A carbon fiber paper based on pitch / polyacrylonitrile-based nonwoven felt, and a method for preparing and using the same

The pitch/polyacrylonitrile-based nonwoven carbon fiber paper prepared by electrospinning technology and high-temperature carbonization process solves the problems of poor conductivity and uneven thickness of carbon fiber paper, and realizes low-cost, high-conductivity and controllable thickness carbon fiber paper, which is suitable for gas diffusion layer of fuel cell.

CN120443420BActive Publication Date: 2026-11-24DONGHUA UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510610208.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-05-13
Publication Date
2026-11-24
Estimated Expiration
2045-05-13

AI Technical Summary

Technical Problem

Existing carbon fiber paper suffers from poor conductivity, uneven thickness, and high cost in proton exchange membrane fuel cells.

Method used

Carbon fiber paper based on pitch/polyacrylonitrile nonwoven mat was prepared by electrospinning technology. By adjusting parameters such as the concentration of spinning solution and spinning flow rate, and combining pre-oxidation, resin impregnation, hot pressing curing and carbonization graphitization processes, the conductivity and thickness were simultaneously controlled.

Benefits of technology

Low-cost, highly conductive, controllable-thickness, and ultra-thin carbon fiber paper was prepared, which is suitable for the gas diffusion layer of fuel cells, improving battery performance and reducing preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120443420B_ABST
    Figure CN120443420B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of carbon fiber paper technology, and provides a carbon fiber paper based on pitch / polyacrylonitrile-based nonwoven felt, its preparation method, and its application. The method of this invention includes the following steps: a soluble pitch solution and an acrylonitrile-itaconic acid copolymer solution are sequentially stirred, mixed, and degassed; an electrospinning solution is electrospinned; the pitch / polyacrylonitrile-based nonwoven felt is sequentially dried and pre-oxidized to obtain a pre-oxidized felt; the pre-oxidized felt is impregnated in a resin solution, and then sequentially dried, hot-pressed, carbonized, and graphitized. This invention introduces a soluble pitch component into the electrospinning solution, utilizing the characteristic that polycyclic aromatic hydrocarbons easily form carbon crystals at high temperatures, to regulate the distribution of graphite microcrystals inside the carbon fiber, thereby improving the electron transfer performance of the carbon fiber paper and achieving simultaneous and precise control of "conductivity, permeability, and ultra-thin thickness," which has good application effects in fuel cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon fiber paper technology, and in particular to a carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt, its preparation method, and its application. Background Technology

[0002] The gas diffusion layer (GDL) is a core component of a proton exchange membrane fuel cell (PEMFC), situated between the catalyst layer and the bipolar plates. It primarily performs multiple functions, including the transport of fuel gas from the bipolar plates to the catalyst layer, the transfer of electrons, heat, and water generated by the electrochemical reactions in the catalyst layer to the bipolar plates, and supporting the catalyst layer and microporous layer. Therefore, it plays a crucial role in the overall performance of the PEMFC. Consequently, carbon fiber paper, with its excellent electrical conductivity, chemical resistance, mechanical stability, and permeability, is widely used in GDLs.

[0003] The factors affecting the conductivity of carbon fiber paper mainly fall into two categories: the electronic conductivity of the carbon fiber matrix material itself and the electronic conductivity between the resin carbon and the fibers, with the former having a more significant impact on conductivity. A method for preparing carbon fiber paper (application number: 201810741949.5) uses mesophase pitch-based carbon fiber as a functional additive, mixing it with polyacrylonitrile-based carbon fiber in a certain proportion before wet papermaking to improve the conductivity of the carbon fiber paper. Patent application number 202110706943.6 proposes a method of adding a mesophase pitch fiber layer to the surface of carbon fiber base paper using a melt-blowing method to improve the conductivity of the carbon fiber paper. While mixing the two types of fibers for papermaking or melt-blowing can improve the conductivity of carbon fiber paper, pitch-based carbon fiber is brittle and prone to breakage during service, disrupting the original conductive pathways and causing an increase in the resistivity of the carbon fiber paper. This makes it difficult to meet the current urgent requirements of PEMFCs for high energy density and fast response speed.

