A high-temperature-resistant leak-proof sealing gasket and a preparation method thereof
By preparing vermiculite-based composite fillers and compounding them with nitrile rubber, the problems of insufficient heat resistance and oxidation resistance of gaskets in high-temperature environments were solved, and the stable use and performance improvement of gaskets in high-temperature environments were achieved.
Patent Information
- Application Number
- CN202510573944.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-06
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-05-06
AI Technical Summary
Existing gaskets have insufficient heat resistance and oxidation resistance in high-temperature environments, and are also expensive, making them difficult to meet long-term use requirements.
A high-temperature resistant and leak-proof sealing gasket was prepared by compounding vermiculite-based composite filler with nitrile rubber and then performing in-situ graphene growth, carbon dot deposition, and polymer resin intercalation, thereby improving its heat resistance and sealing performance.
It significantly improves the high-temperature resistance, oxidation resistance, and sealing performance of gaskets, reduces costs, and enables long-term stable use in high-temperature environments.
Smart Images

Figure CN120441930B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sealing materials, and in particular to a high-temperature resistant leak-proof sealing gasket and its preparation method. Background Technology
[0002] Gaskets are widely used for sealing various equipment in modern industry. They can be classified into metal gaskets and non-metal gaskets based on their material. Rubber gaskets are a typical type of non-metallic gasket, widely used due to their long service life and good sealing performance.
[0003] With the rapid development of industry, higher requirements are being placed on the performance of gaskets. For example, gaskets used in heat exchangers and heating equipment need to operate at temperatures above 100°C for extended periods and at temperatures up to 150°C during intermittent operation. This poses a challenge to the high-temperature resistance of gaskets. Conventional rubber gaskets often cannot meet the long-term use requirements under high-temperature environments, or they age faster when used in high-temperature environments, resulting in a significantly shortened service life.
[0004] Patent CN118374036A discloses a high-performance composite gasket and its preparation method, which is the applicant's previous research result. It can give the gasket system excellent antioxidant properties by compounding reduced carbon dots, modified multi-walled carbon nanotubes, modified carbon fibers and other materials to prepare anti-aging reinforced modified composite particles, thereby improving the anti-aging effect. However, the carbon nanotubes and other materials used are expensive, and their heat and oxygen aging resistance needs to be further improved.
[0005] Vermiculite is an inexpensive, lamellar silicate mineral with stable chemical properties and excellent thermal insulation, sound insulation, antibacterial properties, and cold resistance. When heated, the evaporation of moisture within its structure causes the vermiculite to expand in volume. The expanded vermiculite has a low bulk density, stable chemical properties, and excellent temperature resistance, thermal insulation, wear resistance, and corrosion resistance (Qian Yupeng, Jiang Xuefeng, He Yicheng, et al. Preparation of high-expansion-rate expanded vermiculite by composite method [J]. Bulletin of the Chinese Ceramic Society, 2017, 36(9):5.DOI:CNKI:SUN:GSYT.0.2017-09-001.). Expanded vermiculite is used as a reinforcing filler in rubber systems or further in sealing materials. For example, patent CN107188453B discloses a method for preparing a vermiculite-based high-temperature resistant sealing material, and patent CN115650632B discloses a high-temperature resistant vermiculite-based composite sealing gasket and its preparation method. Therefore, applying expanded vermiculite to rubber gasket materials is expected to improve their heat resistance and reduce their cost. However, expanded vermiculite has poor compatibility with rubber systems and is also brittle and prone to pulverization. The aforementioned patents have not effectively solved this problem.
[0006] Therefore, it is now necessary to improve existing technologies to provide more reliable solutions. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to provide a high-temperature resistant leak-proof sealing gasket and its preparation method, which addresses the shortcomings of the prior art.
[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: In its first aspect, the present invention provides a high-temperature resistant, leak-proof sealing gasket, the raw materials for which are prepared include the following components by weight: 100 parts of nitrile rubber; 26-39 parts of vermiculite-based composite filler; 2-7 parts zinc oxide; 3-8 parts paraffin oil; 2.5-9 parts of silica; 1-6 parts of vulcanizing agent; Stearic acid 0.8-2.4 parts; Vulcanization accelerator: 0.5-1.7 parts; The vermiculite-based composite filler was prepared by the following method: S1. Preparation of composite modified vermiculite: Expanded vermiculite is subjected to in-situ growth of graphene, carbon dot deposition, organic treatment and polymer resin intercalation treatment to obtain composite modified vermiculite; S2, glass fiber pretreatment; S3. The pretreated glass fiber is coated with composite modified vermiculite to obtain vermiculite-based composite filler.
[0009] Preferably, step S1 specifically includes: S1-1, In-situ grown graphene: Expanded vermiculite, copper chloride, and ruthenium trichloride were added to an aqueous solution of citric acid, ultrasonically treated, and then heated to dryness. The resulting product was pretreated under a hydrogen atmosphere and under heating, and then heated and reacted in a mixed gas composed of argon, ethylene, and hydrogen. After the reaction was completed, it was cooled to obtain graphene-composite expanded vermiculite. S1-2, Carbon point deposition: Graphene-composite expanded vermiculite, citric acid, and mercaptopropionic acid were added to a mixed solution of ethanol and deionized water, stirred, and then glucose and 1,2-cyclohexanediamine were added. The mixture was ultrasonically dispersed, and the resulting mixture was transferred to a reaction vessel and subjected to hydrothermal reaction under heating. After the reaction was completed, the mixture was cooled, centrifuged and filtered, the solid product was washed, and vacuum dried to obtain supported vermiculite. S1-3, Organic treatment: Loaded vermiculite and hexadecyltrimethylammonium bromide were added to deionized water, stirred, filtered, the solid product was washed and dried to obtain organic vermiculite; S1-4, Polymer resin intercalation treatment: Ethylene propylene diene monomer (EPDM) rubber and maleic anhydride were added to xylene, heated and stirred, and a xylene solution containing benzoyl peroxide was added dropwise. After the addition was complete, the reaction was carried out to obtain a polymer resin solution. Organic vermiculite and butyl rubber were added to a polymer resin solution, heated and stirred under reflux. After the reaction was completed, the mixture was filtered, the solid product was washed, and vacuum dried to obtain composite modified vermiculite.
[0010] Preferably, step S1 specifically includes: S1-1, In-situ grown graphene: Take 0.5-2g of expanded vermiculite, 0.033-0.134g of copper chloride, and 0.026-0.104g of ruthenium trichloride and add them to 50-200mL of citric acid aqueous solution with a mass concentration of 2.5-10%. Sonicate for 15-60min and heat to dryness at 120-150℃. Transfer the obtained product to a tube furnace and pretreat at 750-900℃ for 5-20min in a hydrogen atmosphere. Then, heat at 880-1000℃ for 15-60min in a mixed gas atmosphere with a volume ratio of argon:ethylene:hydrogen of 2:2:1 and cool to room temperature to obtain graphene-composite expanded vermiculite. S1-2, Carbon point deposition: Take 1-4g of graphene-composite expanded vermiculite, 0.42-1.90g of citric acid, and 0.21-0.84g of mercaptopropionic acid and add them to a mixed solution consisting of 30-120mL of ethanol and 20-80mL of deionized water. Stir under sealed conditions for 5-30min. Then add 0.24-0.96g of glucose and 0.06-0.24g of 1,2-cyclohexanediamine. Disperse the mixture under sealed conditions using ultrasonication for 10-40min. Transfer the resulting mixture to a reaction vessel and hydrothermally react at 180-230℃ for 4-16h. Cool to room temperature, centrifuge and filter. Wash the solid product with ethanol and deionized water sequentially, and vacuum dry at 70-100℃ for 6-24h to obtain supported vermiculite. S1-3, Organic treatment: Take 0.5-2g of supported vermiculite and 0.1-0.4g of hexadecyltrimethylammonium bromide and add them to 50-200mL of deionized water. Stir for 1-4h, filter, wash the solid product with deionized water, and dry to constant weight to obtain organic vermiculite. S1-4, Polymer resin intercalation treatment: Take 0.25-1g of EPDM rubber and 0.025-0.1g of maleic anhydride and add them to 45-180mL of xylene. Stir at 90-110℃ for 5-30min while maintaining stirring. Add 2.5-20mL of xylene solution containing 3-12mg of benzoyl peroxide dropwise over 10-30min. Then react for 1-4h to obtain a polymer resin solution. Take 0.5-2g of organomodified vermiculite and 0.1-0.4g of butyl rubber and add them to the polymer resin solution. Stir and reflux at 60-80℃ for 12-48h, filter, wash the solid product with acetone and ethanol in sequence, and dry it under vacuum to constant weight to obtain composite modified vermiculite.
