Surface treatment method for preventing cracks in large-section titanium alloy square billet pre-rolling

By employing a multi-stage electroplating and heating synergistic treatment method, the cracking problem of large-section titanium alloy billets during the rolling process was solved, forming a uniform and dense nickel plating layer, reducing temperature gradient and stress concentration, and improving yield and finished product quality.

CN120394558BActive Publication Date: 2026-11-24CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202510588331.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-24
Estimated Expiration
2045-05-08

AI Technical Summary

Technical Problem

Large-section titanium alloy billets are prone to cracking during rolling, and existing technologies are unable to effectively solve this problem, especially due to the reduced plasticity and cracking risk caused by the rapid drop in surface temperature.

Method used

A multi-stage electroplating and heating synergistic treatment method is adopted, including surface pretreatment, first-stage electroplating to form an initial nickel plating layer, stress relief treatment, second-stage electroplating to thicken the nickel plating layer, and pre-rolling heating, to form a uniform and dense nickel plating layer to reduce temperature gradient and stress concentration.

Benefits of technology

It significantly reduces the risk of cracking in large-section titanium alloy billets during rolling, improves yield and finished product quality, reduces surface scratches and peeling of finished products, and enhances material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120394558B_ABST
    Figure CN120394558B_ABST
Patent Text Reader

Abstract

This invention discloses a surface treatment method for pre-rolling large-section titanium alloy square billets to prevent cracking, belonging to the field of titanium alloy surface treatment technology. The method includes: S1. sequentially grinding and degreasing the surface of the titanium alloy square billet; S2. electroplating nickel onto the pre-treated billet to form an initial nickel plating layer; S3. heating and holding the nickel-plated billet under vacuum conditions; S4. performing a second electroplating of nickel on the stress-relieved billet to form a thickened nickel plating layer; S5. uniformly heating and holding the second-plated nickel billet before rolling. This invention forms a uniform and dense nickel plating layer on the surface of the large-section titanium alloy square billet through electroplating, which reduces the rate of temperature drop on the surface of the billet after it exits the furnace, significantly reduces the temperature gradient between the billet surface and interior, and ensures the rolling plasticity of the billet during the initial rolling stage; it effectively solves the technical problem of cracking easily in large-section titanium alloy square billets during the rolling process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy surface treatment technology, and relates to a method for reducing cracking during the rolling of large-section titanium alloy square billets, specifically a surface treatment method for pre-rolling large-section titanium alloy square billets to prevent cracking. Background Technology

[0002] In the field of hot rolling of titanium alloy bars and wires, using large-section square billets in high-speed continuous rolling mills is an important direction for improving material utilization and production efficiency. However, compared with small-diameter billets, the risk of cracking is higher when rolling large-section titanium alloy billets, which can seriously reduce the surface quality of finished wires and even lead to steel pile-up accidents. The main reasons are as follows: First, compared with pure titanium, which has high ductility, titanium alloy billets have high strength and poor plasticity, resulting in greater deformation resistance during rolling deformation and a higher risk of billet cracking. Second, after the large-section titanium alloy billets are heated and taken out of the furnace, the surface temperature drops rapidly due to the large surface area in contact with air (leading to a decrease in surface plasticity) and thus falling below the ideal initial rolling temperature, making it easy for surface cracking to occur in the roughing and intermediate rolling stages with large deformation.

[0003] Currently, there are three main solutions to the above problems in existing technologies: First, by increasing the heating temperature and extending the holding time, the rolling performance can be improved by utilizing the material's plasticity at high temperatures. However, this method is prone to causing structural defects such as grain coarsening. Second, smaller-sized, small-section titanium alloy billets can be used to reduce the temperature gradient between the core and the surface, thereby reducing the risk of subsequent rolling cracks. However, this leads to a decrease in the yield per rolling pass, making it difficult to meet the production needs of large-size coiled products. Third, the material's plasticity can be improved through surface treatment or rolling process optimization. For example, CN119634457A uses multi-pass rolling pretreatment to enhance the surface plasticity of the slab, but its process route is complex and difficult to match the high-speed continuous rolling rhythm. CN117772792A controls thin plate cracking by coating a high-temperature anti-oxidation layer combined with multi-stage rolling, but this method requires repeated heating and welding operations, significantly increasing costs.

