A method for preparing a cellulose acetate self-supporting carbonized membrane

By employing metal coordination crosslinking and Lewis acid activation, the problem of forming a self-supporting membrane during the carbonization process of cellulose acetate was solved, enabling the preparation of a highly efficient and environmentally friendly self-supporting carbonized cellulose acetate membrane, reducing production costs and improving thermal stability.

CN120443419BActive Publication Date: 2026-11-20GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510464645.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-14
Publication Date
2026-11-20
Estimated Expiration
2045-04-14

AI Technical Summary

Technical Problem

In existing technologies, the carbonization process of cellulose acetate (CA) is difficult to form a stable self-supporting membrane structure, and the production cost is high. The carbonization process also generates toxic gases, requiring a large amount of waste gas treatment.

Method used

Cellulose acetate membranes were prepared by electrospinning using metal coordination crosslinking and Lewis acid activation. The membranes underwent deacetylation, metal salt reaction, Lewis acid reaction, and carbonization to form stable self-supporting carbonized membranes.

Benefits of technology

It improves the interaction forces of cellulose acetate molecular chains, reduces the formation of volatile substances and tar, significantly improves thermal stability, eliminates the pre-oxidation step, reduces production costs, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120443419B_ABST
    Figure CN120443419B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a cellulose acetate self-supporting carbonized film, and the cellulose acetate self-supporting carbonized film is prepared by the following steps: taking cellulose acetate as a precursor, adopting electrostatic spinning technology to prepare a cellulose acetate film, sequentially performing deacetylation, metal crosslinking and Lewis acid activation treatment on the film, and placing the film in a nitrogen atmosphere after cleaning and drying to perform carbonization, so that the cellulose acetate self-supporting carbonized film is finally obtained. The cellulose acetate self-supporting film is prepared by the method of metal crosslinking and Lewis acid activation, the pre-oxidation step in the existing CA carbonized film technology is omitted, energy loss is reduced, and the method has more advantages in economy and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of carbonized film preparation technology, and specifically relates to a method for preparing a cellulose acetate self-supporting carbonized film. Background Technology

[0002] Carbonized membranes, due to their unique physical and chemical properties such as high flexibility, excellent electrical characteristics, thermal stability, and high specific surface area, have shown broad application prospects in various fields such as electronic devices, sensors, energy storage devices, and smart fabrics. Polyacrylonitrile (PAN) is the most commonly used precursor material for carbonized membranes, but its production cost is high, and the carbonization process generates toxic gases such as ammonia and hydrogen cyanide, requiring large-scale waste gas treatment.

[0003] In recent years, cellulose acetate (CA), as a naturally derived biopolymer, has been considered a potential alternative to polyvinyl acetate (PAN) due to its significant advantages such as low cost, renewability, good biocompatibility, and environmental friendliness. However, it is difficult to form a stable self-supporting membrane structure during the carbonization process of CA.

[0004] On the other hand, researchers have effectively synthesized polyvinylpyrrolidone (PVP) self-supporting carbonized films using a metal coordination crosslinking method. Currently, existing technologies have not applied metal crosslinking to the preparation of CA self-supporting carbonized films. Developing a method for preparing CA self-supporting carbonized films using metal crosslinking technology is of great significance for reducing costs and preparing environmentally friendly CA-based carbonized films. Summary of the Invention

[0005] To address the problems existing in the prior art, one objective of this invention is to provide a method for preparing a cellulose acetate self-supporting carbonized membrane, the method comprising the following steps:

[0006] (1) Preparation of electrospinning solution: cellulose acetate (CA), acetone and N,N-dimethylacetamide (DMAC) are mixed and stirred at room temperature for 3-12 h. After stirring evenly, the mixture is allowed to stand for 12 h to obtain the precursor spinning solution.