[0011] Preferably, the expanded vermiculite is prepared by the following method: soaking vermiculite in hydrogen peroxide with a mass concentration of 5-20% for 2-8 hours, controlling the solid-liquid ratio to be 1:2-7, taking out the soaked vermiculite, calcining it at 400-500℃ for 1-5 minutes, cooling it to room temperature, and ball milling it to a particle size of less than 0.5-5μm to obtain expanded vermiculite.
[0012] Preferably, step S2 specifically involves: immersing the glass fiber in hydrochloric acid under heating, filtering, washing with deionized water until neutral, and vacuum drying to constant weight to obtain pretreated glass fiber.
[0013] Preferably, step S2 specifically involves: immersing the glass fiber in hydrochloric acid with a concentration of 0.5-2 mol / L at 40-50°C for 15-90 minutes, filtering, washing with deionized water until neutral, and vacuum drying at 90-120°C to constant weight to obtain the pretreated glass fiber.
[0014] Preferably, step S3 specifically includes: S3-1. Take the composite modified vermiculite and add it to a mixture of ethanol and deionized water, then disperse it by ultrasonication to obtain a vermiculite dispersion. S3-2. Add pretreated glass fiber to vermiculite dispersion, disperse ultrasonically, then stir under heating, raise the temperature, stir until dry, rinse the obtained product and dry under vacuum to constant weight to obtain vermiculite-based composite filler.
[0015] Preferably, step S3 specifically includes: S3-1. Take 0.5-2g of composite modified vermiculite and add it to 50-200mL of a mixture of ethanol and deionized water in a volume ratio of 1:1. Disperse the mixture by ultrasonication for 15-60min to obtain a vermiculite dispersion. S3-2. Add 0.25-0.1g of pretreated glass fiber to the vermiculite dispersion, ultrasonically disperse for 15-60min, then stir at 50-85℃ for 1-4h, raise the temperature to 95-105℃, stir until dry, rinse the product with deionized water and vacuum dry at 70-100℃ to constant weight to obtain vermiculite-based composite filler.
[0016] Preferably, the vulcanizing agent is selected from at least one of vulcanizing agents DCP, BIPB, or DBPH; The vulcanization accelerator is at least one of the following: vulcanization accelerator TMTD, vulcanization accelerator ZBX, vulcanization accelerator ZDMC, vulcanization accelerator NA-22, and vulcanization accelerator CZ.
[0017] In a first aspect, the present invention provides a method for preparing the high-temperature resistant, leak-proof sealing gasket as described above, comprising the following steps: 1) Internal mixing: Add nitrile rubber, vermiculite-based composite filler, zinc oxide, silica, and stearic acid to an internal mixer and mix at 75-95℃ for 2-10 minutes to obtain the internally mixed rubber compound; 2) Open milling: Add the internally mixed rubber compound, vulcanizing agent, paraffin oil and vulcanization accelerator into the open mill, mix at 55-78℃ for 5-25 minutes, discharge the material, place it in the injection molding machine to press into sheets to obtain raw rubber gaskets. 3) Vulcanization: The raw rubber gasket is vulcanized in a vulcanizing machine at 160-190℃ for 12-50 minutes and the vulcanization pressure is 5-25MPa to obtain the high temperature resistant and leak-proof sealing gasket.
[0018] The beneficial effects of this invention are: This invention provides a high-temperature resistant leak-proof sealing gasket and its preparation method. By preparing a multi-component composite filler with a special structural system based on expanded vermiculite, the vermiculite-based composite filler is used in combination with nitrile rubber, which can significantly improve the high-temperature resistance and thermo-oxidative aging resistance of nitrile rubber, and at the same time improve its sealing performance. This results in a significant improvement in the overall performance of the prepared sealing gasket, which can better meet the sealing requirements in high-temperature environments.
[0019] Vermiculite can significantly improve the heat resistance of nitrile rubber matrix and further enhance its wear resistance and corrosion resistance. However, vermiculite is brittle and prone to pulverization. Graphene can improve various properties of rubber, but it suffers from defects such as easy curling, easy agglomeration, and difficulty in dispersing in organic systems. Glass fiber has strong heat resistance, good corrosion resistance, and high mechanical strength, which can improve the mechanical properties and high-temperature resistance of rubber. However, it has shortcomings such as poor compatibility with organic systems, brittleness, and poor wear resistance. In the vermiculite-based composite filler structure system prepared in this invention, the multi-component components such as vermiculite, graphene, and glass fiber are organically combined through the design of a special composite structure system, which can effectively overcome the above-mentioned shortcomings, give full play to the reinforcing effect of each component, and further enhance the complementary effect through the mutual cooperation of each component. In addition, the introduction of carbon dots in the system also endows the system with excellent antioxidant effect.
[0020] In the vermiculite-based composite filler structure system of the present invention, graphene is grown in situ on the surface and between layers of vermiculite. Graphene with excellent mechanical strength forms a network-like structure that coats the vermiculite, which can significantly improve the brittleness of vermiculite and prevent it from pulverizing. The oxides formed by Cu and Ru can serve as stress nodes in the network structure, further improving its strength. On the other hand, the unique zero bandgap structure of graphene allows electrons and holes to move freely within it. Its combination with carbon dots can help improve the electron transport rate and promote the enhancement of the reducibility of carbon dots.
[0021] In the vermiculite-based composite filler structure system of the present invention, since graphene is grown in situ on the vermiculite surface, it can overcome the inherent defect of easy curling. Furthermore, the polymer resin intercalation treatment improves the compatibility of the entire system with the resin, and can simultaneously solve the problem of poor compatibility between vermiculite, graphene, glass fiber and resin system.
[0022] In the vermiculite-based composite filler structure system of this invention, vermiculite readily forms a dense physical layer structure within the nitrile rubber system, thereby improving sealing performance. The lamellar structure of vermiculite allows it to peel off to form a sheet-like reinforcing structure under stress or friction, contributing to enhanced wear resistance. Furthermore, the network coating structure of graphene on the vermiculite further enhances wear resistance and reduces the coefficient of friction, thus endowing the prepared gasket with excellent wear resistance. This allows it to maintain its sealing performance for extended periods even in high-friction environments, resisting wear and ensuring reliability during long-term use. The advantages of vermiculite and graphene in this performance also compensate for the insufficient wear resistance of glass fiber.
[0023] In the vermiculite-based composite filler structure system of the present invention, the introduction of reducing carbon points endows the vermiculite-based composite filler structure system with excellent antioxidant capacity. Combined with the improvement of high temperature resistance of the system by vermiculite, graphene and glass fiber, the vermiculite-based composite filler has excellent heat and oxygen aging resistance, thereby making up for the shortcomings of nitrile rubber in this respect.