[0004] Existing surface treatment technologies are mostly focused on plate rolling scenarios. The surface strengthening or coating protection solutions they employ have significant limitations in the continuous rolling of large-section square billets. On the one hand, the local rolling treatment used in plate rolling (such as CN119634457A) cannot effectively cover the edge area of ​​the square billet, and the processing efficiency is difficult to meet the mass production needs of long-size square billets. On the other hand, the special protective layer for thin plates (such as CN117772792A) is prone to peeling off in high-temperature and large-deformation rolling, which exacerbates the risk of surface defects.

[0005] Therefore, how to fundamentally solve the risk of surface cracking in large-section titanium alloy billets caused by the rapid drop in surface temperature after exiting the furnace has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] The technical problem this invention aims to solve is the tendency of titanium alloy billets with a cross-sectional thickness of 200-300 mm to crack during the rolling process. This invention provides a surface treatment method for large-section titanium alloy billets, involving multi-stage electroplating and heat treatment, which can significantly reduce the risk of billet cracking during high-speed hot rolling and greatly improve the yield.

[0007] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:

[0008] In a first aspect, the present invention provides a surface treatment method for pre-rolling large-section titanium alloy square billets to resist cracking, comprising the following steps:

[0009] S1. Surface pretreatment: The titanium alloy billet is subjected to surface grinding and degreasing treatment in sequence;

[0010] S2. First stage electroplating: Electroplating nickel onto the pretreated billet to form an initial nickel plating layer;

[0011] S3. Stress relief treatment: Heat and hold the nickel-plated billet under vacuum conditions;

[0012] S4. Second stage electroplating: The stress-relieved billet is electroplated with nickel a second time to form a thickened nickel plating layer;

[0013] S5. Pre-rolling heating: The secondary nickel-plated billet is heated to a uniform temperature and kept at that temperature before rolling.

[0014] In step S1 above, the side length of the titanium alloy square billet is 200-300mm and the length is 5000-6000mm.

[0015] In step S1 above, the surface after grinding meets the following requirements: surface roughness Ra is 3.3~7.5μm, side length difference is ≤20mm, and diagonal difference is ≤10mm.

[0016] In step S1 above, the degreasing treatment includes: placing the titanium alloy billet in an alkaline degreasing solution and immersing it at 50-90°C for 20-30 minutes; after immersion, cleaning it in clean water at 45-55°C and at 40-70 kHz to remove alkaline residue.

[0017] Furthermore, the components of the alkaline degreasing solution include: NaOH 20-30 g / L, Na2CO3 20-35 g / L, Na3PO4 15-25 g / L, and Na2SiO3 5-8 g / L.

[0018] In step S2 above, a nickel plating solution is used for electroplating, the components of which include: nickel sulfate 25-35 g / L, sodium hypophosphite 20-30 g / L, trisodium citrate 10-20 g / L, ammonium chloride 8-12 g / L, and sodium acetate 8-12 g / L.

[0019] In step S2 above, the electroplating parameters for the first stage are: pH = 4.5–5.5, electroplating temperature 40–60℃, and current density 2–4 A / dm³. 2 The electroplating time is 45–60 minutes, and the coating thickness is 15–20 μm.

[0020] In step S3 above, the stress relief treatment is carried out in a vacuum heating furnace at a heating temperature of 200-350°C and a holding time of 60-90 minutes.

[0021] In step S4 above, a nickel plating solution is used for electroplating, the components of which include: nickel sulfate 25-35 g / L, sodium hypophosphite 20-30 g / L, trisodium citrate 10-20 g / L, ammonium chloride 8-12 g / L, and sodium acetate 8-12 g / L.

[0022] In step S4 above, the electroplating parameters for the second stage are: pH = 4.5–5.5, electroplating temperature 55–65℃, and current density 3–5 A / dm³. 2 The electroplating time is 3 hours, and the total coating thickness is 45-50 μm.

[0023] In step S5 above, the temperature of the pre-rolling heating is (T) β -50)~(T β -20℃, heat preservation time 60~90min.