[0007] (2) Cellulose acetate membranes were prepared using electrospinning technology;

[0008] (3) The above fiber membrane was immersed in 0.1 M NaOH methanol solution for deacetylation treatment. After the treatment was completed, it was washed with ultrapure water until neutral and then dried.

[0009] (4) The above fiber membrane is immersed in a metal salt solution for reaction. After the reaction is completed, it is washed and dried to obtain a cellulose acetate crosslinked membrane.

[0010] (5) The above cross-linked membrane is immersed in a Lewis acid solution for reaction. After the reaction is completed, it is washed and dried to obtain the activated cellulose acetate cross-linked membrane.

[0011] (6) The activated cellulose acetate crosslinked membrane was placed in a tube furnace and carbonized under a nitrogen atmosphere to obtain a self-supporting carbonized cellulose acetate membrane.

[0012] In step (1), the volume ratio of acetone to DMAC is 2:1; the concentration of the electrospinning solution is 10-20 wt / v.

[0013] In step (2), the electrospinning process parameters are: spinning voltage of 10-35 kV, feeding rate of 0.1-0.3 mm / min, spinning temperature of 18-30 ℃, relative humidity of 35-60%, and spraying distance of 10-30 cm.

[0014] In step (3), the degree of deacetylation is 25%-65%.

[0015] The metal salt solution in step (4) consists of one or more of Co(NO3)2, Cu(NO3)2, and Fe(NO3)3, with a concentration of 3-6 wt / v%, and the reaction conditions are heating in a water bath at 60 ℃ for 5-8 h.

[0016] Metal ions in metal salt solutions can undergo coordination reactions with carbonyl groups in cellulose acetate to form cross-linked structures. These cross-linked structures can effectively increase the interaction forces between cellulose acetate molecular chains, effectively restrict the movement of cellulose acetate molecular chains at high temperatures, thereby slowing down its thermal decomposition process and providing conditions for the formation of self-supporting carbonized films.

[0017] In step (5), the Lewis acid solution is one or more of NH4Cl, ZnCl2, and AlCl3, with a concentration of 3-6 wt / v%, and the reaction conditions are heating in a water bath at 60 ℃ for 5-8 h.

[0018] The decomposition of cellulose mainly involves dehydrogenation and depolymerization. Depolymerization primarily forms L-glucose, which further decomposes to produce volatile carbon compounds and tar. The relatively low carbon residue after cellulose decomposition is mainly due to the dominance of depolymerization. Dehydrogenation can inhibit the formation of L-glucose, leading to an increase in solid residue, reducing the formation of volatile substances and tar, and ultimately improving the carbon residue. In the presence of Lewis acids such as ZnCl2 and NH4Cl, dehydrogenation reactions are more likely to occur, causing cellulose to cyclize and making it easier to form self-supporting films after carbonization.

[0019] The carbonization conditions in step (6) include: the initial temperature of the tube furnace is 25 ℃, the temperature is increased to 700 ℃ at 2.5 ℃ / min, and the temperature is held for 2 hours before natural cooling.

[0020] The second objective of this invention is to provide a cellulose acetate carbonized membrane prepared by the above method.

[0021] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0022] (1) The present invention uses metal coordination to crosslink with CA, which solves the problem of the difficulty in forming a stable self-supporting film structure during the carbonization process of CA. This improvement enhances the intermolecular forces of CA, effectively restricts the movement of CA molecular chains at high temperatures, thereby slowing down its thermal decomposition process and providing favorable conditions for the preparation of CA self-supporting carbonized films.

[0023] (2) In this invention, Lewis acid was used to activate the CA membrane, which reduced the formation of volatile substances and tar during CA decomposition and successfully prepared a self-supporting carbonized cellulose acetate membrane, providing a new method for developing self-supporting carbonized cellulose acetate membranes.