[0024] In the vermiculite-based composite filler structure system of this invention, maleic anhydride-grafted EPDM rubber and butyl rubber are compounded as intercalation polymer resins. Besides improving the film-forming ability and compatibility with the nitrile rubber matrix, the vermiculite-based composite filler also has the following effects: maleic anhydride-grafted EPDM rubber has excellent heat resistance, ozone resistance, and weather resistance, which can improve the problems of poor high-temperature resistance and poor heat-oxygen aging resistance of butyl rubber; butyl rubber has excellent airtightness and watertightness, which can overcome the problems of insufficient airtightness and oil resistance of both EPDM rubber and nitrile rubber; therefore, the combination of maleic anhydride-grafted EPDM rubber and butyl rubber also has a significant improving effect on the overall performance of the nitrile rubber matrix. Attached Figure Description
[0025] Figure 1 The tensile strength test results are for the examples and comparative examples; Figure 2 The compression rebound rate test results are for the examples and comparative examples; Figure 3 The sealing performance test results are for the examples and comparative examples; Figure 4 The results of high-temperature resistance tests are for the examples and comparative examples; Figure 5 The results of heat and oxygen aging resistance tests are for the examples and comparative examples; Figure 6 The results of high-temperature wear resistance tests are for the examples and comparative examples; Figure 7 The infrared absorption spectrum of the supported vermiculite prepared in Example 1; Figure 8 The results show the antioxidant properties of the vermiculite-based composite fillers prepared in Example 1 and Comparative Examples 1-3. Detailed Implementation
[0026] The present invention will be further described in detail below with reference to embodiments, so that those skilled in the art can implement it based on the description.
[0027] It should be understood that terms such as “having,” “comprising,” and “including” as used herein do not exclude the presence or addition of one or more other elements or combinations thereof.
[0028] Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, the materials and reagents used in the following examples are commercially available. For examples where specific conditions are not specified, conventional conditions or conditions recommended by the manufacturer are followed. For reagents or instruments whose manufacturers are not specified, they are all commercially available products.
[0029] This invention provides a high-temperature resistant, leak-proof sealing gasket, the raw materials for which are prepared include the following components by weight: 100 parts of nitrile rubber; 26-39 parts of vermiculite-based composite filler; 2-7 parts zinc oxide; 3-8 parts paraffin oil; 2.5-9 parts of silica; 1-6 parts of vulcanizing agent; Stearic acid 0.8-2.4 parts; Vulcanization accelerator 0.5-1.7 parts.
[0030] The preparation method of the high-temperature resistant leak-proof sealing gasket includes the following steps: 1) Internal mixing: Add nitrile rubber, vermiculite-based composite filler, zinc oxide, silica, and stearic acid to an internal mixer and mix at 75-95℃ for 2-10 minutes to obtain the internally mixed rubber compound; 2) Open milling: Add the internally mixed rubber compound, vulcanizing agent, paraffin oil and vulcanization accelerator into the open mill, mix at 55-78℃ for 5-25 minutes, discharge the material, place it in the injection molding machine to press into sheets to obtain raw rubber gaskets. 3) Vulcanization: The raw rubber gasket is vulcanized in a vulcanizing machine at 160-190℃ for 12-50 minutes and the vulcanization pressure is 5-25MPa to obtain a high-temperature resistant and leak-proof sealing gasket.
[0031] The vermiculite-based composite filler was prepared by the following method: S1. Preparation of composite modified vermiculite: Expanded vermiculite is subjected to in-situ growth of graphene, carbon dot deposition, organic treatment, and polymer resin intercalation to obtain composite modified vermiculite; specific steps include: S1-1, In-situ grown graphene: Take 0.5-2g of expanded vermiculite, 0.033-0.134g of copper chloride, and 0.026-0.104g of ruthenium trichloride and add them to 50-200mL of citric acid aqueous solution with a mass concentration of 2.5-10%. Sonicate for 15-60min and heat to dryness at 120-150℃. Transfer the obtained product to a tube furnace and pretreat at 750-900℃ for 5-20min in a hydrogen atmosphere. Then, heat at 880-1000℃ for 15-60min in a mixed gas atmosphere with a volume ratio of argon:ethylene:hydrogen of 2:2:1 and cool to room temperature to obtain graphene-composite expanded vermiculite. Expanded vermiculite is prepared by the following method: vermiculite is soaked in hydrogen peroxide with a mass concentration of 5-20% for 2-8 hours, and the solid-liquid ratio is controlled at 1:2~7. After soaking, the vermiculite is taken out, calcined at 400-500℃ for 1-5 minutes, cooled to room temperature, and ball-milled until the particle size is below 0.5-5μm to obtain expanded vermiculite.
[0032] S1-2, Carbon point deposition: Take 1-4g of graphene-composite expanded vermiculite, 0.42-1.90g of citric acid, and 0.21-0.84g of mercaptopropionic acid and add them to a mixed solution consisting of 30-120mL of ethanol and 20-80mL of deionized water. Stir under sealed conditions for 5-30min. Then add 0.24-0.96g of glucose and 0.06-0.24g of 1,2-cyclohexanediamine. Disperse the mixture under sealed conditions using ultrasonication for 10-40min. Transfer the resulting mixture to a reaction vessel and hydrothermally react at 180-230℃ for 4-16h. Cool to room temperature, centrifuge and filter. Wash the solid product with ethanol and deionized water sequentially, and vacuum dry at 70-100℃ for 6-24h to obtain supported vermiculite. S1-3, Organic treatment: Take 0.5-2g of supported vermiculite and 0.1-0.4g of hexadecyltrimethylammonium bromide and add them to 50-200mL of deionized water. Stir for 1-4h, filter, wash the solid product with deionized water, and dry to constant weight to obtain organic vermiculite. S1-4, Polymer resin intercalation treatment: Take 0.25-1g of EPDM rubber and 0.025-0.1g of maleic anhydride and add them to 45-180mL of xylene. Stir at 90-110℃ for 5-30min while maintaining stirring. Add 2.5-20mL of xylene solution containing 3-12mg of benzoyl peroxide dropwise over 10-30min. Then react for 1-4h to obtain a polymer resin solution. This polymer resin solution is the maleic anhydride-grafted EPDM rubber (EPDM-g-MAH) solution. Take 0.5-2g of organomodified vermiculite and 0.1-0.4g of butyl rubber and add them to the polymer resin solution. Stir and reflux at 60-80℃ for 12-48h, filter, wash the solid product with acetone and ethanol in sequence, and dry it under vacuum to constant weight to obtain composite modified vermiculite.
[0033] S2, Glass fiber pretreatment: Glass fibers are immersed in hydrochloric acid with a concentration of 0.5-2 mol / L at 40-50℃ for 15-90 min, filtered, washed with deionized water until neutral, and vacuum dried at 90-120℃ to constant weight to obtain pretreated glass fibers.
[0034] S3. The pretreated glass fiber is coated with composite modified vermiculite to obtain vermiculite-based composite filler: S3-1. Take 0.5-2g of composite modified vermiculite and add it to 50-200mL of a mixture of ethanol and deionized water in a volume ratio of 1:1. Disperse the mixture by ultrasonication for 15-60min to obtain a vermiculite dispersion. S3-2. Add 0.25-0.1g of pretreated glass fiber to the vermiculite dispersion, ultrasonically disperse for 15-60min, then stir at 50-85℃ for 1-4h, raise the temperature to 95-105℃, stir until dry, and use deionized water to lightly rinse the product to remove the uncoated composite modified vermiculite on the surface. Then vacuum dry at 70-100℃ to constant weight to obtain vermiculite-based composite filler.
[0035] In a preferred embodiment, the vulcanizing agent is selected from at least one of vulcanizing agents DCP, BIPB, or DBPH.
[0036] In a preferred embodiment, the vulcanization accelerator is at least one of vulcanization accelerator TMTD, vulcanization accelerator ZBX, vulcanization accelerator ZDMC, vulcanization accelerator NA-22, and vulcanization accelerator CZ.
[0037] Nitrile rubber (NBR) possesses excellent oil resistance, abrasion resistance, and strength, making it a commonly used material for preparing sealing gaskets. However, it suffers from poor high-temperature resistance and poor resistance to thermo-oxidative aging. This invention addresses this issue by preparing a multi-component composite filler with a special structural system based on expanded vermiculite. The vermiculite-based composite filler, when used in combination with NBR, significantly improves the high-temperature resistance and thermo-oxidative aging resistance of NBR, while simultaneously enhancing its sealing performance. This results in a significant improvement in the overall performance of the prepared sealing gasket, better meeting the sealing requirements under high-temperature environments. The following detailed explanation of the mechanism of action of the vermiculite-based composite filler, along with specific preparation steps, will facilitate understanding of this invention.
