High flame retardant aluminum alloy photovoltaic cable and preparation method thereof

By introducing expanded graphite and modified montmorillonite into aluminum alloy photovoltaic cables, combined with a specific ratio of polyethylene and crosslinking agents, the problems of insufficient flame retardancy and mechanical properties of aluminum alloy photovoltaic cables have been solved, and cables with high efficiency, flame retardancy and stable performance have been prepared.

CN120388794BActive Publication Date: 2026-11-20YUNNAN JULI CABLE MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510543687.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-28
Publication Date
2026-11-20
Estimated Expiration
2045-04-28

AI Technical Summary

Technical Problem

Existing aluminum alloy photovoltaic cables have shortcomings in terms of flame retardancy, environmental protection, and mechanical properties. Traditional flame retardants pose environmental pollution risks, and inorganic flame retardants require high filling amounts, leading to performance degradation. Nitrogen-phosphorus flame retardants have poor compatibility and are prone to failure.

Method used

A highly flame-retardant aluminum alloy photovoltaic cable was prepared by constructing an efficient flame-retardant system using expanded graphite and modified montmorillonite, combined with a specific ratio of polyethylene and crosslinking agent, and through melt blending, molding and cold pressing processes.

Benefits of technology

It achieves high flame retardancy and excellent mechanical properties, ensuring stable use of cables in harsh environments and avoiding the environmental pollution risks of traditional flame retardants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application discloses a kind of high flame-retardant aluminum alloy photovoltaic cables and preparation method thereof, it is related to cable technical field.The preparation method of the high flame-retardant aluminum alloy photovoltaic cable includes the following steps: step 1: ethylene-vinyl acetate copolymer, polyethylene, expanded graphite, modified montmorillonite, initiator, crosslinking agent, additive are mixed, melt blending, moulding, cold pressing, and outer sheath is obtained;Step 2: aluminum alloy is used as wire core, and oxygen barrier layer, insulating layer are wrapped, and basic wire core is obtained;The basic wire core is combined, and mineral fireproof material is filled, and the outer sheath is wrapped, and the high flame-retardant aluminum alloy photovoltaic cable is obtained.The prepared high flame-retardant aluminum alloy photovoltaic cable guarantees mechanical properties while having high flame retardancy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cable technology, specifically to a high flame-retardant aluminum alloy photovoltaic cable and its preparation method. Background Technology

[0002] In recent years, with the global emphasis on renewable energy, photovoltaic power generation technology has developed rapidly, and the large-scale construction of photovoltaic power plants has placed higher demands on the performance of supporting cables. As a key transmission component of photovoltaic systems, photovoltaic cables need to be exposed to complex outdoor environments for extended periods, enduring harsh conditions such as ultraviolet radiation, high temperatures, and humidity. Therefore, they must possess excellent weather resistance, high flame retardancy, and stable mechanical properties. Among these, aluminum alloy photovoltaic cables have become an ideal choice for photovoltaic systems due to their outstanding resistance to high and low temperatures and long service life. However, traditional aluminum alloy cables still have shortcomings in the synergistic optimization of flame retardancy, environmental friendliness, and mechanical properties.

[0003] Currently, most flame-retardant cables on the market use halogenated flame retardants (such as PVC). Although these offer good flame retardant performance, they release toxic gases such as dioxins during combustion, polluting the environment and potentially endangering personnel safety. Furthermore, the flame retardancy of ordinary aluminum alloy cables still needs further improvement; higher flame retardancy better meets the safety requirements of high-density wiring in photovoltaic power plants. While inorganic flame retardants such as aluminum hydroxide are environmentally friendly, they require high filler content (>60%) to achieve the V-0 standard, which significantly reduces the cable's mechanical and processing properties, impacting practical applications. Nitrogen-phosphorus synergistic flame retardants, although highly efficient, suffer from poor compatibility with the substrate and are prone to migration and failure. Their flame retardant performance may degrade over long-term use, affecting the cable's mechanical properties as well.