[0004] Carbon fiber is composed of more than 90% carbon elements and has very few surface-active functional groups, resulting in high surface inertness. The wet papermaking process improves the dispersion uniformity and stability of short-cut carbon fibers in the aqueous phase by introducing additives (water-soluble dispersants, surfactants, etc.), but it still cannot effectively prevent the formation of fiber bundles during the papermaking process. This results in uneven paper thickness, rough surface, and poor air permeability after forming, which increases the contact resistance between the carbon fiber paper and the catalyst layer during battery operation and reduces battery performance. The patent application "A Continuous Production Process for Carbon Fiber Paper for Fuel Cell Gas Diffusion Layer" (application number: 202210520497.4) describes a process for producing loose carbon fiber paper by air-flow web forming and combing of chopped carbon fibers. Carbon powder is then injected perpendicular to the paper surface using a high-pressure injection device for fixation. The paper is then immersed in a resin-based slurry, and the thickness is controlled by a rolling mill. After carbonization and graphitization, a special carbon fiber paper is obtained, improving the dispersion and conductivity issues of chopped carbon fibers. However, the preparation process is complex, costly, and the carbon powder affects the air permeability of the carbon fiber paper. Patent application number 202310262305.9 describes a process for preparing a polyacrylonitrile-based nonwoven felt using electrospinning. After processing, the corresponding carbon fiber paper is obtained, avoiding the fiber dispersion problem. However, the conductivity problem of the polyacrylonitrile-based carbon fiber paper is not improved.

[0005] Pitch-based carbon fiber graphite crystallite has strong controllability in size control, with single crystal size greater than 10 nm. Its easy graphitization property makes the internal electron transport path of the fiber rich, and the single filament resistance can be less than 0.12 mΩ·cm, but it is brittle. Polyacrylonitrile-based carbon fiber graphite crystallite has high difficulty in size control, with single crystal size less than 10 nm. Its difficult graphitization property makes it have a disordered graphite structure, with outstanding mechanical properties but high resistivity.

[0006] Therefore, the research yielded a functional carbon fiber paper with good mechanical properties, low cost, high conductivity, controllable thickness, and ultrathinness, which has important application value and practical significance. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art by providing a carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt, its preparation method and application, so as to solve the problems of poor conductivity, uneven thickness and high cost of carbon fiber paper in the prior art.

[0008] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0009] This invention provides a method for preparing carbon fiber paper based on pitch / polyacrylonitrile-based nonwoven felt, comprising the following steps:

[0010] 1) The soluble asphalt solution and the acrylonitrile-itaconic acid copolymer solution are stirred, mixed, and degassed in sequence to obtain the electrospinning solution;

[0011] 2) Electrospin the electrospinning solution to obtain pitch / polyacrylonitrile-based nonwoven felt; the pitch / polyacrylonitrile-based nonwoven felt is then dried and pre-oxidized in sequence to obtain pre-oxidized felt;

[0012] 3) The pre-oxidized felt is impregnated in a resin solution, and then successively dried, hot-pressed, cured, carbonized, and graphitized to obtain carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt.

[0013] Preferably, the soluble asphalt solution in step 1) comprises asphalt extract and an organic solvent; the mass fraction of the soluble asphalt solution is 5-35%.

[0014] The mass fraction of the acrylonitrile-itaconic acid copolymer solution is 12-30%;

[0015] The mass ratio of the acrylonitrile-itaconic acid copolymer solution to the soluble asphalt solution is 1:0.10-0.65. Preferably, the asphalt extract is prepared by mixing asphalt and an organic solvent, and then sequentially extracting, centrifuging, rotary evaporating, and drying the mixture to obtain the asphalt extract.

[0016] The asphalt includes one or more of naphthalene pitch, petroleum pitch and coal pitch.

[0017] The organic solvent comprises one or more of n-heptane, quinoline, pyridine, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide;

[0018] The mass ratio of the asphalt to the organic solvent is 1:4 to 8.

[0019] Preferably, the extraction method is one or more of ultrasound-assisted extraction, Soxhlet extraction, and magnetic stirring.

[0020] The stirring and mixing temperature and the degassing temperature are independently 40–90°C, and the stirring and mixing time and the degassing time are independently 3–12 h.

[0021] Preferably, the electrospinning flow rate in step 2) is 0.8–2.2 mL / h, the electrospinning time is 2–6 h, and the thickness of the pitch / polyacrylonitrile-based nonwoven felt is 0.14–0.30 mm.

[0022] Preferably, the drying temperature in step 2) is 60–100°C, and the drying time is 1–3 hours.

[0023] The pre-oxidation process includes three pre-oxidation steps: the first pre-oxidation is carried out at a temperature of 170–200°C for 10–20 min; the second pre-oxidation is carried out at a temperature of 220–260°C for 25–90 min; and the third pre-oxidation is carried out at a temperature of 280–320°C for 30–60 min.

[0024] Preferably, the resin solution in step 3) has a mass fraction of 5-18%, the resin in the resin solution is boron phenolic resin, and the solvent is methanol and / or ethanol; the impregnation time in the resin solution is 10-80 min.