[0024] The beneficial effects of this invention are:

[0025] (1) The present invention forms a uniform and dense nickel plating layer on the surface of a large cross-section titanium alloy billet by electroplating, which can effectively reduce the rate of temperature drop of the surface layer of the billet after it exits the furnace, significantly reduce the temperature gradient between the surface and the interior of the billet, and ensure the plastic deformation capacity of the billet during the rolling stage; at the same time, the nickel plating layer itself has good thermal conductivity and ductility, which can suppress stress concentration during heating and rolling, thereby greatly reducing the risk of billet rolling cracking and improving the quality and yield of titanium alloy products.

[0026] (2) This invention employs a staged electroplating and heat treatment synergistic process: stress relief treatment is performed after the first electroplating, which can enhance the diffusion effect between the initial coating and the surface atoms of the titanium alloy billet, forming a more robust metallurgical bonding layer; on this basis, a second electroplating is performed to further increase the thickness of the coating. This process not only improves the bonding force between the coating and the substrate, but also improves the uniformity of the coating, reduces local stress concentration during rolling, and lowers the risk of surface cracking.

[0027] (3) The nickel-plated surface has low friction characteristics. During high-speed rolling, it can significantly reduce the sliding friction between the titanium alloy surface and equipment such as rolls and guides, effectively reducing the occurrence rate of surface scratches and other defects during rolling, thereby reducing the amount of subsequent peeling of finished coils and improving material utilization. Attached Figure Description

[0028] Figure 1 Images of the TC4 surface before (left) and after (right) electroplating treatment, as shown in the example.

[0029] Figure 2 Images showing the surface quality of the TC4 rough-rolled billet (left) and finished coil (right) as an example;

[0030] Figure 3 Images showing the surface quality of the TC4 rough-rolled billet (left) and finished coil (right) in Comparative Example 1;

[0031] Figure 4 Images showing the surface quality of the TC4 rough-rolled billet (left) and finished coil (right) in Comparative Example 2. Detailed Implementation

[0032] To make the technical problems, solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with the embodiments. Unless otherwise defined, all technical terms used herein have the same meaning as understood by one of ordinary skill in the art.

[0033] This invention discloses a surface treatment method for pre-rolling large-section titanium alloy square billets to prevent cracking, comprising the following steps:

[0034] (1) Surface grinding: Select a rolling mill billet with dimensions of 200~300×200~300×5000~6000mm, perform surface mechanical grinding and edge chamfering on the titanium alloy billet, remove surface oxide scale and defects such as cracks and heavy scale, control the surface roughness to Ra 3.3~7.5μm, control the side length difference to ≤20mm, and the diagonal difference to ≤10mm.

[0035] (2) Degreasing treatment: The ground titanium alloy billet is placed in an alkaline degreasing solution composed of 20-30 g / L sodium hydroxide, 20-35 g / L sodium carbonate, 15-25 g / L sodium phosphate, and 5-8 g / L sodium silicate. The alkaline degreasing solution is heated to 50-90℃ and soaked for 20-30 minutes, with appropriate stirring during the process to enhance the degreasing effect. Then, the billet is placed in clean water at 45-55℃ for ultrasonic cleaning at a frequency of 40-70 kHz to remove residual alkaline solution from the surface.

[0036] (3) First-stage electroplating: The titanium alloy billet treated in step (2) is electroplated with nickel. The nickel plating solution formula is: nickel sulfate 25-35 g / L, sodium hypophosphite 20-30 g / L, trisodium citrate 10-20 g / L, ammonium chloride 8-12 g / L, sodium acetate 8-12 g / L, and appropriate amount of water. The titanium alloy billet is used as the cathode and placed in the electroplating tank. The pH value is controlled at 4.5-5.5, the electroplating temperature is 40-60℃, and the current density is 2-4 A / dm³. 2 The electroplating time is 45–60 minutes, forming an initial nickel plating layer with a thickness of 15–20 μm on the surface of the titanium alloy billet. After electroplating, the billet is rinsed with running water to remove residual plating solution and then left to dry.

[0037] (4) Stress relief treatment: The titanium alloy billet after step (3) is sent into a vacuum heat treatment furnace at a temperature of 200-350℃ and a holding time of 60-90min to eliminate the residual stress of the billet and the coating, so that the electroplating layer is firmly bonded to the surface of the titanium alloy billet.

