A nano-porous titanium material, a preparation method thereof and application thereof in preparing a titanium abutment for implants
By forming a nanoporous titanium oxide coating on the surface of titanium materials, the problem of poor performance of smooth titanium abutment materials in peri-implant inflammatory response was solved, achieving high hardness and anti-inflammatory effects that promote soft tissue integration, thereby improving the integration capacity of implants.
Patent Information
- Application Number
- CN202510538746.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-04-27
AI Technical Summary
Existing smooth titanium abutment materials are not effective in treating peri-implant inflammatory responses, and the nanotube structure reduces the material's hardness, making it difficult to meet the requirements for implantation.
By forming a titanium oxide coating with a nanoporous structure on the surface of titanium material, and then using anodizing and annealing treatment with a DC voltage of <40V, the microstructure is optimized to improve hardness, while also possessing a biomimetic coating that has anti-inflammatory properties and promotes soft tissue integration.
It achieves high hardness and excellent anti-inflammatory effect at the implant perforation site, improves the soft tissue integration capacity of the implant, and solves the problem of peri-implant inflammatory response.
Smart Images

Figure CN120330840B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of biomimetic materials technology, specifically relating to a nanoporous titanium material, its preparation method, and its application in the preparation of titanium implant abutments. Background Technology
[0002] Clinically, titanium is a common material used to construct the perigender contour of implants, whether as the transgingival portion of soft tissue-level implants or the superstructure abutment of bone-level implants. When this portion experiences an inflammatory response caused by microorganisms, it leads to peri-implant disease. Severe peri-implant disease can cause irreversible resorption of the surrounding bone tissue, i.e., peri-implantitis, ultimately resulting in implant loosening and failure.
[0003] Studies show that smooth titanium abutments, compared to rough microstructures, can inhibit bacterial adhesion in the early stages of plaque biofilm formation. Therefore, polishing processes are currently used to create smooth microstructures in clinical titanium abutments. However, epidemiological surveys show that approximately 20% of dental implant patients and about 10% of implant sites still experience peri-implantitis. This indicates that simply creating a smooth titanium abutment cannot prevent peri-implantitis; further optimizing the transgingival titanium abutment to improve soft tissue integration (STI) is a crucial issue that urgently needs to be addressed.
[0004] Since the discovery that anodizing can construct nanoscale tubular arrays on titanium surfaces, these intricate nanomorphic structures have attracted considerable attention due to their simple and economical fabrication process and controllable nanoscale dimensions. Recent studies have shown that titanium dioxide nanotubes (TiO2 nanotubes, TNT) can suppress inflammatory responses by modulating macrophage polarization. Compared to smooth titanium surfaces, nanotube-modified titanium surfaces, under LPS-induced inflammatory conditions, can alleviate macrophage immune inflammatory responses by reducing the release of pro-inflammatory mediators (TNF-α, MCP-1, NO), indicating that nanostructured surfaces exhibit better tolerance in microenvironments with a risk of bacterial contamination.
[0005] Although nanotube structures can interfere with the soft tissue integration capacity around implants by influencing the inflammatory fibrous complex, their unique tubular structure significantly reduces the material's rigidity, making them unsuitable for implant placement. Summary of the Invention
[0006] The purpose of this invention is to provide a nanoporous titanium material, its preparation method, and its application in the preparation of implant titanium abutments. The nanoporous titanium material prepared by this invention has excellent hardness properties, meeting the requirements of implant titanium abutments; at the same time, it can achieve excellent anti-inflammatory and soft tissue integration effects.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] This invention provides a method for preparing nanoporous titanium materials, comprising the following steps:
[0009] Titanium material is placed in an electrolyte as an anode, and anodizing treatment is performed on the titanium material using a two-electrode system to obtain anodized titanium material. The anodizing treatment is performed using a DC voltage, wherein the DC voltage is <40V.
[0010] The anodized titanium material is annealed to obtain the nanoporous titanium material, the surface of which has a titanium oxide coating with a nanoporous structure.
[0011] Preferably, the electrolyte comprises ammonium fluoride, water, and ethylene glycol; the mass percentage of ammonium fluoride in the electrolyte is 0.1-0.5%; and the volume percentage of water in the electrolyte is 1-4%.