[0025] Step 3) The drying temperature is 50-100℃ and the time is 20-60 min; the hot pressing curing temperature is 130-170℃, the pressure is 5-13 MPa, and the time is 10-25 min.

[0026] Preferably, the carbonization temperature in step 3) is 800–1400℃ and the time is 5–30 min; the graphitization temperature is 2000–2800℃ and the time is 5–20 min; the heating rate from room temperature to carbonization temperature and the heating rate from carbonization temperature to graphitization temperature are independently 3–10℃ / min; carbonization and graphitization are carried out under a protective atmosphere.

[0027] The present invention also provides carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt prepared by the aforementioned preparation method, wherein the carbon fiber paper has a resistivity of 3-8 mΩ·cm, a thickness of 0.05-0.12 mm, and an air permeability of 1500-2200 mL·mm / (cm). 2 ·hr·mmAq).

[0028] The present invention also provides the application of the aforementioned carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt in the gas diffusion layer of a proton exchange membrane fuel cell.

[0029] The beneficial effects of this invention include the following:

[0030] 1) This invention uses soluble pitch and polyacrylonitrile-based carbon fiber as raw materials for carbon fiber paper. Pitch has a macromolecular structure of polycyclic aromatic hydrocarbons and alkyl side chains, which exhibits soft carbon properties and a high degree of graphitization under high temperature conditions. Compared with polyacrylonitrile-based carbon fiber, pitch-based carbon fiber often has higher electrical conductivity but poorer mechanical properties. Based on this, by introducing a soluble pitch component into a polyacrylonitrile copolymer (acrylonitrile-itaconic acid copolymer) solution, the distribution of graphite microcrystals inside the fiber is controlled by utilizing the characteristic that polycyclic aromatic hydrocarbons easily form carbon crystals at high temperatures, thereby improving the electron transfer performance of carbon fiber paper. This expands the preparation process of carbon fiber paper for fuel cell gas diffusion layers and reduces the preparation cost of carbon fiber paper.

[0031] 2) This invention uses electrospinning technology to prepare carbon fiber paper. By adjusting parameters such as the concentration of the spinning solution, the spinning flow rate, and the spinning time, nonwoven mats with different thicknesses and pore structures can be accurately prepared without the need for dispersants, thus solving the problems of poor fiber dispersion and uneven thickness. Carbon fiber paper based on pitch / polyacrylonitrile is prepared through processes such as pre-oxidation, resin impregnation, hot pressing curing, carbonization, and graphitization, achieving simultaneous and precise control of the "conductivity, air permeability, and ultrathinness" of carbon fiber paper.

[0032] 3) The method of inducing fiber graphitization by pitch large-size graphite microcrystals in the high-temperature carbonization stage of this invention is simple to operate, has low energy consumption and low cost. On the basis of good mechanical properties, it realizes the preparation of low-cost, high-conductivity, controllable thickness, and ultra-thin functional carbon fiber paper. It is easy to mass-produce high-performance carbon fiber paper and has good application effect in fuel cells, providing a new path for further industrial production of carbon fiber paper. Attached Figure Description

[0033] Figure 1 Here is a scanning electron microscope image of the surface of the resin-impregnated pre-oxidized felt from Example 1;

[0034] Figure 2 This is a scanning electron microscope image of the surface of the carbon fiber paper in Example 2;

[0035] Figure 3 This is a cross-sectional scanning electron microscope image of the resin-impregnated pre-oxidized felt from Example 3;

[0036] Figure 4 This is a scanning electron microscope image of the cross-section of carbon fiber paper in Example 4;

[0037] Figure 5 The images show in-situ X-ray diffraction patterns of carbon fiber paper treated with carbonization in Example 5 and carbon fiber paper treated with carbonization in Comparative Example 1. Detailed Implementation

[0038] This invention provides a method for preparing carbon fiber paper based on pitch / polyacrylonitrile-based nonwoven felt, comprising the following steps:

[0039] 1) The soluble asphalt solution and the acrylonitrile-itaconic acid copolymer solution are stirred, mixed, and degassed in sequence to obtain the electrospinning solution;

[0040] 2) Electrospin the electrospinning solution to obtain pitch / polyacrylonitrile-based nonwoven felt; the pitch / polyacrylonitrile-based nonwoven felt is then dried and pre-oxidized in sequence to obtain pre-oxidized felt;

[0041] 3) The pre-oxidized felt is impregnated in a resin solution, and then successively dried, hot-pressed, cured, carbonized, and graphitized to obtain carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt.

[0042] In this invention, the soluble asphalt solution in step 1) comprises asphalt extract and organic solvent; the mass fraction of the soluble asphalt solution is preferably 5-35%, more preferably 10-30%, and even more preferably 15-25%.