[0024] (3) In conventional understanding, CA has poor thermal stability and is prone to decomposition at high temperatures. Pre-oxidation is a key step in the preparation of carbonized films from CA. Pre-oxidation treatment can convert CA into a thermally stable intermediate, preventing excessive decomposition or combustion during subsequent high-temperature carbonization. In addition, pre-oxidation treatment can also ensure that CA is uniformly converted into carbon during carbonization, avoiding local overheating or incomplete carbonization, and forming a self-supporting film structure. However, this invention found that the thermal stability of CA can be significantly improved through metal coordination crosslinking, Lewis acid activation, etc., omitting the pre-oxidation step, and is more energy-efficient and environmentally friendly, overcoming previous technical biases. Attached Figure Description

[0025] Figure 1 The cellulose acetate self-supporting carbonized membrane prepared in Example 1 of this invention;

[0026] Figure 2 The carbonized cellulose acetate membrane prepared in Comparative Example 1 of this invention;

[0027] Figure 3 This refers to the carbonization product of the cellulose acetate crosslinked membrane prepared in Comparative Example 2 of this invention;

[0028] Figure 4 The cellulose acetate self-supporting carbonized membrane prepared in Comparative Example 3 of this invention;

[0029] Figure 5Thermogravimetric analysis (TGA) curves of cellulose acetate films prepared in Examples 1, 1, and 2 of this invention, after Lewis acid treatment and metal crosslinking, the original cellulose acetate film, and the cellulose acetate film after metal crosslinking, were obtained by heating from room temperature to 800 °C at a rate of 10 °C / min under a N2 atmosphere.

[0030] Figure 6 This is a flowchart of the present invention. Detailed Implementation

[0031] To further understand the present invention, the present invention will be further described below with reference to the accompanying drawings and embodiments, but the present invention is not limited to the following embodiments.

[0032] Example 1:

[0033] This embodiment provides a method for preparing a carbonized cellulose acetate membrane, the method comprising the following steps:

[0034] (1) Preparation of electrospinning solution:

[0035] 1.53 g CA was dissolved in 9 ml of a mixed solution of acetone and DMAC, wherein the volume ratio of acetone to DMAC was 2:1. The solution was stirred at room temperature for 6 h to completely dissolve CA, and then allowed to stand for 12 h to remove bubbles, thus obtaining the CA spinning solution.

[0036] (2) Preparation of cellulose acetate film using electrospinning technology:

[0037] The CA spinning solution obtained in step (1) was transferred to a 10 ml disposable syringe. The relative humidity of the environment in the spinning instrument was controlled at 50%, the voltage of the spinning instrument was adjusted to 21 kV, the injection speed was 0.1 mm / min, the distance between the needle and the receiver was 20 cm, and the receiver rotation speed was 120 r / h. Release paper was wrapped on the roller receiver to receive the electrospun fibers. The fibers were dried under vacuum at 60 ℃ for 12 h to obtain a cellulose acetate film.

[0038] (3) Deacetylation treatment of the fiber membrane:

[0039] Weigh 0.21 g of NaOH powder and dissolve it in 50 ml of methanol solution. Soak the cellulose acetate film obtained in step (2) in the above NaOH methanol solution and let it stand at room temperature for 24 h for deacetylation treatment. After treatment, rinse with ultrapure water until neutral and dry at 60 °C for 12 h to obtain deacetylated cellulose acetate film.

[0040] (4) Weigh 1.51 g of Co(NO3)2 powder and dissolve it in 50 ml of methanol solution to prepare a metal salt solution. Immerse the deacetylated cellulose acetate film obtained in step (3) in the above metal salt solution and heat it in a water bath at 60 °C for 6 h to carry out the reaction. After the reaction is completed, wash it with methanol and dry it under vacuum at 60 °C for 12 h to obtain a cellulose acetate crosslinked film.