[0012] Preferably, the DC voltage is 10 to 30V.
[0013] Preferably, the anodizing treatment time is 20 to 40 minutes.
[0014] Preferably, the cathode of the two-electrode system is a carbon rod; and the titanium material is titanium foil.
[0015] Preferably, the annealing temperature is 450–550°C, and the holding time is 1–3 hours.
[0016] Preferably, the heating rate of the annealing treatment is 1 to 5 °C / min.
[0017] Preferably, the average pore size of the nanoporous structure is 40–80 nm; and the thickness of the titanium oxide coating is 1–3 μm.
[0018] The present invention provides a nanoporous titanium material prepared by the preparation method described above, wherein the surface of the nanoporous titanium material has a titanium oxide coating with a nanoporous structure.
[0019] This invention provides the application of the nanoporous titanium material described in the above technical solution in the preparation of titanium implant abutments.
[0020] This invention provides a method for preparing nanoporous titanium materials, comprising the following steps: placing titanium material as the anode in an electrolyte, performing anodizing treatment on the titanium material using a two-electrode system to obtain anodized titanium material, wherein the anodizing treatment is performed using a DC voltage < 40V; and annealing the anodized titanium material to obtain the nanoporous titanium material, wherein the surface of the nanoporous titanium material has a nanoporous titanium oxide coating. This invention controls the DC voltage of the anodizing treatment, thereby obtaining a nanoporous structure on the surface of the titanium material through anodizing, and the resulting nanoporous titanium oxide coating can serve as a biomimetic coating. Simultaneously, this invention optimizes the microstructure of the anodized titanium material through annealing, improving the mechanical properties (hardness) of the nanoporous titanium material. Therefore, the nanoporous titanium material prepared by this invention, while meeting the working strength requirements of the implant abutment at the gingival perforation site, achieves anti-inflammatory and soft tissue integration effects due to its nanoporous biomimetic coating, thereby further improving the implant's structural integrity (STI). Attached Figure Description
[0021] Figure 1 The image shows a surface electron microscope (SEM) image (×10k) of the nanoporous titanium material prepared in Example 1 of this invention.
[0022] Figure 2 The image shows a surface electron microscope (SEM) image (×30k) of the nanoporous titanium material prepared in Example 1 of this invention.
[0023] Figure 3 The image shows a surface electron microscope (SEM) image (×100k) of the nanoporous titanium material prepared in Example 1 of this invention.
[0024] Figure 4 The AFM-roughness characterization results are for the nanoporous titanium material prepared in Example 1 of this invention.
[0025] Figure 5 This is a surface electron microscope image of the nanotube titanium material prepared in Comparative Example 1 of this invention;
[0026] Figure 6 These are the test results of the real-time quantitative polymerase chain reaction in this invention. Detailed Implementation
[0027] This invention provides a method for preparing nanoporous titanium materials, comprising the following steps:
[0028] Titanium material is placed in an electrolyte as an anode, and anodizing treatment is performed on the titanium material using a two-electrode system to obtain anodized titanium material. The anodizing treatment is performed using a DC voltage, wherein the DC voltage is <40V.
[0029] The anodized titanium material is annealed to obtain the nanoporous titanium material, the surface of which has a titanium oxide coating with a nanoporous structure.
[0030] In this invention, unless otherwise specified, all raw materials / components used in the preparation are commercially available products well known to those skilled in the art.
[0031] This invention uses titanium material as the anode in an electrolyte and employs a two-electrode system to perform anodizing treatment on the titanium material, obtaining anodized titanium material. The anodizing treatment is performed using a direct current voltage (DC) < 40V. In this invention, the titanium material is preferably titanium foil. Before the anodizing treatment, the titanium material is preferably pre-cleaned, preferably by ultrasonic cleaning sequentially with acetone, ethanol, and water. The water is preferably deionized water. This invention does not have specific requirements for the specific implementation of the ultrasonic cleaning, as long as the pre-cleaning treatment removes oil and dirt from the surface of the titanium material.
