Perovskite-type sodium-ion battery negative electrode material precipitating nano high-entropy alloy in situ and preparation method thereof
Patent Information
- Application Number
- CN202510593661.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-05-09
AI Technical Summary
[0004]本发明为解决现有钠离子电池负极材料比容量低的问题,提供原位析出纳米高熵合金的钙钛矿型钠离子负极材料,其材料通式为LaFex1Cux2Nix3Alx4Mnx5O3@FeCuNiAlMn,其中x1+x2+x3+x4+x5=1,FeCuNiAlMn为析出于负极材料表面的纳米高熵合金颗粒
Smart Images

Figure CN120413643B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery anode material technology, and in particular to perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys and its preparation method. Background Technology
[0002] Compared to lithium resources, sodium resources are abundant and environmentally friendly, which can alleviate the limitations on battery development caused by lithium resource shortages to some extent, thus making it a potential next-generation battery system to replace lithium-ion batteries. However, because sodium ions have a larger radius than lithium ions, their ion diffusion rate during insertion-extraction cycles is slower. This means that the energy density of sodium-ion batteries still has considerable room for improvement compared to lithium-ion batteries, hindering their application and widespread adoption.
[0003] Sodium-ion batteries consist of a positive electrode, a negative electrode, a separator, an electrolyte, and a battery casing. While extensive research has been conducted on positive electrode materials, research on negative electrode materials is insufficient. Existing sodium-ion battery negative electrode material systems mainly focus on carbon-based materials, such as the patents CN119591080A ("A Preparation Method and Application of a Sodium-ion Battery Negative Electrode Material"), CN119601621A ("A Pitch-based Hard Carbon Negative Electrode Material with High First-Time Efficiency, High Rate Capacity, and Its Preparation Method"), and CN119143176B ("A Sodium-ion Battery Negative Electrode Material and Its Preparation Method Composed of Bismuth Oxide Chloride and Sulfur Oxide Co-doped Carbon Quantum Dots"). These carbon-based materials possess good cycle stability, but their specific capacity is relatively low. Therefore, developing a novel negative electrode material with high energy density and low cost, along with its preparation method, is crucial for the commercial application of sodium-ion batteries. Summary of the Invention
[0004] This invention addresses the problem of low specific capacity in existing sodium-ion battery anode materials by providing a perovskite-type sodium-ion anode material with in-situ precipitation of nano-high-entropy alloys, the general formula of which is LaFe. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@FeCuNiAlMn, where x1+x2+x3+x4+x5=1, and FeCuNiAlMn are nano-high-entropy alloy particles precipitated on the surface of the negative electrode material.
[0005] In addition, the present invention also provides a method for preparing the above-mentioned in-situ precipitated nano-high-entropy alloy perovskite-type sodium-ion anode material, comprising the following steps: S1: Dissolve La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 completely in deionized water and stir thoroughly to obtain a homogeneous solution; S2: Stir the solution in a water bath, add citric acid, until a viscous sol is obtained; S3: Dry the sol to obtain a dry gel, and then grind it to obtain a precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are then calcined in air to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. x1 Cu x2 Ni x3 Alx4Mn x5 O3, i.e., intermediate product A; S5: The intermediate product A discs were calcined at high temperature in a CO / Ar mixed atmosphere to obtain a perovskite oxide LaFe with nano-Fe particles precipitated in situ on the surface. x1 Cu x2 Ni x3 Alx4Mn x5 O3@Fe, i.e., intermediate product B; S6: The intermediate product B discs were calcined at medium temperature in a CO / Ar mixed atmosphere to obtain perovskite oxide LaFe with in-situ precipitated nano-FeCu alloy particles on the surface. x1 Cu x2 Ni x3 Alx4Mn x5 O3@FeCu, i.e., intermediate product C; S7: The intermediate product C wafers were calcined at low temperature in a CO / Ar mixed atmosphere to obtain a perovskite-type sodium-ion battery anode material with in-situ precipitated nano-FeCuNiAlMn high-entropy alloy particles on the surface, namely LaFe x1 Cu x2 Ni x3 Alx4Mn x5 O3@FeCuNiAlMn.