[0041] (5) Weigh 0.75 g of NH4Cl powder and dissolve it in 25 ml of ultrapure water to prepare a Lewis acid solution. Immerse the cellulose acetate crosslinked membrane obtained in step (4) into the Lewis acid solution and heat it in a water bath at 60 °C for 6 h to carry out the reaction. After the reaction is completed, wash it with ultrapure water and dry it under vacuum at 60 °C for 12 h to obtain the activated cellulose acetate crosslinked membrane.

[0042] (6) The above composite fiber membrane is placed in a tube furnace for carbonization treatment. The initial temperature of the tube furnace is 25℃, and the temperature is increased to 700℃ at 2.5℃ / min. The temperature is held for 2 hours and then naturally cooled to room temperature to obtain a self-supporting carbonized cellulose acetate membrane.

[0043] Example 1: Product image of cellulose acetate carbonized film (as shown) Figure 1 As shown.

[0044] Comparative Example 1:

[0045] This comparative example omits steps (4) and (5), does not perform metal crosslinking and Lewis acid activation treatment, adds a pre-oxidation step before step (6), and other conditions are the same as in Example 1.

[0046] Pre-oxidation: The CA membrane obtained in the above steps is placed in a tube furnace for carbonization treatment. The initial temperature of the tube furnace is 25 ℃, and the temperature is increased to 240 ℃ at 1 ℃ / min. The temperature is held for 2 h and then naturally cooled to room temperature to obtain the pre-oxidized cellulose acetate product.

[0047] Figure 2 This is a carbonized product of cellulose acetate that has not undergone metal crosslinking and Lewis acid activation treatment; the resulting product is black and does not form a film. Figure 2 It can be seen that CA films without metal crosslinking and Lewis acid activation treatment have poor thermal stability and are difficult to form self-supporting films.

[0048] Comparative Example 2:

[0049] This comparative example omits step (5), does not perform Lewis acid activation treatment, adds a pre-oxidation step before step (6), and other conditions are the same as in Example 1.

[0050] Pre-oxidation: The CA cross-linked membrane obtained in the above steps is placed in a tube furnace for carbonization treatment. The initial temperature of the tube furnace is 25 ℃, and the temperature is increased to 240 ℃ at 1 ℃ / min. The temperature is held for 2 h and then naturally cooled to room temperature to obtain the pre-oxidized product of cellulose acetate cross-linked membrane.

[0051] The carbonization product of the crosslinked membrane prepared in Comparative Example 2 of this invention is as follows: Figure 3 As shown, the resulting product is black and has a high shrinkage rate. From Figure 3 It can be seen that the film-forming effect of cellulose acetate after metal crosslinking treatment is improved compared with Comparative Example 1.

[0052] Comparative Example 3:

[0053] This comparative example adds a pre-oxidation step before step (6), and the other conditions are the same as in Example 1.

[0054] Pre-oxidation: The CA cross-linked membrane obtained in the above steps is placed in a tube furnace for carbonization treatment. The initial temperature of the tube furnace is 25 ℃, and the temperature is increased to 240 ℃ at 1 ℃ / min. The temperature is held for 2 h and then naturally cooled to room temperature to obtain the pre-oxidized product of cellulose acetate cross-linked membrane.

[0055] The carbonization product of the crosslinked membrane prepared in Comparative Example 3 of this invention is as follows: Figure 4 As shown, the carbonized film is black, similar to the carbonized film obtained in the example. From Figure 4 It can be seen that cellulose acetate, after metal crosslinking and Lewis acid activation treatment, can form a stable self-supporting structure during carbonization. Furthermore, the pre-oxidation step can be omitted, thereby reducing energy consumption.