[0038] (5) Second-stage electroplating: Using the same electroplating solution formula as in step (3), the titanium alloy billet treated in step (4) is electroplated again to further thicken the nickel plating layer. The pH value is controlled at 4.5–5.5, the electroplating temperature at 55–65℃, and the current density at 3–5 A / dm³. 2 The electroplating time is 3 hours, and the nickel plating layer thickness is 45-50 μm. After electroplating, the surface of the blank is rinsed with running water to remove any residual plating solution, and then left to dry.

[0039] (6) Pre-rolling heating: The billet processed in step (5) is sent into an electric heating furnace for heating, and the temperature is set to (T). β -50)~(T β -20℃, hold at that temperature for 60-90 minutes to ensure uniform temperature in all parts of the billet, and then remove it from the furnace for rolling.

[0040] The following specific embodiments will be provided to explain the solution of the present invention. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0041] Example

[0042] I. Surface Treatment for Crack Resistance in Pre-rolling of Large-Section Titanium Alloy Square Billets

[0043] Example: A pre-rolling surface treatment was performed on a TC4 titanium alloy square billet with a phase transformation point of 980℃. The specific steps were as follows:

[0044] (1) Surface grinding: Select a large cross-section TC4 titanium alloy square billet with dimensions of 200×200×5500mm, perform surface mechanical grinding and edge chamfering on the titanium alloy square billet, remove surface oxide scale and defects such as cracks and heavy scale, control the surface roughness to Ra 3.5μm, the side length difference to be 17mm, and the diagonal difference to be 8mm.

[0045] (2) Degreasing treatment: The ground titanium alloy billet is placed in an alkaline degreasing solution composed of 25 g / L sodium hydroxide, 25 g / L sodium carbonate, 15 g / L sodium phosphate and 6 g / L sodium silicate, and soaked at 70°C for 30 min, with appropriate stirring during the process to enhance the degreasing effect; then, the billet is placed in clean water at 50°C for ultrasonic cleaning at a frequency of 60 kHz to remove the residual alkaline solution on the surface.

[0046] (3) First-stage electroplating: The titanium alloy billet treated in step (2) is electroplated with nickel. The nickel plating solution formula is: 25 g / L nickel sulfate, 20 g / L sodium hypophosphite, 10 g / L trisodium citrate, 10 g / L ammonium chloride, 8 g / L sodium acetate, and appropriate amount of water. The titanium alloy billet is used as the cathode and placed in the electroplating tank. The pH value is controlled at 5.0, the electroplating temperature is 50℃, and the current density is 2.0 A / dm³. 2 The electroplating time is 50 minutes to form an initial nickel plating layer with a thickness of 15μm on the surface of the titanium alloy billet. After electroplating, the billet is rinsed with running water to remove the residual plating solution on the surface, and then left to dry.

[0047] (4) Stress relief treatment: The titanium alloy billet after step (3) is sent into a vacuum heat treatment furnace at a temperature of 300°C for 80 minutes to eliminate the residual stress of the billet and the coating, so that the electroplating layer is firmly bonded to the surface of the titanium alloy billet.

[0048] (5) Second-stage electroplating: Using the same electroplating solution formulation as in step (3), the titanium alloy billet treated in step (4) is electroplated again to further thicken the nickel plating layer. The pH value is controlled at 5.5, the electroplating temperature at 55℃, and the current density at 5.0 dm³. 2 The electroplating time is 3 hours, and the total thickness of the nickel plating layer is 47 μm. After electroplating, the surface of the blank is cleaned with running water to remove any residual plating solution, and then left to dry.

[0049] (6) Pre-rolling heating: The billet processed in step (5) is sent into an electric heating furnace for heating. The temperature is set to 950℃ and held for 90 minutes to ensure that the temperature of each part of the billet is uniform. Then it is taken out of the furnace for rolling to obtain a coil.

[0050] Comparative Example 1: The TC4 titanium alloy square billet was subjected to pre-rolling surface treatment according to the process shown in the example. The difference from the example is that the two-stage electroplating treatment was not performed (i.e., steps 1 to 5 in the example were cancelled). The remaining processes and parameters were the same as those in the example.