[0004] In conclusion, solving the above problems and developing a high flame-retardant aluminum alloy photovoltaic cable is of great significance. Summary of the Invention

[0005] The purpose of this invention is to provide a high flame-retardant aluminum alloy photovoltaic cable and its preparation method, so as to solve the problems mentioned in the background art.

[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: A method for preparing a high flame-retardant aluminum alloy photovoltaic cable includes the following steps: Step 1: Mix ethylene-vinyl acetate copolymer, polyethylene, expanded graphite, modified montmorillonite, initiator, crosslinking agent, and additives, melt blend, mold, and cold press to obtain the outer sheath; Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0007] In a more optimized manner, the raw materials of the outer sheath include the following components: by weight, 40-50 parts of ethylene-vinyl acetate copolymer, 20-30 parts of polyethylene, 22-25 parts of expanded graphite, 5-8 parts of modified montmorillonite, 0.5-1 parts of initiator, 2-3 parts of crosslinking agent, and 0.5-1 parts of additives.

[0008] In a more optimized manner, the preparation of the modified montmorillonite includes the following steps: adding montmorillonite and boric acid sequentially to anhydrous ethanol, heating to 70-75°C and stirring for 4-5 hours; adding 1-amino-10-undecene and isopropyl p-aminobenzoate, and continuing to stir for 8-9 hours; washing with hot ethanol and drying to obtain modified montmorillonite.

[0009] More preferably, the modified montmorillonite raw material includes the following components: 10 parts montmorillonite, 3-4 parts boric acid, 1-2 parts 1-amino-10-undecene, and 1-2 parts isopropyl p-aminobenzoate; wherein the montmorillonite is calcium-based montmorillonite with an interlayer spacing of 1.8-2.2 nm.

[0010] More preferably, the crosslinking agent comprises an ionic liquid and triallyl isocyanurate in a mass ratio of (1.5~2):(0.5~1).

[0011] A more optimized method for preparing the ionic liquid is as follows: 1-vinylimidazolium and tris(2-chloroethyl) phosphate are mixed evenly in a molar ratio of (3.2~3.5):1, and stirred at a temperature of 45~55℃ for 5~7 days under a nitrogen atmosphere; after cooling, the mixture is washed with ethyl acetate, and the solvent is evaporated to obtain the ionic liquid.

[0012] More preferably, the polyethylene comprises high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of (10~15):(5~10):3:2.

[0013] More optimally, the melt blending conditions are: blending at 150~180℃ and 50~100rpm for 10~20 minutes; the compression molding conditions are: compression molding at 170~180℃ and 8~12MPa; and the cold pressing conditions are: cold pressing at room temperature and 8~12MPa for 5~10 minutes.

[0014] In a more optimized manner, the raw materials of the mineral fire retardant include the following components, by weight: 25-35 parts expanded perlite, 25-35 parts aluminum hydroxide, 10-20 parts chopped glass fiber, 5-12 parts microsilica powder, 8-12 parts vermiculite, 2-4 parts titanium dioxide, 1-2 parts organosilicon water-repellent agent, and 0.5-1 part sodium molybdate.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: by introducing expanded graphite and modified montmorillonite, a highly efficient flame retardant system is constructed; and by introducing crosslinking agents and polyethylene of specific components, mechanical properties are effectively guaranteed; thus, the prepared aluminum alloy photovoltaic cable ensures mechanical properties while possessing high flame retardancy.

[0016] The solution ensures high flame retardancy by introducing a specific ratio of expanded graphite and modified montmorillonite. Expanded graphite, a common flame retardant, possesses a unique layered structure that forms a dense carbon layer, effectively isolating oxygen and heat transfer, thus inhibiting combustion and significantly improving flame retardant performance. However, it has limitations: firstly, poor dispersibility; secondly, excessive introduction significantly impacts mechanical properties, while insufficient introduction reduces flame retardancy. Therefore, montmorillonite is introduced in this solution to: 1) utilize montmorillonite intercalation between graphite layers to promote graphite dispersion; and 2) form a carbon-silicon dual-network barrier, achieving synergistic flame retardancy. Montmorillonite is modified by grafting boric acid, 1-amino-10-undecene, and isopropyl p-aminobenzoate sequentially through the reactions of hydroxyl groups with boric acid and boric acid with amino groups; dispersing montmorillonite; and simultaneously introducing elements such as boron and nitrogen into the modified montmorillonite to enhance flame retardancy. Furthermore, the alkenyl groups it contains can effectively cross-link within the cable, enhancing mechanical properties. Furthermore, compared to other montmorillonite, the introduction of montmorillonite of specific specifications has better overall performance.