[0056] Figure 5 The thermogravimetric analysis (TGA) curves of the cellulose acetate films prepared in Examples 1, 1, and 2 of this invention, after Lewis acid treatment and metal crosslinking, the original cellulose acetate film, and the cellulose acetate film after metal crosslinking, were obtained by heating from room temperature to 800 °C at a rate of 10 °C / min under a N2 atmosphere. Figure 5It can be seen that the residual carbon content of the cellulose acetate film after decomposition after metal crosslinking treatment is significantly higher than that of the original cellulose acetate film. This indicates that the crosslinking structure formed by metal ions and carbonyl groups in cellulose acetate can effectively increase the interaction force between cellulose acetate molecular chains and restrict the movement of cellulose acetate molecular chains at high temperatures. The cellulose acetate film treated with metal crosslinking and Lewis acid activation has the highest residual carbon content. This is mainly because cellulose is more prone to dehydrogenation in the presence of Lewis acid, reducing the formation of volatile substances and tar. These results show that metal crosslinking and Lewis acid activation treatment significantly improve the thermal stability of cellulose acetate films, thereby enabling the formation of a stable self-supporting film structure during carbonization.

Claims

1. A method for preparing a self-supporting carbonized cellulose acetate membrane, characterized in that... Includes the following steps: (1) Preparation of electrospinning solution: cellulose acetate (CA), acetone and N,N-dimethylacetamide (DMAC) are mixed and stirred at room temperature for 3-12 h. After stirring evenly, the mixture is allowed to stand for 12 h to obtain the precursor spinning solution. (2) Cellulose acetate membranes were prepared using electrospinning technology; (3) The above cellulose acetate membrane was immersed in 0.1 M NaOH methanol solution for deacetylation treatment. After the treatment was completed, it was washed with ultrapure water until neutral and dried to obtain deacetylated cellulose acetate membrane. (4) The above deacetylated cellulose acetate membrane was immersed in a methanol solution of metal salt for reaction. After the reaction was completed, it was washed and dried to obtain a cross-linked cellulose acetate membrane. (5) The above-mentioned cellulose acetate cross-linked membrane was immersed in Lewis acid aqueous solution for reaction. After the reaction was completed, it was washed and dried to obtain the activated cellulose acetate cross-linked membrane. (6) The activated cellulose acetate crosslinked membrane was placed in a tube furnace and carbonized under a nitrogen atmosphere to obtain a self-supporting carbonized cellulose acetate membrane.

2. The method for preparing a self-supporting carbonized cellulose acetate film according to claim 1, characterized in that: In step (1), the volume ratio of acetone to DMAC is 2:1; the concentration of the electrospinning solution is 10-20 wt / v.

3. The method for preparing a self-supporting carbonized cellulose acetate film according to claim 1, characterized in that: In step (2), the electrospinning process parameters are: spinning voltage of 10-35 kV, feeding rate of 0.1-0.3 mm / min, spinning temperature of 18-30 ℃, relative humidity of 35-60%, and spraying distance of 10-30 cm.

4. The method for preparing a self-supporting carbonized cellulose acetate membrane according to claim 1, characterized in that: In step (3), the degree of deacetylation is 25%-65%.

5. The method for preparing a self-supporting carbonized cellulose acetate membrane according to claim 1, characterized in that: The metal salt mentioned in step (4) is one or more of Co(NO3)2, Cu(NO3)2, and Fe(NO3)3, with a solution concentration of 3-6 wt / v%, and the reaction conditions are heating in a water bath at 60 ℃ for 5-8 h.

6. The method for preparing a self-supporting carbonized cellulose acetate film according to claim 1, characterized in that: In step (5), the Lewis acid is one or more of NH4Cl, ZnCl2, and AlCl3, with a solution concentration of 3-6 wt / v%, and the reaction conditions are heating in a water bath at 60 ℃ for 5-8 h.

7. The method for preparing a self-supporting carbonized cellulose acetate film according to claim 1, characterized in that: The carbonization conditions in step (6) include: the initial temperature of the tube furnace is 25 ℃, the temperature is increased to 700 ℃ at 2.5 ℃ / min, and the temperature is held for 2 hours before natural cooling.

8. A self-supporting carbonized cellulose acetate membrane, characterized in that, Prepared by the method according to any one of claims 1-7.