[0032] In this invention, the cathode of the two-electrode system is preferably a carbon rod. The electrolyte preferably comprises ammonium fluoride, water, and ethylene glycol, with the water preferably being deionized water. The mass percentage of ammonium fluoride in the electrolyte is preferably 0.1-0.5%, and in the examples, it can be 0.3%. The volume percentage of water in the electrolyte is preferably 1-4%, and in the examples, it can be 2%. The DC voltage is preferably 10-30V, and in the examples, it can be 20V. This invention optimizes the DC voltage of the anodizing treatment and, by preferably using hydrogen fluoride to prepare the electrolyte and optimizing the volume percentage of water in the electrolyte, successfully forms nanopores on the surface of the titanium material. These nanopores are pit-like porous structures obtained on the surface of the titanium material through anodizing treatment, rather than nanotubes.
[0033] In this invention, the anodizing treatment time is preferably 20 to 40 minutes, more preferably 30 minutes.
[0034] After obtaining the anodized titanium material, the present invention anneals the anodized titanium material to obtain the nanoporous titanium material, the surface of which has a titanium oxide coating with a nanoporous structure. In this invention, the annealing is preferably performed in an air atmosphere. The heating rate of the annealing is preferably 1–5 °C / min, and in the embodiment, it can be 3 °C / min. The annealing temperature is preferably 450–550 °C, and in the embodiment, it can be 500 °C. The holding time of the annealing is preferably 1–3 h, and in the embodiment, it can be 2 h.
[0035] In this invention, the average pore size of the nanopore structure is preferably 40-80 nm, and in the embodiments it can be 60 nm.
[0036] In this invention, the thickness of the titanium oxide coating is preferably 1 to 3 μm, and in the embodiment it can be 2 μm.
[0037] The present invention provides a nanoporous titanium material prepared by the preparation method described above, wherein the surface of the nanoporous titanium material has a titanium oxide coating with a nanoporous structure.
[0038] In this invention, the nanoporous titanium material is titanium dioxide.
[0039] In this invention, the average pore size of the nanopore structure is preferably 40-80 nm, and in the embodiments it can be 60 nm.
[0040] In this invention, the thickness of the titanium oxide coating is preferably 1 to 3 μm, and in the embodiment it can be 2 μm.
[0041] This invention provides the application of the nanoporous titanium material described in the above technical solution in the preparation of titanium implant abutments.
[0042] In this invention, the implant titanium abutment is specifically the titanium abutment of the transgingival portion.
[0043] To further illustrate the present invention, the technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0044] Example 1
[0045] This embodiment provides a method for preparing nanoporous titanium material, specifically including the following steps:
[0046] Pure titanium foil (1cm×1cm×0.2mm) was ultrasonically cleaned sequentially with acetone, ethanol and deionized water to remove oil stains.
[0047] The electrolyte was prepared by dissolving deionized water and ammonium fluoride (NH4F) in ethylene glycol. The volume percentage of deionized water in the electrolysis was 2%, and the mass percentage of ammonium fluoride (NH4F) was 0.3%. A carbon rod was used as the cathode, and cleaned pure titanium foil was used as the anode. Anodizing was performed at a DC voltage of 20V for 30 minutes to obtain the anodized titanium foil.
[0048] Then, the anodized titanium foil was annealed in air at 500°C for 2 hours at a heating rate of 4°C / min, and then naturally cooled in the furnace to obtain the annealed titanium foil.
[0049] Annealed titanium foil was ultrasonically cleaned sequentially with acetone, ethanol and deionized water to obtain nanoporous titanium material (TNP).
[0050] The nanoporous titanium material prepared in this embodiment is titanium dioxide material. The surface of the nanoporous titanium material prepared in this embodiment has a titanium dioxide coating with a nanoporous structure, and the average pore size of the nanoporous structure is 60 nm.
[0051] Comparative Example 1
[0052] This comparative example provides a method for preparing nanotube titanium material, specifically including the following steps:
[0053] Pure titanium foil (1cm×1cm×0.2mm) was ultrasonically cleaned sequentially with acetone, ethanol and deionized water to remove oil stains.
[0054] The electrolyte was prepared by dissolving deionized water and ammonium bifluoride (NH4HF2) in ethylene glycol. The volume percentage of deionized water in the electrolysis was 5%, and the mass percentage of ammonium bifluoride (NH4HF2) was 0.3%. A carbon rod was used as the cathode, and cleaned pure titanium foil was used as the anode. Anodizing was performed at a DC voltage of 40V for 30 minutes to obtain the anodized titanium foil.