[0006] Preferably, the ratio of the total amount of Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 in step S1 to La(NO3)3 is 1:1.
[0007] Preferably, in step S2, the water bath temperature is 60~80℃ and the stirring time is 4~6h.
[0008] Preferably, in step S2, the ratio of the amount of citric acid to the total amount of Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1.
[0009] Preferably, in step S3, the sol is dried by a blower dryer at a temperature of 100-200°C for 8-12 hours.
[0010] Preferably, in step S4, the calcination temperature of the disc is 500~600℃, the calcination time is 3~6h, and the heating rate and cooling rate are 4~6℃ / min.
[0011] Preferably, in step S5, the calcination temperature of the intermediate product A is 1000~1150℃, the content of the CO / Ar mixed atmosphere is 5%~10%, the calcination time is 1~2h, the heating rate and cooling rate are 8~10℃ / min, and the heating and cooling processes are carried out under an Ar atmosphere.
[0012] Preferably, in step S6, the calcination temperature of the intermediate product B is 800~950℃, the content of the CO / Ar mixed atmosphere is 5%~10%, the calcination time is 1~2h, the heating rate and cooling rate are 5~8℃ / min, and the heating and cooling processes are carried out under an Ar atmosphere.
[0013] Preferably, in step S7, the calcination temperature of the intermediate product C is 500~650℃, the content of the CO / Ar mixed atmosphere is 5%~10%, the calcination time is 1~2h, the heating rate and cooling rate are 4~6℃ / min, and the heating and cooling processes are carried out under an Ar atmosphere.
[0014] Compared with the prior art, the beneficial effects of the present invention are: (1) This invention prepares a perovskite-type sodium ion anode material with in-situ precipitation of nano-high entropy alloy by sol-gel method. The metal nitrate raw material is cheap and readily available, the preparation process is simple and easy to control, and the reaction conditions are mild. (2) The perovskite-type anode material prepared by the present invention has a stable layered structure, which can effectively alleviate the volume expansion caused by the insertion and extraction of sodium ions and improve the energy density of sodium-ion battery anode. (3) The in-situ precipitated high-entropy nano-alloy particles prepared by the present invention are stably anchored on the surface of the perovskite matrix. Due to the high-entropy effect, the nanoparticles have excellent structural stability and catalytic activity, which is beneficial to improving the conductivity and capacity retention of the sodium-ion battery anode. (4) The present invention achieves in-situ composition transformation of nanoparticles on the surface of perovskite matrix from Fe→FeCu→FeCuNiAlMn through a stepwise thermal calcination process, while maintaining the nanoscale size and uniform distribution of alloy particles, which is conducive to the precise control of the composition and performance of nano high-entropy alloy particles. Attached Figure Description
[0015] Figure 1 This is a schematic diagram of the preparation process of in-situ precipitation of nano-high-entropy alloy particles on the surface of a perovskite matrix in Examples 1, 2, and 3 of the present invention; Figure 2 LaFe prepared in Example 1 of this invention 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 Microstructure of O3@FeCuNiAlMn; Figure 3 LaFe prepared in Example 1 of this invention 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3 and LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 XRD diffraction pattern of O3@FeCuNiAlMn; Figure 4 This is a charge-discharge curve of the sodium-ion half-cell prepared in Example 1 of the present invention. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0017] Example 1 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 After accurately weighing the stoichiometric ratio of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution. S2: Stir the solution in a water bath at 80℃ for 6 hours, add citric acid, and continue stirring until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1. S3: The sol was dried in a 100℃ forced-air drying oven for 10 hours to obtain a dry gel, and then ground for 20 minutes to obtain the precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 500℃ for 5 hours, with the heating and cooling rates controlled at 5℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3; S5: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3 discs were calcined at 1100℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 10℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@Fe; S6: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@Fe discs were calcined at 900℃ in a 10% CO / Ar mixed atmosphere for 1 hour, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloy with in-situ precipitated nano-FeCu alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@FeCu; S7: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1O3@FeCu discs were calcined at 500℃ for 2 hours in a 10% CO / Ar mixed atmosphere, with the heating and cooling rates controlled at 6℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloys with in-situ precipitated nano-FeCuNiAlMn high-entropy alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@FeCuNiAlMn sodium-ion battery anode material.