[0017] In this design, a specific proportion of polyethylene is introduced to improve mechanical properties and compatibility. High-density polyethylene, in conjunction with montmorillonite, provides rigidity and heat resistance, effectively improving mechanical strength, while low-density polyethylene enhances flexibility and processing performance, preventing embrittlement. Maleic anhydride-grafted polyethylene acts as a compatibilizer, improving the interfacial bonding between expanded graphite and the polymer matrix. Ethylene-zinc methacrylate copolymer effectively enhances melt strength and impact resistance. Therefore, the synergistic effect of these multiple components enables the cable to maintain high flame retardancy while also possessing excellent mechanical properties.

[0018] The proposed solution employs a composite crosslinking agent of ionic liquid and triallyl isocyanurate. This agent effectively promotes the formation of a crosslinked network, improving mechanical and flame-retardant properties, thereby enhancing practical applicability. The ionic liquid, prepared by reacting 1-vinylimidazolium with tris(2-chloroethyl) phosphate, possesses both flame-retardant and plasticizing properties, improving molecular chain fluidity. Synergistically, it works with triallyl isocyanurate to create a more ordered polymer aggregate and a denser network. This crosslinked network formation enhances thermal stability and mechanical strength, allowing the outer sheath to maintain structural integrity at high temperatures. Furthermore, the incorporation of a cold-pressing process further reduces defects. Detailed Implementation

[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] It should be noted that the following proportions are by weight. There are no special restrictions on the manufacturers of the raw materials involved in this invention. Exemplary examples include: expanded graphite with a particle size of 50-100 μm and an expansion ratio ≥200 mL / g; calcium-based montmorillonite with an interlayer spacing of 1.8-2.2 nm, model number HW-Ca-NA; boric acid with CAS number 10043-35-3; 1-amino-10-undecene with CAS number 25378-91-6; isopropyl p-aminobenzoate with CAS number 41904-76-7; and 1-vinylimidazole with CAS number 1072. -63-5; Tris(2-chloroethyl) phosphate CAS number is 115-96-8; Ethylene-vinyl acetate copolymer vinyl acetate content 28-33%, melt index 2-6g / 10min; High-density polyethylene model is ExxonMobil™-HDPE-HD6704; Low-density polyethylene model is Dow™-LDPE-640I, maleic anhydride grafted polyethylene model is Admer®NF538, Ethylene-zinc methacrylate copolymer model is DuPont™-Surlyn®8920; Peroxidation initiator is dicumyl peroxide; All related raw materials are commercially available.

[0021] In the following examples, the raw materials of the mineral fire retardant include the following components, by weight: 30 parts expanded perlite, 30 parts aluminum hydroxide, 15 parts chopped glass fiber, 10 parts microsilica powder, 10 parts vermiculite, 3 parts titanium dioxide, 1.5 parts organosilicon water-repellent agent, and 0.5 parts sodium molybdate.