[0051] Comparative Example 2: The TC4 titanium alloy square billet was subjected to pre-rolling surface treatment according to the process shown in the example. The difference from the example is that the second-stage electroplating treatment was not performed (i.e., step 5 in the example was cancelled). The remaining processes and parameters were the same as those in the example.

[0052] II. Quality Inspection of Surface-treated Billets and Rolled Wire Rods

[0053] 1. Appearance quality inspection of billets and coils

[0054] The square billet after the two-stage electroplating treatment in the example has a surface friction roughness of 2.5 to 3.0 μm, a friction coefficient of 0.15, and a critical scratch load Lc (coating adhesion) of 25.8 N. Figure 1 Images of the TC4 in this embodiment before (left) and after (right) surface electroplating treatment. Figure 2 Images showing the surface quality of the TC4 square billet after rough rolling (left) and the finished coil (right) as illustrated in this example. Figure 1 It can be seen that after the two-stage electroplating process, the surface of the billet has a uniform and dense nickel plating layer, and the surface is smooth. Figure 2 It can be seen that after rough rolling, the billet surface did not crack, there was no visible coating peeling, and the finished coil surface quality was good.

[0055] Comparative Example 1, which was not surface-treated, had a surface friction roughness of 8.5–12 μm, which was relatively high, and a friction coefficient of 0.45. Figure 3 Images showing the surface quality of the TC4 square billet after rough rolling (left) and the finished coil (right) in Comparative Example 1, provided by [source missing]. Figure 3It can be seen that after rough rolling, obvious cracks appear on the surface of the billet, and large areas of cracks extending along the rolling direction appear on the surface of the finished coil, with severe surface scratches.

[0056] The two comparative examples have coatings that have undergone the first stage of electroplating treatment, with a friction coefficient of 0.3 and a critical scratch load Lc (coating adhesion) of 10.2 N. Figure 4 Images showing the surface quality of the TC4 square billet after rough rolling (left) and the finished coil (right) in Comparative Example 2 are provided by [source missing]. Figure 3 It can be seen that after rough rolling, micro-cracks appear locally on the surface of the billet, and crack spots extending along the rolling direction appear locally on the surface of the finished coil.

[0057] 2. Surface properties and process temperature testing of billets and coils

[0058] (1) The surface temperature changes of the billet after exiting the furnace and before rough rolling were recorded by infrared thermal imager. The results are shown in Table 1.

[0059] Table 1. Surface temperature results of TC4 billets after heating and before rough rolling.

[0060]

[0061] As shown in Table 1, the surface temperature drop rate of the billet in Example 1 (nickel-plated square billet) was significantly reduced when it reached the roughing mill after being heated and exiting the furnace. Within 0–30 seconds, the average temperature drop rate was 1.7 °C / s, compared to 3.6 °C / s in Comparative Example 1 and 3.0 °C / s in Comparative Example 2. Although Comparative Example 2 only had one plating layer, the reduction in surface temperature drop rate was not significant, but the overall temperature gradient of the billet was not significantly different. Therefore, it can be seen that after treatment by the method of this invention, the surface temperature drop rate can be reduced by approximately 52%, and the temperature is more uniform from beginning to end of the billet.

[0062] (2) The surface quality of the blank and the coil was inspected, and the surface defects of the finished coil were counted. The data results are shown in Table 2.

[0063] Table 2 Statistical Results of Surface Quality Data for Finished TC4 Circular Wires

[0064] index Example Comparative Example 1 Comparative Example 2 Number of surface cracks (cracks / m) Not detected 12~15 5~10 Maximum crack depth (mm) Not detected 1.2~2.5 0.5~1.5 Surface scratch rate (%) 5% 35% 8% Yield (%) 96% 84% 88% Peeling volume (mm) Remove 0.15~0.3mm Remove 0.7mm Remove 0.5mm