[0018] Example 2 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 After accurately weighing the stoichiometric ratio of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution. S2: Stir the solution in a water bath at 70°C for 5 hours, add citric acid, and continue stirring until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1. S3: The sol was dried in a 200℃ forced-air drying oven for 8 hours to obtain a dry gel, and then ground for 30 minutes to obtain the precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 600℃ for 4 hours, with the heating and cooling rates controlled at 6℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3; S5: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3 discs were calcined at 1000℃ in a 10% CO / Ar mixed atmosphere for 1 hour, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.2 Cu 0.2 Ni0.2 Al 0.2 Mn 0.2 O3@Fe; S6: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3@Fe discs were calcined at 850℃ in a 10% CO / Ar mixed atmosphere for 1.5 h, with the heating and cooling rates controlled at 10℃ / min. The heating and cooling processes were carried out in an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-FeCu alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3@FeCu; S7: The intermediate product C discs were calcined at 550℃ in a 10% CO / Ar mixed atmosphere for 1 h, with the heating and cooling rates controlled at 6℃ / min. The heating and cooling processes were carried out under an Ar atmosphere to obtain LaFe with in-situ precipitation of nano-FeCuNiAlMn high-entropy alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3@FeCuNiAlMn sodium-ion battery anode material.
[0019] Example 3 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 After accurately weighing the stoichiometric amount of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution.
[0020] S2: Stir the solution in a water bath at 60°C for 4 hours, add citric acid, and continue stirring until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1.
[0021] S3: Place the sol in a 100℃ forced-air drying oven and dry for 8 hours to obtain a dry gel, then grind for 15 minutes to obtain the precursor powder.
[0022] S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 500℃ for 3 hours, with the heating and cooling rates controlled at 4℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3.
[0023] S5: LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3 discs were calcined at 1000℃ in a 5% CO / Ar mixed atmosphere for 1 h, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@Fe.
[0024] S6: LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@Fe discs were calcined at 800℃ in a 5% CO / Ar mixed atmosphere for 1 h, with the heating and cooling rates controlled at 5℃ / min. The heating and cooling processes were carried out in an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-FeCu alloy particles on the surface. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@FeCu.
[0025] S7: LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@FeCu discs were calcined at 500℃ for 1 h in a 5% CO / Ar mixed atmosphere, with the heating and cooling rates controlled at 4℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloys with in-situ precipitation of nano-FeCuNiAlMn high-entropy alloy particles on the surface. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2O3@FeCuNiAlMn sodium-ion battery anode material.
[0026] Comparative Example 1 S1: Combine La(NO3)3, Fe(NO3)3, and Cu(NO3)2 according to the chemical formula LaFe 0.3 Cu 0.7 After accurately weighing the stoichiometric amount of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution.
[0027] S2: Stir the solution in a water bath at 50°C for 5 hours, then add citric acid until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, and Cu(NO3)2 is 1:1.
[0028] S3: The sol was dried in a 100℃ forced-air drying oven for 10 hours to obtain a dry gel, which was then ground for 15 minutes to obtain the precursor.
[0029] S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 550℃ for 2 hours, with the heating and cooling rates controlled at 5℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.3 Cu 0.7 O3.
[0030] S5: LaFe 0.3 Cu 0.7 O3 discs were calcined at 900℃ in a 5% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 10℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.3 Cu 0.7 O3@Fe.