[0022] Example 1: A method for preparing a high flame-retardant aluminum alloy photovoltaic cable, comprising the following steps: Pre-preparation: 10 parts of montmorillonite and 3.8 parts of boric acid were added sequentially to anhydrous ethanol, and the mixture was heated to 70°C and stirred for 4 hours; 2 parts of 1-amino-10-undecene and 1 part of isopropyl p-aminobenzoate were added, and the mixture was stirred for another 9 hours; the mixture was washed with hot ethanol and dried to obtain modified montmorillonite. 1-Vinylimidazole and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere. After cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain an ionic liquid. Step 1: Mix 42 parts of ethylene-vinyl acetate copolymer, 28 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 13:10:3:2), 22 parts of expanded graphite, 6 parts of modified montmorillonite, 0.5 parts of peroxide initiator, 2 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 1.5:0.5), and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are as follows: blend at 175℃ and 80 rpm for 15 minutes; mold at 180℃ and 10 MPa; and cold press at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0023] Example 2: A method for preparing a high flame-retardant aluminum alloy photovoltaic cable, comprising the following steps: Pre-preparation: 10 parts of montmorillonite and 3.8 parts of boric acid were added sequentially to anhydrous ethanol, and the mixture was heated to 70°C and stirred for 4 hours; 2 parts of 1-amino-10-undecene and 1 part of isopropyl p-aminobenzoate were added, and the mixture was stirred for another 9 hours; the mixture was washed with hot ethanol and dried to obtain modified montmorillonite. 1-Vinylimidazole and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere. After cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain an ionic liquid. Step 1: Mix 40 parts of ethylene-vinyl acetate copolymer, 30 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 15:10:3:2), 22 parts of expanded graphite, 5 parts of modified montmorillonite, 0.5 parts of peroxide initiator, 2.5 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 1.5:1), and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are as follows: blend at 175℃ and 80 rpm for 15 minutes; mold at 180℃ and 10 MPa; and cold press at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0024] Example 3: A method for preparing a high flame-retardant aluminum alloy photovoltaic cable, comprising the following steps: Pre-preparation: 10 parts of montmorillonite and 3.8 parts of boric acid were added sequentially to anhydrous ethanol, and the mixture was heated to 70°C and stirred for 4 hours; 2 parts of 1-amino-10-undecene and 1 part of isopropyl p-aminobenzoate were added, and the mixture was stirred for another 9 hours; the mixture was washed with hot ethanol and dried to obtain modified montmorillonite. 1-Vinylimidazole and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere. After cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain an ionic liquid. Step 1: Mix 50 parts of ethylene-vinyl acetate copolymer, 20 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 10:5:3:2), 25 parts of expanded graphite, 8 parts of modified montmorillonite, 0.5 parts of peroxide initiator, 3 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 2:1), and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are as follows: blend at 175℃ and 80 rpm for 15 minutes; mold at 180℃ and 10 MPa; and cold press at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0025] Comparative Example 1: Single introduction of expanded graphite; otherwise the same as Example 1; specifically including the following steps: Pre-preparation: 1-vinylimidazolium and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere; after cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain the ionic liquid; Step 1: Mix 42 parts of ethylene-vinyl acetate copolymer, 28 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 13:10:3:2), 28 parts of expanded graphite, 0.5 parts of peroxide initiator, 2 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 1.5:0.5), and 0.5 parts of antioxidant 1010, and melt blend them. The process conditions are as follows: blend at 175℃ and 80 rpm for 15 minutes; mold at 180℃ and 10 MPa; and cold press at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0026] Comparative Example 2: Montmorillonite was directly introduced; the rest was the same as in Example 1; specifically, the