[0032] Step 2: Add phosphoric acid to the reaction stock solution, with the molar amount of phosphoric acid being 1 times that of iron ions. After stirring evenly, add an equal volume of hydrogen peroxide and stir at 10 rpm for 1 hour to allow the above raw materials to undergo a series of complex reactions to form polyphosphoric ferric sulfate.

[0033] Step 3: Add metasilicic acid and modified graphene to polyphosphoric ferric sulfate, with the amount of metasilicic acid being 4.2 times the total mass of the original reaction solution and the amount of modified graphene being 2.9 wt% of the original reaction solution; after mixing, place in an ultrasonic environment and mature for 15 minutes to obtain composite polyphosphoric ferric sulfate.

[0034] The composite polyferric sulfate prepared in this embodiment has a polyferric concentration of 11.02 wt%, and the concentrations of magnesium and sodium are both less than 2.0 wt%, and both are unavoidable impurities from the by-products of the raw material titanium dioxide.

[0035] Comparative Example 1 Step 1: Take about 150.5g of ferrous sulfate, a byproduct of titanium dioxide preparation, and place it in 1L of deionized water to prepare a ferrous sulfate solution with a concentration of 150.5g / L. Then add magnesium sulfate to the ferrous sulfate solution, ensuring that the mass of magnesium sulfate is 1.2 times the mass of ferrous sulfate. At this point, the pH value of the slurry is measured to be 3.1, which meets the standard for reaction conditions. This solution can then be used as the stock solution for later use.

[0036] Step 2: Add an equal volume of sodium chloride to the reaction stock solution and stir at 120 rpm for 1 hour to allow the above raw materials to undergo a series of complex reactions to form polyferric sulfate.

[0037] The composite polyferric sulfate prepared in this embodiment has a polyferric concentration of 18.06 wt%, a magnesium concentration of 11.31 wt%, and a sodium concentration of 11.58 wt%.

[0038] Test case Samples: Examples 1-3, Comparative Example 1 (1) Stability observation The polyferric sulfate products prepared in Examples 1 to 3 and Comparative Example 1 were used as samples and placed in storage bags for 30 days. The morphological changes of the samples before and after storage were then observed. Observation revealed that the composite polyferric sulfate in Examples 1 to 3 showed essentially no difference in morphology before and after storage, while the sample in Comparative Example 1, compared to before storage, produced a noticeable yellow solid precipitate after storage. Therefore, it can be concluded that the composite polyferric sulfate in Examples 1 to 3 has stronger stability.

[0039] (2) Solid phase analysis The content relationships of substances in the polyferric salt sample prepared in Comparative Example 1 were determined, and the results are summarized in Table 2 below: Table 2 Results of the determination of the content relationship of substances in Comparative Example 1

[0040] The sample was then allowed to stand for 30 days, after which a distinct yellow solid phase was observed to precipitate. The solid phase was washed with ethanol, dried, and then subjected to X-ray diffraction analysis. The XRD pattern of the solid phase is shown below. Figure 1 As shown, by Figure 1 It can be concluded that the main component of the solid phase is MgFe4(SO4)6(OH)2·20H2O.

[0041] The above analysis demonstrates that the solid phase produced during the use of traditional polyferric salt coagulants is due to the magnesium content in the raw materials. This invention, through modification with phosphorus and silicon and the introduction of modified graphene, not only reduces the oxidation of ferric salts in the aquatic environment but also helps maintain the stability of the polyferric salt coagulant. Furthermore, by controlling the dosage of each element and environmental conditions, the material properties of the polyferric salt are further stabilized, enabling its long-term and stable application in water treatment processes.

[0042] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for producing composite polyferric sulfate, characterized in that, Includes the following steps: S1 Take ferrous sulfate, a byproduct of titanium dioxide production, and prepare a ferrous sulfate solution. S2. Add sulfuric acid and hydrochloric acid to ferrous sulfate solution, then add phosphorus source, stir well, add hydrogen peroxide to react and generate polyphosphoric ferric sulfate; then add silicic acid and modified graphene to polyphosphoric ferric sulfate, place in an ultrasonic environment to mature, and obtain the composite polyphosphoric ferric sulfate. In step S2, ferrous sulfate solution, concentrated sulfuric acid, and hydrochloric acid are used as reaction raw materials. The amount of phosphorus source added is controlled at a phosphorus-to-iron ratio of 1-1.3:

1. The amount of silicic acid added is 3.5-5 times the total mass of the reaction raw materials, and the amount of modified graphene added is 2.5-8% of the total mass of the reaction raw materials. In step S2, the modified graphene is prepared as follows: Graphene oxide was placed in ethanol and ultrasonically dispersed to obtain a graphene dispersion. Vinyl POSS and hydrogen peroxide were added to the graphene dispersion, and the mixture was heated under stirring. After cooling, the mixture was dried to obtain the modified graphene.

2. The method for producing composite polyferric sulfate according to claim 1, characterized in that, In step S1, the concentration of ferrous sulfate is 135-180 g / L; in step S2, the pH value of the slurry after adding sulfuric acid and hydrochloric acid is controlled to be 3-5.

3. The method for producing composite polyferric sulfate according to claim 1, characterized in that, During the heating reaction, first heat to 120-150℃, preheat for 20-40 minutes, then raise the temperature to 180-250℃ and react for 1-3 hours.

4. The method for producing composite polyferric sulfate according to claim 1, characterized in that, During cooling, the cooling rate should be controlled at 5-20℃ / min.

5. The method for producing composite polyferric sulfate according to claim 1, characterized in that, The ratio of graphene oxide to vinyl POSS by mass is 1-3:1, and the amount of hydrogen peroxide is 0.5-5 wt% of the total mass of graphene oxide and vinyl POSS.

6. The composite polyferric sulfate prepared by the production method according to any one of claims 1 to 5, characterized in that, By mass fraction, the iron content is 9.5-12.5%, the sulfate ion content is 3-5.8%, and the modified graphene content is 2.5-5.5%.

Citation Information

Patent Citations

  • Modified polyferric sulfate and preparation method thereof

    CN115959756A

  • Mixed sewage treating agent and preparation method thereof

    CN106517382A

  • Preparation method of inorganic modified polymeric ferric sulfate

    CN113371762A

  • Water-swelling acrylic gel material and preparation method thereof

    CN118772325A