[0055] Then, the anodized titanium foil was annealed in air at 500°C for 2 hours at a heating rate of 4°C / min, and then naturally cooled in the furnace to obtain the annealed titanium foil.
[0056] The annealed titanium foil was ultrasonically cleaned sequentially with acetone, ethanol and deionized water to obtain titanium nanotube material (TNT).
[0057] The nanotube titanium material prepared in this comparative example is titanium dioxide material. The surface of the nanotube titanium material prepared in this comparative example has a titanium dioxide coating with a nanotube structure, and the average pore size of the nanotube structure is 60 nm.
[0058] Test case
[0059] (1) SEM testing
[0060] Figure 1 The surface electron microscope image (×10k) of the nanoporous titanium material prepared in Example 1; Figure 2 Surface electron microscope image (×30k) of the nanoporous titanium material prepared in Example 1; Figure 3 The image shows a surface electron microscope (SEM) image (×100k) of the nanoporous titanium material prepared in Example 1. Figure 1 , Figure 2 and Figure 3As shown, in Example 1, nanoporous titanium material was successfully prepared by anodizing and annealing. The surface of the nanoporous titanium material has a titanium oxide coating with a nanoporous structure.
[0061] Figure 5 This is a surface electron microscope (SEM) image of the titanium nanotube material prepared in Comparative Example 1. Figure 5 It can be seen that Comparative Example 1 was able to successfully prepare nanotube structures by controlling the conditions of the anodic oxidation process.
[0062] (2) AFM test
[0063] The surface morphology of the pure titanium foil (Ti) used in Example 1 and the prepared nanoporous titanium material (TNP) was tested using atomic force microscopy (AFM). The test results are as follows: Figure 4 As shown, Figure 4 The left image shows the surface roughness test results for pure titanium foil (Ti) and nanoporous titanium material (TNP). Figure 4 The middle image shows the surface morphology of pure titanium foil (Ti). Figure 4 The right image in the image shows the surface morphology of nanoporous titanium (TNP) material. Figure 4 It can be seen that the surface roughness of the nanoporous titanium material (TNP) prepared in Example 1 is significantly increased. The test data of the surface roughness of the pure titanium foil (Ti) used in Example 1 and the prepared nanoporous titanium material (TNP) are shown in Table 1.
[0064] Table 1 Surface roughness of pure titanium foil and nanoporous titanium materials
[0065] Group Ti TNP 1 16 23 2 13.7 24.8 3 12.7 21.5 4 12.6 33.1 5 13.4 23.6 6 5.51 25.7 7 8.66 24.1 8 9.85 46.1 9 7.44 27.1 average value 11.09555556 27.66666667 Standard deviation 3.21506216 7.23248843
[0066] (3) LDH cytotoxicity test
[0067] Cell viability was assessed 1 day after cell seeding using an LDH assay kit: macrophages were seeded at a concentration of 1×10⁶ cells / day. 5 The sample was seeded onto the surface of a 24-well plate and incubated for 24 hours. After washing three times with PBS for 5 minutes each, 500 μL of diluted LDH release reagent was added to each well. After incubation for 1 hour, the supernatant was transferred to a 96-well plate, and the prepared LDH detection working solution was added. The plate was incubated at room temperature in the dark for 30 minutes. The OD value was measured at 490 nm using a microplate reader. Cell viability was calculated using ((experimental group OD value - blank OD value) / (control cell OD value - blank OD value)) × 100%. The LDH cytotoxicity test results are shown in Table 2. Table 2 shows the LDH cytotoxicity test results of the pure titanium foil (Ti) used in Example 1 and the prepared nanoporous titanium material (TNP).
[0068] Table 2 Results of LDH cytotoxicity assay
[0069]
[0070]
[0071] (4) Real-time quantitative polymerase chain reaction (qRT-PCR)
[0072] Macrophages were 1×10 5 The cells were seeded onto the surface of a 24-well plate and cultured for 3 days. After digestion and centrifugation, the supernatant was removed, and total RNA was extracted from macrophages using a total RNA extraction kit, following the manufacturer's instructions. RNA purity and concentration were determined using a NanoDrop 2000 UV-Vis spectrophotometer. cDNA was then synthesized according to the FastKing RT Kit (containing gDNase). The obtained cDNA was amplified using MagicSYBR buffer (Beijing Kangwei Century Biotechnology Co., Ltd., China) in a real-time quantitative PCR system. The results were then analyzed using CFXConnect. TM The expression level of the target gene mRNA was determined using a real-time quantitative PCR detection system (Bio-Rad Laboratories, USA) with GAPDH as an internal control. The primer sequences are shown in Table 3.