following steps were included: Pre-preparation: 1-vinylimidazolium and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere; after cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain the ionic liquid; Step 1: Mix 42 parts of ethylene-vinyl acetate copolymer, 28 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 13:10:3:2), 22 parts of expanded graphite, 6 parts of montmorillonite, 0.5 parts of peroxide initiator, 2 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 1.5:0.5), and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are: blending at 175℃ and 80 rpm for 15 minutes; molding at 180℃ and 10 MPa; and cold-pressing at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0027] Comparative Example 3: The amount of montmorillonite introduced was increased; the rest was the same as in Example 1; specifically, the following steps were included: Pre-preparation: 10 parts of montmorillonite and 3.8 parts of boric acid were added sequentially to anhydrous ethanol, and the mixture was heated to 70°C and stirred for 4 hours; 2 parts of 1-amino-10-undecene and 1 part of isopropyl p-aminobenzoate were added, and the mixture was stirred for another 9 hours; the mixture was washed with hot ethanol and dried to obtain modified montmorillonite. 1-Vinylimidazole and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere. After cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain an ionic liquid. Step 1: Mix 42 parts of ethylene-vinyl acetate copolymer, 28 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 13:10:3:2), 18 parts of expanded graphite, 11 parts of modified montmorillonite, 0.5 parts of peroxide initiator, 2 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 1.5:0.5), and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are as follows: blend at 175℃ and 80 rpm for 15 minutes; mold at 180℃ and 10 MPa; and cold press at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0028] Comparative Example 4: The composition of polyethylene was adjusted; the rest was the same as in Example 1; specifically, the following steps were included: Pre-preparation: 10 parts of montmorillonite and 3.8 parts of boric acid were added sequentially to anhydrous ethanol, and the mixture was heated to 70°C and stirred for 4 hours; 2 parts of 1-amino-10-undecene and 1 part of isopropyl p-aminobenzoate were added, and the mixture was stirred for another 9 hours; the mixture was washed with hot ethanol and dried to obtain modified montmorillonite. 1-Vinylimidazole and tris(2-chloroethyl) phosphate were mixed evenly at a molar ratio of 3.2:1 and stirred at 50°C for 7 days under a nitrogen atmosphere. After cooling, the mixture was washed with ethyl acetate and the solvent was evaporated to obtain an ionic liquid. Step 1: Mix 42 parts of ethylene-vinyl acetate copolymer, 28 parts of polyethylene (high-density polyethylene, low-density polyethylene, and maleic anhydride-grafted polyethylene in a mass ratio of 15:8:5), 22 parts of expanded graphite, 6 parts of modified montmorillonite, 0.5 parts of peroxide initiator, 2 parts of crosslinking agent (ionic liquid and triallyl isocyanurate in a mass ratio of 1.5:0.5), and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are as follows: blend at 175℃ and 80 rpm for 15 minutes; mold at 180℃ and 10 MPa; and cold press at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0029] Comparative Example 5: No ionic liquid was introduced; otherwise, it was the same as Example 1; specifically, it included the following steps: Pre-preparation: 10 parts of montmorillonite and 3.8 parts of boric acid were added sequentially to anhydrous ethanol, and the mixture was heated to 70°C and stirred for 4 hours; 2 parts of 1-amino-10-undecene and 1 part of isopropyl p-aminobenzoate were added, and the mixture was stirred for another 9 hours; the mixture was washed with hot ethanol and dried to obtain modified montmorillonite. Step 1: Mix 42 parts of ethylene-vinyl acetate copolymer, 28 parts of polyethylene (high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of 13:10:3:2), 22 parts of expanded graphite, 6 parts of modified montmorillonite, 0.5 parts of peroxidation initiator, 2 parts of triallyl isocyanurate, and 0.5 parts of antioxidant 1010, and melt-blend them. The process conditions are: blending at 175℃ and 80 rpm for 15 minutes; molding at 180℃ and 10 MPa; and cold-pressing at 10 MPa for 5 minutes to obtain the outer sheath. Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable.