[0038] Vermiculite is a lamellar silicate mineral. When heated, the volume of vermiculite expands due to the evaporation of water within its structure. The expanded vermiculite has a low bulk density, stable chemical properties, and excellent temperature resistance, heat insulation, wear resistance, and corrosion resistance (Qian Yupeng, Jiang Xuefeng, He Yicheng, et al. Preparation of high expansion rate expanded vermiculite by composite method [J]. Bulletin of the Chinese Ceramic Society, 2017, 36(9):5.DOI:CNKI:SUN:GSYT.0.2017-09-001.), (Jing Lulu, Guo Fang, Jing Lvlu, et al. Tribological properties of PBO fiber fabric lining material filled with organic vermiculite [J]. Lubrication and Sealing, 2014, 39(7):6.DOI:10.3969 / j.issn.0254-0150.2014.07.015.). The main preparation mechanism of the vermiculite-based composite filler in this invention is as follows: 1. Preparation of composite modified vermiculite: (1) This invention first prepares expanded vermiculite by combining hydrogen peroxide soaking with high-temperature heat treatment. Hydrogen peroxide soaking removes some impurities from the vermiculite, and the oxygen pressure generated by the subsequent decomposition of H2O2 molecules into the vermiculite interlayers at high temperatures promotes the dissociation and expansion of the structural layers, thus promoting expansion and improving expansion efficiency and treatment effect. The increased interlayer spacing of the expanded vermiculite provides conditions for subsequent interlayer deposition of graphene and carbon dots, as well as the insertion of organic molecules, resin polymers, etc. Expanded vermiculite can also improve the sound insulation performance of the prepared sealing gaskets.
[0039] (2) Then, graphene was loaded onto the surface and between the layers of vermiculite using in-situ growth method by chemical vapor deposition to obtain graphene composite expanded vermiculite; The specific method is as follows: In a weakly acidic solution, Cu2+ and Ru3+ are first loaded onto expanded vermiculite. Then, under the action of high temperature and reducing gas hydrogen, Cu2+ and Ru3+ are converted into elemental Cu and elemental Ru. Both elemental Cu and Ru have a catalytic effect on the chemical vapor deposition of graphene (Jin Yan, Yang Qian, Zhao Wenbin, et al. Study on controllable catalytic reaction system for graphene chemical vapor deposition [J]. Journal of Chemical Industry and Engineering (China), 2020). 71(6):22.DOI:10.11949 / 0438-1157.20200107.), then using ethylene as a carbon source, hydrogen as a reducing gas, and elemental Cu and Ru as composite catalysts (the two composites can play a synergistic enhancement role), graphene was grown in situ on expanded vermiculite at high temperature. Since elemental Cu and Ru are uniformly loaded on the surface and between layers of expanded vermiculite, they can promote full contact between the composite catalyst and the carbon source, promote the aggregation of carbon atoms in the gas phase into graphene structure, significantly improve its catalytic efficiency in promoting graphene growth, and increase the loading of graphene.
[0040] (3) Carbon dots are synthesized in situ on expanded vermiculite through hydrothermal reaction. In this process, graphene-composite expanded vermiculite is first mixed with citric acid and mercaptopropionic acid. In a weakly acidic solution, elemental Cu in graphene-composite expanded vermiculite can form a large amount of Cu2+ on the surface. Raw material precursors such as glucose and 1,2-cyclohexanediamine are combined with Cu2+ through electrostatic adsorption, coordination and other processes. Then, through high-temperature hydrothermal reaction, a large number of uniformly loaded carbon dots are deposited on graphene-composite expanded vermiculite. Cu2+ forms oxides to play a connecting role and together with Ru, it also plays a doping effect on carbon dots. In this process, citric acid and mercaptopropionic acid provide an acidic environment and also serve as carbon and sulfur sources in the subsequent synthesis of carbon dots. Mercaptopropionic acid has good reducing properties, and the prepared carbon dots inherit the reducing properties of the precursor, resulting in excellent antioxidant properties. The doping effect of Cu and Ru on the carbon dots enhances their antioxidant properties by increasing electron cloud density and electron transport rate. Furthermore, the carbon dots exert their antioxidant effect by capturing reactive oxygen species in the system. Because the carbon dots are heavily loaded on the surface and between layers of expanded vermiculite and are stably connected to it, they do not exhibit free aggregation or surface migration in the nitrile rubber system, thus exhibiting stable antioxidant properties without affecting the mechanical strength of the nitrile rubber system. Moreover, the interlayer loading of the carbon dots gives their antioxidant properties a long-lasting effect.
[0041] (4) Then, the expanded vermiculite was organically treated by hexadecyltrimethylammonium bromide. Finally, maleic anhydride-grafted EPDM rubber and butyl rubber were intercalated by solution method to fill the interlayer of expanded vermiculite with a large amount of grafted resin composite to obtain composite modified vermiculite. The intercalation of polymer resin can greatly improve the compatibility and interfacial bonding strength between expanded vermiculite and nitrile rubber system, and can also enhance the coating film-forming performance of expanded vermiculite, which is beneficial for subsequent coating treatment of glass fiber. In this process, EPDM rubber is first subjected to maleic anhydride grafting treatment to obtain a polymer resin solution, namely maleic anhydride-grafted EPDM rubber resin (EPDM-g-MAH) solution. Maleic anhydride grafting treatment can toughen and compatibilize EPDM rubber, improve its mechanical properties and compatibility with nitrile rubber matrix; then, together with butyl rubber and organo-modified vermiculite, resin intercalation of expanded vermiculite is achieved in the solution under stirring and reflux.
[0042] 2. Coating of glass fiber with composite modified vermiculite: First, glass fibers are acid-soaked to improve surface roughness, increase fiber surface area, improve fiber-resin wettability and interfacial adhesion strength, and form abundant silanol groups on the glass fiber surface. Then, the acid-treated glass fibers are dispersed in a vermiculite dispersion. Under heating and stirring, the solution gradually evaporates, and micron-sized composite modified vermiculite gradually precipitates onto the glass fiber surface, achieving coating. Finally, a vermiculite-based composite filler is prepared. The polymer resin intercalated in the composite modified vermiculite effectively promotes film formation, improving coating efficiency and density. Simultaneously, because the glass fiber surface contains abundant silanol groups, and the composite modified vermiculite forms copper ions on its surface in the mixture, the coordination and binding of these copper ions with the silanol groups promotes the coating process.
[0043] Vermiculite can significantly improve the heat resistance of nitrile rubber matrices and further enhance their wear resistance and corrosion resistance; however, it suffers from brittleness and a tendency to pulverize. Graphene can improve various properties of rubber, but it is prone to curling, agglomeration, and dispersion in organic systems. Glass fiber exhibits strong heat resistance, good corrosion resistance, and high mechanical strength, which can improve the mechanical properties and high-temperature resistance of rubber; however, it suffers from poor compatibility with organic systems, brittleness, and relatively poor wear resistance. Therefore, while inorganic fillers such as vermiculite, graphene, and glass fiber can all reinforce rubber in some aspects, they inevitably possess certain shortcomings that limit their application effectiveness. In the vermiculite-based composite filler structure system prepared by this invention, vermiculite, graphene, glass fiber, and other multi-component components are organically combined through a special composite structure design. This effectively overcomes the aforementioned shortcomings, fully utilizes the reinforcing effect of each component, and further enhances the complementary effect through the mutual cooperation of each component. In addition, the introduction of carbon dots into the system endows it with excellent antioxidant properties. The synergistic mechanism of the components in the vermiculite-based composite filler is as follows: (1) Graphene is a two-dimensional honeycomb carbon material with six-membered rings formed by sp2 hybridization between carbon atoms as the basic unit cell. It has excellent mechanical strength and high temperature resistance. Graphene is grown in situ on the surface and between layers of vermiculite. The graphene with excellent mechanical strength forms a network-like structure to coat vermiculite, which can significantly improve the brittleness of vermiculite and prevent it from pulverizing. The oxides formed by Cu and Ru can serve as stress nodes in the network structure, further improving its strength. On the other hand, graphene's unique zero-bandgap structure allows both electrons and holes to move freely within it. The electron mobility of graphene can reach approximately 200,000 cm²•V⁻¹•s⁻¹ (Jin Yan, Yang Qian, Zhao Wenbin, et al. Study on controllable catalytic reaction system prepared by graphene chemical vapor deposition [J]. Journal of Chemical Industry and Engineering, 2020, 71(6):22.DOI:10.11949 / 0438-1157.20200107.). Its combination with carbon dots can help improve the electron transport rate and promote the enhancement of the reducibility of carbon dots.