[0031] Comparative Example 2 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 After accurately weighing the stoichiometric ratio of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution. S2: Stir the solution in a water bath at 70°C for 6 hours, add citric acid, and continue stirring until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1. S3: The sol was dried in a 200℃ forced-air drying oven for 10 hours to obtain a dry gel, and then ground for 30 minutes to obtain the precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 600℃ for 3 hours, with the heating and cooling rates controlled at 5℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 O3; S5: LaFe 0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 O3 discs were calcined at 1000℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 O3@Fe; S6: LaFe 0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 O3@Fe discs were calcined at 900℃ in a 10% CO / Ar mixed atmosphere for 1 hour, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloy with in-situ precipitated nano-FeCu alloy particles on the surface. 0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 O3@FeCu; S7: The intermediate product C discs were calcined at 600℃ in a 10% CO / Ar mixed atmosphere for 1 h, with the heating and cooling rates controlled at 6℃ / min. The heating and cooling processes were carried out under an Ar atmosphere to obtain LaFe with in-situ precipitation of nano-FeCuNiAlMn high-entropy alloy particles on the surface.0.3 Cu 0.1 Ni 0.1 Al 0.1 Mn 0.1 O3@FeCuNiAlMn sodium-ion battery anode material.
[0032] Comparative Example 3 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 After accurately weighing the stoichiometric ratio of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution. S2: Stir the solution in a water bath at 65°C for 6 hours, add citric acid, until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:2. S3: The sol was dried in a 200℃ forced-air drying oven for 8 hours to obtain a dry gel, and then ground for 30 minutes to obtain the precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined at 600℃ in air for 4 hours, with the heating and cooling rates controlled at 5℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3; S5: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3 discs were calcined at 1100℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3@Fe; S6: LaFe 0.2 Cu 0.2 Ni 0.2Al 0.2 Mn 0.2 O3@Fe discs were calcined at 900℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloy with in-situ precipitated nano-FeCu alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3@FeCu; S7: The intermediate product C discs were calcined at 600℃ in a 10% CO / Ar mixed atmosphere for 1 h, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere to obtain LaFe with in-situ precipitation of nano-FeCuNiAlMn high-entropy alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.2 Mn 0.2 O3@FeCuNiAlMn sodium-ion battery anode material.
[0033] Comparative Example 4 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 After accurately weighing the stoichiometric ratio of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution. S2: Stir the solution in a water bath at 80℃ for 6 hours, add citric acid, and continue stirring until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1. S3: The sol was dried in a 150℃ forced-air drying oven for 10 hours to obtain a dry gel, and then ground for 20 minutes to obtain the precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 500℃ for 5 hours, with the heating and cooling rates controlled at 5℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3; S5: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3 discs were calcined at 1300℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 10℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@Fe; S6: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@Fe discs were calcined at 1200℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 8℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloy with in-situ precipitated nano-FeCu alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@FeCu; S7: LaFe 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@FeCu discs were calcined at 900℃ in a 10% CO / Ar mixed atmosphere for 2 hours, with the heating and cooling rates controlled at 6℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloys with in-situ precipitated nano-FeCuNiAlMn high-entropy alloy particles on the surface. 0.2 Cu 0.2 Ni 0.2 Al 0.3 Mn 0.1 O3@FeCuNiAlMn sodium-ion battery anode material.
[0034] Comparative Example 5 S1: Combine La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, Mn(NO3)2 according to the chemical formula LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2After accurately weighing the stoichiometric amount of O3, it was completely dissolved in deionized water and stirred thoroughly to obtain a homogeneous solution.
[0035] S2: Stir the solution in a water bath at 60°C for 4 hours, add citric acid, and continue stirring until a viscous sol is obtained. The ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:1.
[0036] S3: The sol was dried in a 200℃ forced-air drying oven for 10 hours to obtain a dry gel, which was then ground for 15 minutes to obtain the precursor powder.
[0037] S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are calcined in air at 500℃ for 3 hours, with the heating and cooling rates controlled at 4℃ / min, to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3.
[0038] S5: LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3 discs were calcined at 1000℃ in a 5% CO / Ar mixed atmosphere for 1 h, with the heating and cooling rates controlled at 4℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe with in-situ precipitated nano-Fe particles on the surface. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@Fe.
[0039] S6: LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@Fe discs were calcined at 800℃ for 1 hour in a 5% CO / Ar mixed atmosphere, with the heating and cooling rates controlled at 2℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloy with in-situ precipitated nano-FeCu alloy particles on the surface. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@FeCu.