[0073] Table 3 Primer sequences designed
[0074]
[0075]
[0076] The results of the real-time quantitative polymerase chain reaction (qRT-PCR) test are shown in Table 4 and Figure 6 As shown in Table 4 and Figure 6 The results of PCR tests are for the pure titanium foil (Ti) used in Example 1 and the prepared nanoporous titanium material (TNP).
[0077] Table 4. PCR test results
[0078]
[0079] From Table 4 and Figure 6 The results show that RT-qPCR was used to detect the expression of pro-inflammatory and anti-inflammatory genes. Figure 6As shown in Table 4, there was no significant difference in the expression of the M0 marker (CD68) in macrophages cultured on Ti and TNP surfaces. However, the expression of the M1 marker (CD86) was significantly decreased in macrophages cultured on TNP surfaces, a trend also observed in pro-inflammatory cytokines (TNF-α, iNOS, IL-1β). Conversely, the expression of the M2 marker (CD206) was increased in macrophages cultured on TNP surfaces, and the expression of the anti-inflammatory cytokine TGF-β was also significantly increased.
[0080] (5) Transcriptome sequencing - inflammation-related genes
[0081] Macrophages were 1×10 5 After seeding samples onto the surface of 24-well plates and culturing for 3 days, total RNA from macrophages was extracted using TRIzol reagent according to the manufacturer's protocol. The quality and purity of the RNA samples were assessed by agarose gel electrophoresis, NanoPhotometer spectrophotometer, and Agilent 2100 bioanalyzer. Library construction and sequencing were performed by Shanghai Weihuan Biotechnology Co., Ltd. using an Illumina PE150. Clean reads were precisely aligned to the reference genome using HISAT2 software. Differential gene analysis between the control and reference genomes was performed using DESeq2, with p-value <0.05, and fold change >1.5 or <0.667 considered significant. Gene ontology (GO) analysis and Kyoto Encyclopedia of Genetics and Genomes (KEGG) pathway analysis were performed using clusterProfiler software.
[0082] Experimental Conclusions: RNA sequencing and enrichment analysis revealed that biological processes and cellular components related to "cell projection membrane," "postsynaptic membrane," "focal adhesion," "actin binding," and "collagen trimer" attracted the attention of this invention. These are closely related to the interaction between the extracellular matrix, cell membrane, and cytoskeleton. This suggests that the mechanism by which the nanoporous titanium material prepared in Example 1 induces polarization in human macrophages may be related to changes in cell morphology and the cytoskeleton. Transcriptome sequencing and enrichment analysis of inflammation-related genes are shown in Table 5. The genes in Table 5 can be found in the National Center for Biotechnology Information (NCBI). Table 5 includes some common anti-inflammatory and pro-inflammatory genes. As shown in Table 5, the nanoporous material prepared in Example 1 upregulated inflammation-inhibiting genes and downregulated inflammation-promoting genes.
[0083] Table 5. Enrichment analysis results of transcriptome sequencing-inflammation-related genes.
[0084]
[0085]
[0086] (6) Contact angle surface energy test
[0087] The contact angle and surface energy of the pure titanium foil (Ti) used in Example 1 and the prepared nanoporous titanium material (TNP) were tested, and the test results are shown in Tables 6 and 7.
[0088] Table 6. Test results of surface energy at the contact angle of Ti
[0089]
[0090] Table 7. Contact Angle Surface Energy Test Results of TNP
[0091]
[0092] (7) Nanoindentation test
[0093] The pure titanium foil (Ti) used in Example 1 and the prepared nanoporous titanium material (TNP) were subjected to nanoindentation testing. The testing tool used was a nanoindenter. The two core indicators of nanoindentation testing were hardness and elastic modulus. The testing method was as follows: a nanoindenter was pressed into the surface of the material, and then the hardness value of the material was calculated according to the formula (H = Pmax / Ac), where Pmax is the maximum indentation load and Ac is the contact area between the indenter and the material.