[0044] (2) Graphene has an extremely high specific surface area and strength, which can significantly improve the tensile strength, tear strength and wear resistance of rubber matrix, and also enhance air tightness and heat resistance. In this vermiculite-based composite filler structure system, since graphene is grown in situ on the vermiculite surface, it can overcome the inherent defect of easy curling. Furthermore, the polymer resin intercalation treatment can improve the compatibility of the entire system with the resin, and can simultaneously solve the problem of poor compatibility between vermiculite, graphene, glass fiber and resin system.
[0045] (3) Vermiculite readily forms a dense physical layer structure in nitrile rubber systems, thereby improving sealing performance. The lamellar structure of vermiculite allows it to peel off to form a sheet-like reinforcing structure under stress or friction, which helps to improve its wear resistance. The network coating structure of graphene on vermiculite can further improve wear resistance and reduce the coefficient of friction, thus giving the prepared gasket excellent wear resistance. This allows it to maintain its sealing performance for a long time even in environments with high friction, and it is not easily worn, ensuring reliability during long-term use. The advantages of vermiculite and graphene in this performance can also compensate for the lack of wear resistance of glass fiber.
[0046] (3) The introduction of reducing carbon points endows the vermiculite-based composite filler structure with excellent antioxidant capacity. Combined with the improvement of the high temperature resistance of the system by vermiculite, graphene and glass fiber, the vermiculite-based composite filler has excellent heat and oxygen aging resistance, thus making up for the shortcomings of nitrile rubber in this respect.
[0047] (4) Maleic anhydride-grafted EPDM rubber and butyl rubber are compounded as intercalation polymer resins. In addition to improving the film-forming ability of vermiculite-based composite fillers and their compatibility with nitrile rubber matrix, they also have the following effects: Maleic anhydride-grafted EPDM rubber has excellent heat resistance, ozone resistance and weather resistance, which can improve the problems of poor high temperature resistance and poor heat and oxygen aging resistance of butyl rubber; Butyl rubber has excellent air tightness and water tightness, which can overcome the problems of insufficient air tightness and oil resistance of EPDM rubber and nitrile rubber; Therefore, the combination of maleic anhydride-grafted EPDM rubber and butyl rubber also has a significant effect on improving the comprehensive performance of nitrile rubber matrix.
[0048] Therefore, it can be seen that the various components in the vermiculite-based composite filler structure system can significantly improve the overall performance of the nitrile rubber matrix through mutual cooperation.
[0049] The above is the general concept of the present invention. Based on this, detailed embodiments and comparative examples are provided below to further illustrate the present invention.
[0050] The main sources of raw materials involved in the following examples and comparative examples are as follows: Nitrile rubber, JSR N220S, Shanghai Yiyong New Material Technology Co., Ltd.; Zinc oxide, Jiangsu Xianfeng Nanomaterials Technology Co., Ltd.; Paraffin oil, Nantong Runfeng Petrochemical Co., Ltd.; Silica (M-5), Jiangsu Runfeng Synthetic Technology Co., Ltd.; Stearic acid, Jiangsu Runfeng Synthetic Technology Co., Ltd.; DCP (dicumyl peroxide), a vulcanizing agent, is manufactured by Shanghai Bojing Chemical Co., Ltd. Vulcanization accelerator NA-22, Guangzhou Housheng New Materials Co., Ltd.; Vermiculite, 325 mesh, Shijiazhuang Jinli Mining Co., Ltd.; Ethylene propylene diene monomer (EPDM) rubber, Dow 763P, purchased from Suzhou Guoyao New Materials Co., Ltd. Maleic anhydride, Rongsheng New Material Technology (Nantong, Jiangsu) Co., Ltd.; Butyl rubber, brand: JSR Japan, purchased from Shanghai Renen Import & Export Trading Co., Ltd.; Glass fiber, 20μm in diameter, 3mm in length, Jiangsu Jingshengyuan New Material Technology Co., Ltd. Graphene, product name: JCSRGO, size: 0.06-0.12μm, specific surface area: 150-200m2 / g; Suzhou Beike Nanotechnology Co., Ltd.
[0051] All other ingredients not specified are standard commercially available products. Example 1
[0052] A high-temperature resistant, leak-proof sealing gasket, the raw materials for which are prepared include the following components by weight: 100 parts of nitrile rubber; 34 parts of vermiculite-based composite filler; 4.5 parts zinc oxide; 5 parts paraffin oil; 6 parts of silica; 4 parts of vulcanizing agent DCP; 1.5 parts stearic acid; 1.2 parts of vulcanization accelerator NA-22.
[0053] The method for preparing this sealing gasket includes the following steps: 1) Internal mixing: Nitrile rubber, vermiculite-based composite filler, zinc oxide, silica, and stearic acid are added to an internal mixer and mixed at 85°C for 6 minutes to obtain the internally mixed rubber compound; 2) Open milling: Add the internally mixed rubber compound, vulcanizing agent, paraffin oil and vulcanization accelerator to the open mill, mix at 70°C for 12 minutes, discharge the material, place it in the injection molding machine to press into sheets to obtain raw rubber gaskets; 3) Vulcanization: The raw rubber gasket is vulcanized in a vulcanizing machine at 180°C for 23 minutes and the vulcanization pressure is 10MPa to obtain a high-temperature resistant and leak-proof sealing gasket.
[0054] The vermiculite-based composite filler was prepared by the following method: S1. Preparation of composite modified vermiculite: S1-1. In-situ growth of graphene: 1g of expanded vermiculite, 0.067g of copper chloride, and 0.052g of ruthenium trichloride were added to 100mL of 5% citric acid aqueous solution, ultrasonically treated for 30min, and heated to dryness at 140℃. The resulting product was transferred to a tube furnace and pretreated at 850℃ for 10min in a hydrogen atmosphere. Then, it was kept at 900℃ for 30min in a mixed gas atmosphere with a volume ratio of argon:ethylene:hydrogen of 2:2:1 to grow graphene in situ on the expanded vermiculite. After cooling to room temperature, graphene composite expanded vermiculite was obtained. The preparation method of expanded vermiculite is as follows: vermiculite is soaked in hydrogen peroxide with a mass concentration of 10% for 4 hours, the solid-liquid ratio is 1:5, the soaked vermiculite is calcined at 450℃ for 3 minutes, cooled to room temperature, and ball-milled to a particle size of less than 1μm to obtain expanded vermiculite. S1-2, Carbon point deposition: Take 2g of graphene-composite expanded vermiculite, 0.85g of citric acid, and 0.42g of mercaptopropionic acid and add them to a mixed solution consisting of 60mL of ethanol and 40mL of deionized water. Stir for 15min under a sealed environment. Then add 0.48g of glucose and 0.12g of 1,2-cyclohexanediamine. Disperse the mixture by ultrasonication for 20min under a sealed environment. Transfer the resulting mixture to a reaction vessel lined with polytetrafluoroethylene and hydrothermally react at 200℃ for 8h. After cooling to room temperature, centrifuge and filter. Wash the solid product with ethanol and deionized water in sequence and vacuum dry at 80℃ for 12h to obtain supported vermiculite. S1-3, Organic treatment: Take 1g of supported vermiculite and 0.2g of hexadecyltrimethylammonium bromide and add them to 100mL of deionized water. Stir for 2h, filter, wash the solid product with deionized water until bromide ions cannot be detected in the washing liquid with 0.1mol / L silver nitrate solution, dry to constant weight to obtain organic vermiculite; S1-4, Polymer Resin Intercalation Treatment: Take 0.5g of EPDM rubber and 0.05g of maleic anhydride and add them to 90mL of xylene. Stir at 100℃ for 15min while maintaining stirring. Add 10mL of xylene solution containing 6mg of benzoyl peroxide dropwise over 15min. Then react for 1.5h to obtain a polymer resin solution. Take 1g of organomodified vermiculite and 0.2g of butyl rubber and add them to the polymer resin solution. Stir and reflux at 70℃ for 24h. Filter and wash the solid product with acetone and ethanol in sequence. Vacuum dry to constant weight to obtain composite modified vermiculite.