[0030] Performance Test 1: The outer sheaths prepared in the examples and comparative examples were subjected to relevant performance tests. Specifically, the tensile strength was tested using an electronic universal testing machine (dumbbell type) at a tensile rate of 250 mm / min, according to the standard method of GB / T2951.11-2008. The limiting oxygen index (LOI) was tested using an oxygen index tester, according to the standard method of ASTM D2863. The UL-94 rating was tested using a horizontal and vertical burning tester, according to the standard method of ASTM D3801. The obtained data are shown in the table below.

[0031] Conclusion: The data in the table above show that this application has prepared a high flame-retardant aluminum alloy photovoltaic cable with excellent mechanical properties. A comparison of the data from Comparative Examples 1-3 with that of Example 1 indicates that modifying montmorillonite and compounding it with expanded graphite can effectively improve flame retardancy, but the ratio of the two components needs to be effectively controlled to maximize the overall performance. A comparison of the data from Comparative Example 4 with that of Example 1 shows that a specific ratio of the polyethylene component can effectively improve interfacial properties and crosslinking properties, thereby improving mechanical properties and flame retardancy. A comparison of the data from Comparative Example 4 with that of Example 1 shows that the introduction of ionic liquid can further improve mechanical properties and assist in improving flame retardancy.

[0032] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high flame-retardant aluminum alloy photovoltaic cable, characterized in that: Includes the following steps: Step 1: Mix ethylene-vinyl acetate copolymer, polyethylene, expanded graphite, modified montmorillonite, initiator, crosslinking agent, and additives, melt blend, mold, and cold press to obtain the outer sheath; Step 2: Using aluminum alloy as the wire core, wrap it with an oxygen barrier layer and an insulation layer to obtain the basic wire core; combine the basic wire cores, fill them with mineral fire-retardant material, and wrap them with an outer sheath to obtain a high flame-retardant aluminum alloy photovoltaic cable. The raw materials of the outer sheath include the following components: by weight, 40-50 parts ethylene-vinyl acetate copolymer, 20-30 parts polyethylene, 22-25 parts expanded graphite, 5-8 parts modified montmorillonite, 0.5-1 part initiator, 2-3 parts crosslinking agent, and 0.5-1 part additives. The preparation of the modified montmorillonite includes the following steps: by weight, 10 parts of montmorillonite and 3-4 parts of boric acid are added sequentially to anhydrous ethanol, and the mixture is heated to 70-75°C and stirred for 4-5 hours; 1-2 parts of 1-amino-10-undecene and 1-2 parts of isopropyl p-aminobenzoate are added, and the mixture is stirred for another 8-9 hours; the mixture is then washed with hot ethanol and dried to obtain the modified montmorillonite. The crosslinking agent comprises an ionic liquid and triallyl isocyanurate in a mass ratio of (1.5~2):(0.5~1); The ionic liquid is prepared by mixing 1-vinylimidazolium and tris(2-chloroethyl) phosphate in a molar ratio of (3.2~3.5):1, stirring at 45~55℃ for 5~7 days under a nitrogen atmosphere, cooling, washing with ethyl acetate, and evaporating the solvent to obtain the ionic liquid.

2. The method for preparing a high flame-retardant aluminum alloy photovoltaic cable according to claim 1, characterized in that: The montmorillonite is a calcium-based montmorillonite with an interlayer spacing of 1.8~2.2 nm.

3. The method for preparing a high flame-retardant aluminum alloy photovoltaic cable according to claim 1, characterized in that: The polyethylene comprises high-density polyethylene, low-density polyethylene, maleic anhydride-grafted polyethylene, and ethylene-zinc methacrylate copolymer in a mass ratio of (10~15):(5~10):3:

2.

4. The method for preparing a high flame-retardant aluminum alloy photovoltaic cable according to claim 1, characterized in that: The melt blending conditions are: blending at 150~180℃ and 50~100rpm for 10~20 minutes; the compression molding conditions are: compression molding at 170~180℃ and 8~12MPa; the cold pressing conditions are: cold pressing at room temperature and 8~12MPa for 5~10 minutes.

5. The method for preparing a high flame-retardant aluminum alloy photovoltaic cable according to claim 1, characterized in that: The raw materials of the mineral fire retardant include the following components, by weight: 25-35 parts expanded perlite, 25-35 parts aluminum hydroxide, 10-20 parts chopped glass fiber, 5-12 parts microsilica powder, 8-12 parts vermiculite, 2-4 parts titanium dioxide, 1-2 parts organosilicon water-repellent agent, and 0.5-1 part sodium molybdate.

6. The high flame-retardant aluminum alloy photovoltaic cable prepared by the method of preparing a high flame-retardant aluminum alloy photovoltaic cable according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Low-smoke high-flame-retardant aluminum alloy photovoltaic cable and preparation method thereof

    CN118016363A

  • Photovoltaic cable for photovoltaic power generation

    CN118315111A