[0040] S7: LaFe 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@FeCu discs were calcined at 500℃ for 1 h in a 5% CO / Ar mixed atmosphere, with the heating and cooling rates controlled at 10℃ / min. The heating and cooling processes were carried out under an Ar atmosphere, resulting in LaFe alloys with in-situ precipitation of nano-FeCuNiAlMn high-entropy alloy particles on the surface. 0.3 Cu 0.2 Ni 0.2 Al 0.1 Mn 0.2 O3@FeCuNiAlMn sodium-ion battery anode material.
[0041] In the embodiments and comparative examples of the present invention, in step S4, the binder is phenolic resin, and the precursor powder and the binder are mixed in a ratio of 10:1.
[0042] Half-cell performance testing methods 80 wt.% of the negative electrode materials prepared in each example and comparative example, 13 wt.% of the conductive agent (CABOT BP2000), and 7 wt.% of the binder (PVDF) were ground in a mortar for 40 min, sieved, and poured into a glass bottle. NMP was added, and the mixture was stirred for 12 h to form a homogeneous fluid slurry. The slurry was then coated onto carbon-coated Al foil, baked in an oven at 45°C for 0.5 h, and then dried in a vacuum drying oven at 110°C for 12 h. Finally, the electrode was removed and cut into appropriately sized electrode discs using a manual slicer. Using a sodium metal sheet as the counter electrode, 1 mol / L NaClO4 dissolved in ethylene carbonate solution as the electrolyte, and glass fiber GF / A as the separator, button half-cells were assembled in an argon glove box. Battery charge-discharge performance was tested at room temperature.
[0043] The half-cell performance test results are shown in Table 1.
[0044] Table 1 In this invention, a three-step calcination process is used in Examples 1, 2, and 3 to achieve LaFe x1 Cu x2 Ni x3 Al x4 Mn x5 Nano-sized FeCuNiAlMn high-entropy alloy particles gradually precipitate on the O3 surface, such as Figure 1 As shown. In step S5, the high-temperature calcination at 1000~1150℃ causes LaFe... x1 Cux2 Ni x3 Al x4 Mn x5 Fe atoms at the B site in O3 exsolve, thus precipitating nano-sized Fe particles, namely LaFe, on the surface. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@Fe, the medium-temperature calcination at 800~950℃ in step S5 makes LaFe x1 Cu x2 Ni x3 Al x4 Mn x5 The Cu atoms at the B sites in O3@Fe exsolve, thus forming nano-FeCu alloy particles on the surface, namely LaFe. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@FeCu, the low-temperature calcination at 500~650℃ in step seven results in LaFe x1 Cu x2 Ni x3 Al x4 Mn x5 In O3@FeCu, the Ni, Al, and Mn atoms at the B sites also undergo exsolution, ultimately forming nano-FeCuNiAlMn high-entropy alloy particles precipitated on the surface, namely LaFe. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@FeCu@FeCuNiAlMn.
[0045] In Example 1, LaFe 0.2 Cu 0.2 Ni 0.2 A l0.3 Mn 0.1 O3 surface precipitates FeCuNiAlMn high-entropy alloy particles with a size of 15~20nm, such as Figure 2 As shown. Figure 3 XRD results show that the precipitation of FeCuNiAlMn high-entropy alloy particles did not change the perovskite lattice structure of the substrate, which is beneficial to improving the LaFe 0.2 Cu 0.2 Ni 0.2 A l0.3 Mn 0.1 Charge-discharge cycle performance of O3@FeCuNiAlMn anode material.
[0046] Example 1: Charge-discharge cycle performance at a current density of 1C = 300 mA / g, with 1 mol / L NaClO4 dissolved in ethylene carbonate solution, and a voltage window of 2.5-4.0 V, is as follows: Figure 4 As shown in Table 1, the half-cell performance test results of the Examples and Comparative Example 1 are as follows. Compared with Comparative Example 1, due to the precipitation of nano-FeCuNiAlMn high-entropy alloy particles, its high-entropy effect exhibits excellent structural stability and catalytic activity, and the first-cycle charge specific capacity, first-cycle discharge specific capacity, and first-cycle coulombic efficiency are all significantly improved.