[0055] S2. Glass fiber pretreatment: The glass fiber is soaked in 1 mol / L hydrochloric acid at 45°C for 45 min, filtered, washed with deionized water until neutral, and vacuum dried at 100°C to constant weight to obtain pretreated glass fiber.
[0056] S3. Coating the pretreated glass fiber with composite modified vermiculite: S3-1. Take 1g of composite modified vermiculite and add it to 100mL of a mixture of ethanol and deionized water in a volume ratio of 1:1. Disperse the mixture by ultrasonication for 30min to obtain a vermiculite dispersion. S3-2. Add 0.5g of pretreated glass fiber to the vermiculite dispersion, ultrasonically disperse for 30min, then stir at 70℃ for 2h, raise the temperature to 100℃, stir until dry, rinse the obtained product with deionized water, and vacuum dry at 90℃ to constant weight to obtain vermiculite-based composite filler. The obtained vermiculite-based composite filler weighed 1.32g, with a glass fiber weight gain of 0.82g, indicating that the composite modified vermiculite achieved a large-scale coating of glass fiber. Example 2
[0057] A high-temperature resistant, leak-proof sealing gasket, the raw materials for which are prepared include the following components by weight: 100 parts of nitrile rubber; 32 parts of vermiculite-based composite filler; 5 parts zinc oxide; 5 parts paraffin oil; 6.5 parts of silica; 4 parts of vulcanizing agent DCP; 1.5 parts stearic acid; 1.2 parts of vulcanization accelerator NA-22.
[0058] The rest is the same as in Example 1. Example 3
[0059] A high-temperature resistant, leak-proof sealing gasket, the raw materials for which are prepared include the following components by weight: 100 parts of nitrile rubber; 35 parts of vermiculite-based composite filler; 4 parts zinc oxide; 4 parts paraffin oil; 5 parts of silica; 4 parts of vulcanizing agent DCP; Stearic acid 2 parts; 1.2 parts of vulcanization accelerator NA-22.
[0060] The method for preparing this sealing gasket includes the following steps: 1) Internal mixing: Nitrile rubber, vermiculite-based composite filler, zinc oxide, silica, and stearic acid are added to an internal mixer and mixed at 90°C for 5 minutes to obtain the internally mixed rubber compound; 2) Open milling: Add the internally mixed rubber compound, vulcanizing agent, paraffin oil and vulcanization accelerator to the open mill, mix at 70°C for 15 minutes, discharge the material, place it in the injection molding machine to press into sheets, and obtain raw rubber gaskets. 3) Vulcanization: The raw rubber gasket is vulcanized in a vulcanizing machine at 185°C for 20 minutes and the vulcanization pressure is 10MPa to obtain a high-temperature resistant and leak-proof sealing gasket.
[0061] The preparation method of the vermiculite-based composite filler is the same as that in Example 1.
[0062] Comparative Example 1 The only difference between this example and Example 1 is that: The vermiculite-based composite filler in this example was prepared by the following method: S1. Preparation of composite modified vermiculite: S1-1. Preparation of expanded vermiculite: Vermiculite was soaked in 10% hydrogen peroxide for 4 hours with a solid-liquid ratio of 1:5. After soaking, the vermiculite was calcined at 450℃ for 3 minutes, cooled to room temperature, and ball-milled until the particle size was less than 1μm to obtain expanded vermiculite. S1-2, Carbon point deposition: Take 2g of expanded vermiculite, 0.85g of citric acid, and 0.42g of mercaptopropionic acid and add them to a mixed solution consisting of 60mL of ethanol and 40mL of deionized water. Stir for 15min under a sealed environment. Then add 0.48g of glucose and 0.12g of 1,2-cyclohexanediamine and disperse by ultrasonication for 20min under a sealed environment. Transfer the resulting mixture to a reaction vessel lined with polytetrafluoroethylene and hydrothermally react at 200℃ for 8h. After cooling to room temperature, centrifuge and filter. Wash the solid product with ethanol and deionized water in sequence and vacuum dry at 80℃ for 12h to obtain supported vermiculite.
[0063] The remaining steps are the same as in Example 1.
[0064] Comparative Example 2 The only difference between this example and Example 1 is that: The vermiculite-based composite filler in this example was prepared by the following method: S1. Preparation of composite modified vermiculite: S1-1. Graphene is grown in situ to obtain graphene-composite expanded vermiculite. The specific steps are the same as in Example 1. S1-2, Organic treatment: Take 1g of graphene-composite expanded vermiculite and 0.2g of hexadecyltrimethylammonium bromide and add them to 100mL of deionized water. Stir for 2h, filter, wash the solid product with deionized water until bromide ions cannot be detected in the washing liquid with 0.1mol / L silver nitrate solution, dry to constant weight to obtain organic vermiculite; S1-3. Polymer resin intercalation treatment is used to obtain composite modified vermiculite. The specific steps are the same as steps S1-4 in Example 1.
[0065] The remaining steps are the same as in Example 1.
[0066] Comparative Example 3 The only difference between this example and Example 1 is that: The vermiculite-based composite filler in this example was prepared by the following method: S1. Preparation of composite modified vermiculite: S1-1, In-situ grown graphene: 1 g of expanded vermiculite and 0.067 g of copper chloride were added to 100 mL of 5% citric acid aqueous solution, ultrasonicated for 30 min, and then heated to dryness at 140 °C. The resulting product was transferred to a tube furnace and pretreated at 850 °C for 10 min in a hydrogen atmosphere. Then, it was kept at 900 °C for 30 min in a mixed gas atmosphere with a volume ratio of argon:ethylene:hydrogen of 2:2:1 to grow graphene in situ on the expanded vermiculite. After cooling to room temperature, graphene composite expanded vermiculite was obtained. The preparation method of expanded vermiculite is the same as in Example 1. The remaining steps are the same as in Example 1.
[0067] Comparative Example 4 The only difference between this example and Example 1 is that: In this example, the organo-modified vermiculite from Example 1 is used instead of the composite modified vermiculite to coat the pretreated glass fiber.
[0068] Comparative Example 5 The only difference between this example and Example 1 is that: In this example, steps S1-4 are specifically as follows: 0.5 g of EPDM rubber and 0.05 g of maleic anhydride were added to 90 mL of xylene and stirred at 100 °C for 15 min. While stirring, 10 mL of xylene solution containing 6 mg of benzoyl peroxide was added dropwise over 15 min. The reaction was then carried out for 1.5 h to obtain a polymer resin solution. 1 g of organomodified vermiculite was added to the polymer resin solution and stirred under reflux at 70 °C for 24 h. The mixture was filtered, and the solid product was washed sequentially with acetone and ethanol. The product was then vacuum dried to constant weight to obtain composite modified vermiculite.
[0069] Comparative Example 6 The only difference between this example and Example 1 is that: In this example, steps S1-4 are specifically as follows: 0.5g of EPDM rubber was added to 100mL of xylene and stirred at 100℃ for 15min. Then, 1g of organomodified vermiculite and 0.2g of butyl rubber were added and stirred and refluxed at 70℃ for 24h. The mixture was filtered, and the solid product was washed with acetone and ethanol in sequence. It was then vacuum dried to constant weight to obtain composite modified vermiculite.
[0070] Comparative Example 7 A sealing gasket, the raw materials for which are prepared include the following components by weight: 100 parts of nitrile rubber; 12 parts of expanded vermiculite; 8 parts glass fiber; 4 parts graphene; 4.5 parts zinc oxide; 5 parts paraffin oil; 6 parts of silica; 4 parts of vulcanizing agent DCP; 1.5 parts stearic acid; 1.2 parts of vulcanization accelerator NA-22.
[0071] The preparation method of expanded vermiculite is the same as in Example 1.