[0065] As shown in Table 2, the finished coils in the embodiment have fewer surface defects, cracks are basically eliminated, the scratch rate is reduced by 85%, the amount of peeling is reduced from 0.7 mm to 0.15-0.3 mm, and the yield is increased by 12%. This indicates that the nickel plating layer in the embodiment effectively maintains the surface plasticity by suppressing radiative heat dissipation and air convection, and homogenizing the temperature distribution, thus basically eliminating cracks; at the same time, by reducing friction, it reduces scratches on the titanium alloy surface from equipment such as rolls and guides, significantly improving the surface quality of the finished coils. In contrast, the finished coils in Comparative Example 2 still have crack defects on the surface, but the degree of surface scratches is comparable, the amount of peeling is reduced from 0.5 mm to 0.15-0.3 mm, and the yield is increased by 8%. This shows that the two-stage electroplating + stress relief treatment process in the embodiment increases the coating adhesion by 150% (Lc increases from 10.2 N to 25.8 N), making it less prone to peeling. While the first-stage electroplating process in Comparative Example 2 can reduce surface scratches, it cannot effectively alleviate the surface temperature drop after the billet exits the furnace, leading to a decrease in surface plasticity and cracks, resulting in an increase in the amount of peeling off the finished coil and a decrease in the yield.

Claims

1. A surface treatment method for pre-rolling large-section titanium alloy square billets to prevent cracking, characterized in that, Includes the following steps: S1. Surface pretreatment: The titanium alloy billet is subjected to surface grinding and degreasing treatment in sequence; S2. First stage electroplating: Electroplating nickel onto the pretreated billet to form an initial nickel plating layer; S3. Stress relief treatment: Heat and hold the nickel-plated billet under vacuum conditions; S4. Second stage electroplating: The stress-relieved billet is electroplated with nickel a second time to form a thickened nickel plating layer; S5. Pre-rolling heating: The secondary nickel-plated billet is heated to a uniform temperature and kept at that temperature before rolling; In step S1, the cross-sectional side length of the titanium alloy billet is 200~300mm and the length is 5000~6000mm; In steps S2 and S4, the electroplating uses a nickel plating solution with the same composition; The components of the nickel plating solution include: nickel sulfate 25~35g / L, sodium hypophosphite 20~30g / L, trisodium citrate 10~20g / L, ammonium chloride 8~12g / L, and sodium acetate 8~12g / L; In step S2, the electroplating parameters for the first stage are: pH = 4.5~5.5, electroplating temperature 40~60℃, and current density 2~4A / dm³. 2 Electroplating time: 45-60 minutes; plating thickness: 15-20 μm. In step S3, the stress relief treatment is carried out in a vacuum heating furnace at a heating temperature of 200~350℃ and a holding time of 60~90min. In step S4, the electroplating parameters for the second stage are: pH = 4.5~5.5, electroplating temperature 55~65℃, and current density 3~5A / dm³. 2 Electroplating time is 3 hours, and the total coating thickness is 45~50μm.

2. The surface treatment method for pre-rolling large-section titanium alloy square billets to resist cracking according to claim 1, characterized in that: In step S1, the surface after grinding meets the following requirements: surface roughness Ra is 3.3~7.5μm, side length difference is ≤20mm, and diagonal difference is ≤10mm.

3. The surface treatment method for pre-rolling large-section titanium alloy square billets to resist cracking according to claim 1, characterized in that: In step S1, the degreasing treatment includes: placing the titanium alloy billet in an alkaline degreasing solution and immersing it at 50~90℃ for 20~30 minutes; after immersion, cleaning it in clean water at 45~55℃ and at 40~70kHz to remove alkaline residue.

4. The surface treatment method for pre-rolling large-section titanium alloy square billets to resist cracking according to claim 3, characterized in that: The alkaline degreasing solution comprises: NaOH 20~30g / L, Na2CO3 20~35g / L, Na3PO4 15~25g / L, and Na2SiO3 5~8g / L.

5. The surface treatment method for pre-rolling large-section titanium alloy square billets to resist cracking according to claim 1, characterized in that: In step S5, the temperature of the pre-rolling heating is (T) β -50) ~ (T β -20℃, heat preservation time 60~90min.

Citation Information

Patent Citations

  • Rolling method of Ti-6242 titanium alloy sheet

    CN117772792A

  • Method for inhibiting surface cracking in rolling process of high-strength titanium alloy thick plate

    CN119634457A

  • Clad alloy substrates and method for making same

    CN102861981A

  • Plating method of high silicon aluminum alloy

    CN107304479A

  • Method for preparing titanium alloy wide and thick plate through steel mill rolling mill