[0047] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys, characterized in that, Includes the following steps: S1: Dissolve La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 completely in deionized water and stir thoroughly to obtain a homogeneous solution; S2: Stir the solution in a water bath, add citric acid, until a viscous sol is obtained; S3: Dry the sol to obtain a dry gel, and then grind it to obtain a precursor powder; S4: The precursor powder and binder are mixed evenly, then pressed into discs in a mold. The discs are then calcined in air to obtain a high-entropy perovskite oxide LaFe with a single-phase structure. x1 Cu x2 Ni x3 Al x4 Mn x5 O3, i.e., intermediate product A; S5: The intermediate product A discs were calcined at high temperature in a CO / Ar mixed atmosphere (1000-1150℃, CO content 5%-10%, calcination time 1-2 h, heating and cooling rates 8-10℃ / min, all under an Ar atmosphere), to obtain a perovskite oxide LaFe with in-situ precipitated nano-Fe particles on the surface. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@Fe, i.e., intermediate product B; S6: The intermediate product B discs were calcined at a moderate temperature in a CO / Ar mixed atmosphere (800-950℃, CO / Ar content 5%-10%) for 1-2 hours. The heating and cooling rates were 5-8℃ / min, and the heating and cooling processes were carried out in an Ar atmosphere. This yielded perovskite oxide LaFe with in-situ precipitated nano-FeCu alloy particles on the surface. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@FeCu, i.e., intermediate product C; S7: The intermediate product C wafers were calcined at low temperature in a CO / Ar mixed atmosphere (500-650℃, CO / Ar content 5%-10%) for 1-2 hours. The heating and cooling rates were 4-6℃ / min, and the heating and cooling processes were carried out in an Ar atmosphere. This yielded a perovskite-type sodium-ion battery anode material with in-situ precipitated nano-FeCuNiAlMn high-entropy alloy particles, namely LaFe. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@FeCuNiAlMn.
2. The method for preparing perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys according to claim 1, characterized in that, The total amount of Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 mentioned in step S1 is in a ratio of 1:1 to La(NO3)3.
3. The method for preparing perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys according to claim 1, characterized in that, In step S2, the water bath temperature is 60~80℃ and the stirring time is 4~6h.
4. The method for preparing perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys according to claim 1, characterized in that, In step S2, the ratio of the amount of citric acid to the total amount of La(NO3)3, Fe(NO3)3, Cu(NO3)2, Ni(NO3)2, Al(NO3)3, and Mn(NO3)2 is 1:
1.
5. The method for preparing perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys according to claim 1, characterized in that, In step S3, the sol is dried by a blower dryer at a temperature of 100-200°C for 8-12 hours.
6. The method for preparing perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys according to claim 1, characterized in that, In step S4, the calcination temperature of the disc is 500~600℃, the calcination time is 3~6h, and the heating rate and cooling rate are 4~6℃ / min.
7. A perovskite-type sodium-ion battery anode material with in-situ precipitation of nano-high-entropy alloys, characterized in that, The material is prepared according to any one of claims 1-6, and its general formula is LaFe. x1 Cu x2 Ni x3 Al x4 Mn x5 O3@FeCuNiAlMn, where x1+x2+x3+x4+x5=1, and FeCuNiAlMn are nano-high-entropy alloy particles precipitated on the surface of the negative electrode material.
Citation Information
Patent Citations
Bismuth oxychloride and sulfur-nitrogen co-doped carbon quantum dots composite sodium ion battery negative electrode material and preparation method
CN119143176B
Preparation method and application of sodium ion battery negative electrode material
CN119591080A
Asphalt-based hard carbon negative electrode material with high initial efficiency, high magnification and high capacity and preparation method of asphalt-based hard carbon negative electrode material
CN119601621A
One-step synthesized perovskite oxide NaTaO3 sodium-ion battery negative electrode material and preparation method thereof
CN107381640A
High-entropy perovskite oxide for in-situ precipitation of high-entropy alloy and preparation method of high-entropy perovskite oxide
CN119612617A