[0072] The method for preparing this sealing gasket includes the following steps: 1) Internal mixing: Nitrile rubber, expanded vermiculite, glass fiber, graphene, zinc oxide, silica, and stearic acid are added to an internal mixer and mixed at 85°C for 6 minutes to obtain the internally mixed rubber compound; 2) Open milling: Add the internally mixed rubber compound, vulcanizing agent, paraffin oil and vulcanization accelerator to the open mill, mix at 70°C for 12 minutes, discharge the material, place it in the injection molding machine to press into sheets to obtain raw rubber gaskets; 3) Vulcanization: The raw rubber gasket is vulcanized in a vulcanizing machine at 180°C for 23 minutes and the vulcanization pressure is 10MPa to obtain a sealing gasket.
[0073] Performance testing: 1. Tensile strength and compression resilience: The tensile strength was tested in accordance with the standard GB / T 20671.7-2006 Classification System and Test Methods for Non-metallic Gasket Materials Part 7: Tensile Strength Test Method for Non-metallic Gasket Materials. The compression and rebound rate were tested in accordance with the standard GB / T12622-2008, "Test Method for Compression and Rebound Rate of Gaskets for Pipe Flanges".
[0074] The test results are shown in Table 1 below. Figures 1-2 As shown:
[0075] The test results show that the gasket in the embodiment has high tensile strength and excellent resilience. Except for Comparative Examples 2 and 5, the two properties of the other comparative examples have been significantly reduced to varying degrees.
[0076] 2. Sealing performance The sealing performance was tested in accordance with the standard GB / T20671 "Classification System and Test Methods for Non-metallic Gasket Materials - Test Method for Sealing Performance of Gasket Materials", using dry nitrogen as the gas medium to test the gas leakage rate.
[0077] The test results are shown in Table 2 below. Figure 3 As shown:
[0078] The test results show that the gaskets in the examples have excellent sealing performance. The decrease in sealing performance in Comparative Example 1 indicates that graphene has an improving effect on sealing performance. The decrease in sealing performance in Comparative Example 3 is mainly attributed to the lack of ruthenium grafting catalyst, which affects the in-situ growth of graphene. In Comparative Example 4, the lack of polymer resin intercalation treatment for the vermiculite-based composite filler significantly affected the dispersion of the vermiculite-based composite filler in the nitrile rubber matrix system, resulting in a decrease in sealing performance, as well as a decrease in tensile strength and resilience. The decrease in sealing performance in Comparative Example 5 demonstrates the enhancing effect of adding butyl rubber on sealing performance. In Comparative Example 7, the inorganic filler components—expanded vermiculite, glass fiber, and graphene—were directly blended and added to the nitrile rubber system. The inorganic filler components were difficult to disperse in the organic system, resulting in their inability to fully exert their complementary effects, a significant decrease in sealing performance, and a decrease in tensile strength and resilience.
[0079] 3. High temperature resistance The gasket was kept at 200℃ for 48 hours, and then the tensile strength was tested using the same method as above. The tensile strength retention rate was calculated using the following formula: Tensile strength retention rate S = (G1 / G0) × 100%, where G0 represents the tensile strength before aging and G1 represents the tensile strength after aging.
[0080] The test results are shown in Table 3 below. Figure 4 As shown:
[0081] The test results show that the gasket in the embodiment has excellent high temperature resistance and can serve for a long time in high temperature environments.
[0082] 4. Resistance to heat and oxygen aging The aging method was carried out according to the relevant method in standard GB / T3512-2001, with an aging temperature of 180℃ and an aging time of 120 hours. After the aging treatment was completed, the tensile strength retention rate was tested using the same method as above.
[0083] The test results are shown in Table 4 below. Figure 5 As shown:
[0084] The test results show that the gasket in the example has excellent heat and oxygen aging resistance. In Comparative Examples 2 and 3, no carbon points were deposited, and the gasket lost its reducibility, resulting in a significant decrease in heat and oxygen aging resistance.
[0085] 5. High-temperature wear resistance The wear test was conducted using a THT07-135 high-temperature friction and wear testing machine. The friction pair consisted of steel pins (material GCrl5), with a hardness of 9 GPa, a surface roughness of 0.02 µm, a diameter of 5 mm, an applied load of 15 N, a sliding distance of 2500 m, a linear velocity of 0.5 m / s, a test temperature of 200 °C, and a wear rate K. Where ΔV is the wear volume (mm). 3 F is the load (N), and S is the total sliding distance (m).
[0086] The test results are shown in Table 5 below. Figure 6 As shown:
[0087] The test results show that the gasket in the embodiment still has excellent wear resistance at high temperatures, which can ensure reliability during long-term use.
[0088] 6. Infrared absorption spectroscopy characterization Reference Figure 7 The infrared absorption spectrum of the supported vermiculite prepared in Example 1 is shown, where 900 cm⁻¹ -1 450cm -1 and 650cm -1 The nearby characteristic peaks originate from the stretching vibrations of Si-O-Si, the bending vibrations of Si-O-Si, and the bending vibrations of Al-O-Si in the vermiculite structure, respectively; 540 cm⁻¹ -1 and 600cm -1 The nearby peaks are characteristic peaks of copper oxide and ruthenium oxide; the characteristic peaks near 1580 cm⁻¹ and 1050 cm⁻¹ are from sp2 hybrid C-C bond peaks and sp3 hybrid C-C bond peaks in graphene, respectively, indicating that the in-situ growth of graphene was successfully achieved; the appearance of amino, mercapto, and carboxyl characteristic peaks indicates the successful deposition of carbon dots; the successful synthesis of supported vermiculite was characterized by this infrared absorption spectrum.
[0089] 7. Antioxidant properties The antioxidant properties of the vermiculite-based composite fillers prepared in Example 1 and Comparative Examples 1-3 were tested according to the following methods: Vermiculite-based composite filler was added to ethanol and ultrasonically dispersed for 30 min to prepare a dispersion with a concentration of 1 mg / mL. The antioxidant properties of the dispersion at different times were then tested using a DPPH free radical scavenging ability test kit (catalog number UPLC-MS-4569, specification: 100T / 48S, Shanghai Liquid Chromatography-Mass Testing Co., Ltd.).
[0090] Assay Principle: DPPH free radicals have unpaired electrons, and their alcoholic solution is purple with strong absorption at 515 nm. In the presence of antioxidants, DPPH free radicals are scavenged, the solution color lightens, and the absorbance at 515 nm decreases. Within a certain range, the change in absorbance is directly proportional to the degree of free radical scavenging. In this kit, the degree of absorbance decrease reflects the sample's ability to scavenge DPPH free radicals; that is, the lower the absorbance at 515 nm, the stronger the nitrogen free radical scavenging ability, and the stronger the corresponding antioxidant performance.
[0091] Test results are as follows Figure 8 As shown, the vermiculite-based composite filler prepared in Example 1 has excellent antioxidant properties. The antioxidant properties of the vermiculite-based composite fillers prepared in Comparative Examples 1 and 3 decrease sequentially, while the vermiculite-based composite filler prepared in Comparative Example 2 has virtually no antioxidant capacity.
[0092] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details.