[0094] Table 8 provides hardness data for pure titanium foil (Ti) and nanoporous titanium material (TNP), and Table 9 provides elastic modulus data for pure titanium foil (Ti) and nanoporous titanium material (TNP).
[0095] Table 8. Hardness (GPa) Test Results of Ti and TNP
[0096]
[0097]
[0098] Table 9. Elastic modulus (in GPa) test results for Ti and TNP
[0099] Group Ti TNP 1 24.651075 10.630022 2 25.534692 9.162794 3 25.27606 10.64469 4 24.603748 10.417961 5 25.673361 10.084437 average value 25.1477872 10.1879808 Standard deviation 0.443864555 0.551108683
[0100] (8) Mechanical property testing
[0101] Nanoindentation tests were performed on the nanoporous titanium material (TNP) prepared in Example 1 and the nanotube titanium material (TNT) prepared in Comparative Example 1. A nanoindenter was used as the testing tool. The two core indicators of the nanoindentation test were hardness and elastic modulus. The testing method involved pressing a nanoindenter into the material surface, and then calculating the hardness value of the material according to the formula (H = Pmax / Ac), where Pmax is the maximum indentation load and Ac is the contact area between the indenter and the material. The test results are shown in Table 10.
[0102] Table 10. Mechanical property test results of nanoporous titanium materials and nanotube titanium materials
[0103] Group Hardness GPa Elastic modulus GPa TNP 1.59±0.14 10.18±0.55 TNT 0.92±0.27 12.35±1.34
[0104] The anodizing parameters for preparing nanoporous titanium materials (TNP) and nanotube titanium materials (TNT) in Example 1 and Comparative Example 1 are shown in Table 10. As can be seen from Table 10, this invention can successfully prepare nanoporous titanium materials by controlling the DC voltage of the anodizing process. Moreover, the hardness performance of the prepared nanoporous titanium materials is superior to that of the nanotube titanium materials prepared in Comparative Example 1.
[0105] Table 11 Operating parameters of anodic oxidation treatment in Example 1 and Comparative Example 1
[0106]
[0107]
[0108] As demonstrated by the above embodiments, this invention controls the DC voltage of the anodizing process to obtain a nanoporous structure on the surface of titanium material through anodizing. The resulting nanoporous titanium oxide coating can serve as a biomimetic coating. Simultaneously, this invention optimizes the microstructure of the anodized titanium material through annealing, improving the mechanical properties (hardness) of the nanoporous titanium material. Therefore, the nanoporous titanium material prepared by the method provided by this invention, while meeting the working strength requirements of the implant abutment at the gingival perforation site, achieves anti-inflammatory and soft tissue integration-promoting effects due to its biomimetic nanoporous coating. This further enhances the STI (Surgical Integration Therapy) effect of the implant.
[0109] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. The application of a nanoporous titanium material in the fabrication of titanium implant abutments, characterized in that, The surface of the nanoporous titanium material has a titanium oxide coating with a nanoporous structure. The preparation method of the nanoporous titanium material includes the following steps: Titanium material was placed as the anode in an electrolyte, and anodizing was performed on the titanium material using a two-electrode system to obtain anodized titanium material. The anodizing process was carried out using a DC voltage of 20V. The electrolyte included ammonium fluoride, water, and ethylene glycol. The mass percentage of ammonium fluoride in the electrolyte was 0.3%, and the volume percentage of water in the electrolyte was 2%. The anodizing time was 30 minutes. The cathode of the two-electrode system was a carbon rod, and the titanium material was titanium foil. The anodized titanium material is annealed at a temperature of 450-550°C for 1-3 hours to obtain the nanoporous titanium material, the surface of which has a titanium oxide coating with a nanoporous structure.
2. The application according to claim 1, characterized in that, The heating rate of the annealing process is 1~5℃ / min.
3. The application according to claim 1, characterized in that, The average pore size of the nanoporous structure is 40~80nm; the thickness of the titanium oxide coating is 1~3μm.
Citation Information
Patent Citations
Preparation method for obtaining nano structure with micro-nano morphology through nano treatment of pure titanium surface and application thereof
CN119145020A