Claims
1. A high-temperature resistant, leak-proof sealing gasket, characterized in that, The raw materials for its preparation include the following components by weight: 100 parts of nitrile rubber; 26-39 parts of vermiculite-based composite filler; 2-7 parts zinc oxide; 3-8 parts paraffin oil; 2.5-9 parts of silica; 1-6 parts of vulcanizing agent; Stearic acid 0.8-2.4 parts; Vulcanization accelerator: 0.5-1.7 parts; The vermiculite-based composite filler was prepared by the following method: S1. Preparation of composite modified vermiculite: Expanded vermiculite is subjected to in-situ growth of graphene, carbon point deposition, organic treatment and polymer resin intercalation treatment to obtain composite modified vermiculite; S2, glass fiber pretreatment; S3. The pretreated glass fiber is coated with composite modified vermiculite to obtain vermiculite-based composite filler; Step S1 specifically includes: S1-1, In-situ grown graphene: Expanded vermiculite, copper chloride, and ruthenium trichloride were added to an aqueous solution of citric acid, ultrasonically treated, and then heated to dryness. The resulting product was pretreated under a hydrogen atmosphere and under heating, and then heated and reacted in a mixed gas composed of argon, ethylene, and hydrogen. After the reaction was completed, it was cooled to obtain graphene-composite expanded vermiculite. S1-2, Carbon point deposition: Graphene-composite expanded vermiculite, citric acid, and mercaptopropionic acid were added to a mixed solution of ethanol and deionized water, stirred, and then glucose and 1,2-cyclohexanediamine were added. The mixture was ultrasonically dispersed, and the resulting mixture was transferred to a reaction vessel and subjected to hydrothermal reaction under heating. After the reaction was completed, the mixture was cooled, centrifuged and filtered, the solid product was washed, and vacuum dried to obtain supported vermiculite. S1-3, Organic treatment: Loaded vermiculite and hexadecyltrimethylammonium bromide were added to deionized water, stirred, filtered, the solid product was washed and dried to obtain organic vermiculite; S1-4, Polymer resin intercalation treatment: Ethylene propylene diene monomer (EPDM) rubber and maleic anhydride were added to xylene, heated and stirred, and a xylene solution containing benzoyl peroxide was added dropwise. After the addition was complete, the reaction was carried out to obtain a polymer resin solution. Organic vermiculite and butyl rubber were added to a polymer resin solution, heated and stirred under reflux. After the reaction was completed, the mixture was filtered, the solid product was washed, and vacuum dried to obtain composite modified vermiculite.
2. The high-temperature resistant leak-proof sealing gasket according to claim 1, characterized in that, Step S1 specifically includes: S1-1, In-situ grown graphene: Take 0.5-2g of expanded vermiculite, 0.033-0.134g of copper chloride, and 0.026-0.104g of ruthenium trichloride and add them to 50-200mL of citric acid aqueous solution with a mass concentration of 2.5-10%. Sonicate for 15-60min and heat to dryness at 120-150℃. Transfer the obtained product to a tube furnace and pretreat at 750-900℃ for 5-20min in a hydrogen atmosphere. Then, heat at 880-1000℃ for 15-60min in a mixed gas atmosphere with a volume ratio of argon:ethylene:hydrogen of 2:2:1 and cool to room temperature to obtain graphene-composite expanded vermiculite. S1-2, Carbon point deposition: Take 1-4g of graphene-composite expanded vermiculite, 0.42-1.90g of citric acid, and 0.21-0.84g of mercaptopropionic acid and add them to a mixed solution consisting of 30-120mL of ethanol and 20-80mL of deionized water. Stir under sealed conditions for 5-30min. Then add 0.24-0.96g of glucose and 0.06-0.24g of 1,2-cyclohexanediamine. Disperse the mixture under sealed conditions using ultrasonication for 10-40min. Transfer the resulting mixture to a reaction vessel and hydrothermally react at 180-230℃ for 4-16h. Cool to room temperature, centrifuge and filter. Wash the solid product with ethanol and deionized water sequentially, and vacuum dry at 70-100℃ for 6-24h to obtain supported vermiculite. S1-3, Organic treatment: Take 0.5-2g of supported vermiculite and 0.1-0.4g of hexadecyltrimethylammonium bromide and add them to 50-200mL of deionized water. Stir for 1-4h, filter, wash the solid product with deionized water, and dry to constant weight to obtain organic vermiculite. S1-4, Polymer resin intercalation treatment: Take 0.25-1g of EPDM rubber and 0.025-0.1g of maleic anhydride and add them to 45-180mL of xylene. Stir at 90-110℃ for 5-30min while maintaining stirring. Add 2.5-20mL of xylene solution containing 3-12mg of benzoyl peroxide dropwise over 10-30min. Then react for 1-4h to obtain a polymer resin solution. Take 0.5-2g of organomodified vermiculite and 0.1-0.4g of butyl rubber and add them to the polymer resin solution. Stir and reflux at 60-80℃ for 12-48h, filter, wash the solid product with acetone and ethanol in sequence, and dry it under vacuum to constant weight to obtain composite modified vermiculite.
3. The high-temperature resistant leak-proof sealing gasket according to claim 1, characterized in that, The expanded vermiculite is prepared by the following method: the vermiculite is soaked in hydrogen peroxide with a mass concentration of 5-20% for 2-8 hours, the solid-liquid ratio is controlled at 1:2~7, the soaked vermiculite is taken out, calcined at 400-500℃ for 1-5 minutes, cooled to room temperature, and ball-milled to a particle size of less than 0.5-5μm to obtain expanded vermiculite.
4. The high-temperature resistant leak-proof sealing gasket according to claim 1, characterized in that, Step S2 specifically involves immersing the glass fiber in hydrochloric acid under heating, filtering, washing with deionized water until neutral, and vacuum drying to constant weight to obtain pretreated glass fiber.
5. The high-temperature resistant leak-proof sealing gasket according to claim 4, characterized in that, Step S2 specifically involves immersing the glass fiber in hydrochloric acid with a concentration of 0.5-2 mol / L at 40-50°C for 15-90 minutes, filtering, washing with deionized water until neutral, and vacuum drying at 90-120°C to constant weight to obtain the pretreated glass fiber.
6. The high-temperature resistant leak-proof sealing gasket according to claim 1, characterized in that, Step S3 is as follows: S3-1. Take the composite modified vermiculite and add it to a mixture of ethanol and deionized water, then disperse it by ultrasonication to obtain a vermiculite dispersion. S3-2. Add pretreated glass fiber to vermiculite dispersion, disperse ultrasonically, then stir under heating, raise the temperature, stir until dry, rinse the obtained product and dry under vacuum to constant weight to obtain vermiculite-based composite filler.
7. The high-temperature resistant leak-proof sealing gasket according to claim 6, characterized in that, Step S3 is as follows: S3-1. Take 0.5-2g of composite modified vermiculite and add it to 50-200mL of a mixture of ethanol and deionized water in a volume ratio of 1:
1. Disperse the mixture by ultrasonication for 15-60min to obtain a vermiculite dispersion. S3-2. Add 0.25-0.1g of pretreated glass fiber to the vermiculite dispersion, ultrasonically disperse for 15-60min, then stir at 50-85℃ for 1-4h, raise the temperature to 95-105℃, stir until dry, rinse the product with deionized water and vacuum dry at 70-100℃ to constant weight to obtain vermiculite-based composite filler.
8. The high-temperature resistant leak-proof sealing gasket according to claim 1, characterized in that, The vulcanizing agent is selected from at least one of vulcanizing agents DCP, BIPB, or DBPH; The vulcanization accelerator is at least one of the following: vulcanization accelerator TMTD, vulcanization accelerator ZBX, vulcanization accelerator ZDMC, vulcanization accelerator NA-22, and vulcanization accelerator CZ.
9. A method for preparing a high-temperature resistant, leak-proof sealing gasket as described in any one of claims 2-8, characterized in that, Includes the following steps: 1) Internal mixing: Add nitrile rubber, vermiculite-based composite filler, zinc oxide, silica, and stearic acid to an internal mixer and mix at 75-95℃ for 2-10 minutes to obtain the internally mixed rubber compound; 2) Open milling: Add the internally mixed rubber compound, vulcanizing agent, paraffin oil and vulcanization accelerator into the open mill, mix at 55-78℃ for 5-25 minutes, discharge the material, place it in the injection molding machine to press into sheets to obtain raw rubber gaskets. 3) Vulcanization: The raw rubber gasket is vulcanized in a vulcanizing machine at 160-190℃ for 12-50 minutes and the vulcanization pressure is 5-25MPa to obtain the high temperature resistant and leak-proof sealing gasket.
Citation Information
Patent Citations
A method for preparing a vermiculite-based high-temperature resistant sealing material
CN107188453B
A high-temperature resistant vermiculite-based composite sealing gasket and its preparation method
CN115650632B
Preparation method of vermiculite-based high temperature-resistant sealing material
CN107188453A
Oil-resistant moving-ring sealing ring and preparation method thereof
CN109021467A