[0043] The mass fraction of the acrylonitrile-itaconic acid copolymer solution is preferably 12-30%, more preferably 15-25%, and even more preferably 18-22%.

[0044] The mass ratio of the acrylonitrile-itaconic acid copolymer solution to the soluble asphalt solution is preferably 1:0.10 to 0.65, more preferably 1:0.15 to 0.55, and even more preferably 1:0.20 to 0.40.

[0045] In this invention, the method for preparing asphalt extract is as follows: asphalt and organic solvent are mixed, and the mixture is sequentially extracted, centrifuged, rotary evaporated, and dried to obtain asphalt extract;

[0046] The asphalt preferably includes one or more of naphthalene pitch, petroleum pitch and coal pitch;

[0047] The organic solvent preferably comprises one or more of n-heptane, quinoline, pyridine, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide;

[0048] The mass ratio of the asphalt to the organic solvent is preferably 1:4 to 8, more preferably 1:5 to 7, and even more preferably 1:6.

[0049] In this invention, the asphalt is preferably obtained by grinding and sieving asphalt blocks, with the sieve mesh size being 100 mesh.

[0050] In this invention, the extraction method is preferably one or more of ultrasound-assisted extraction, Soxhlet extraction, and magnetic stirring;

[0051] The stirring and mixing temperature and the degassing temperature are preferably 40-90°C, more preferably 50-80°C, and even more preferably 60-70°C. The stirring and mixing time and the degassing time are preferably 3-12 hours, more preferably 4-10 hours, and even more preferably 5-8 hours.

[0052] In this invention, the extraction temperature is preferably 30–40°C, more preferably 32–38°C, and even more preferably 35–36°C; the extraction time is preferably 10–14 h, more preferably 11–13 h, and even more preferably 12 h; the centrifugation speed is preferably 5000–7000 rpm, more preferably 5500–6500 rpm, and even more preferably 6000 rpm; the centrifugation time is preferably 8–12 min, more preferably 9–11 min, and even more preferably 10 min; the rotary evaporation temperature is preferably 50–100°C, more preferably 70–90°C, and even more preferably 80°C; the rotary evaporation speed is preferably 130–140 rpm, and even more preferably 135 rpm; the drying temperature is preferably 50–70°C, more preferably 55–65°C, and even more preferably 60°C; the drying time is preferably 22–26 h, more preferably 23–25 h, and even more preferably 24 h.

[0053] In this invention, the electrospinning flow rate in step 2) is preferably 0.8–2.2 mL / h, more preferably 1–2 mL / h, and even more preferably 1.2–1.8 mL / h; the electrospinning time is preferably 2–6 h, more preferably 3–5 h, and even more preferably 4 h; the positive voltage for electrospinning is preferably 12–20 kV, more preferably 14–18 kV, and even more preferably 15–16 kV; the thickness of the pitch / polyacrylonitrile-based nonwoven felt is preferably 0.14–0.30 mm, more preferably 0.15–0.28 mm, and even more preferably 0.18–0.25 mm.

[0054] In this invention, the preparation process of the electrospinning solution is as follows: after mixing a soluble asphalt solution and N,N-dimethylformamide, an acrylonitrile-itaconic acid copolymer solution is slowly added multiple times, followed by sequential stirring and vacuum degassing to obtain the electrospinning solution.

[0055] In this invention, by controlling the content of asphalt in the acrylonitrile-itaconic acid copolymer solution, electrospinning solutions with different sensitivities to electric fields can be obtained. In subsequent processing, the differences in the quantity and distribution of graphite microcrystals inside the fiber enable differentiated and precise control of the conductivity of carbon fiber paper. The process is simple and low in cost.

[0056] In this invention, nonwoven felt is obtained by electrospinning the electrospinning solution onto a roller collector using electrospinning technology and adjusting the spinning flow rate, voltage, and time. This process does not require the introduction of external additives, the fibers are evenly dispersed, the thickness and pore structure of the nonwoven felt can be precisely controlled, and it has low energy consumption, low cost, and is easy to mass-produce.

[0057] In this invention, the drying temperature in step 2) is preferably 60-100°C, more preferably 70-90°C, and even more preferably 80°C; the drying time is preferably 1-3 hours, more preferably 1.5-2.5 hours, and even more preferably 2 hours.

[0058] The pre-oxidation process preferably includes three pre-oxidation steps. The temperature of the first pre-oxidation is preferably 170–200°C, more preferably 175–190°C, and even more preferably 180–185°C. The time of the first pre-oxidation is preferably 10–20 min, more preferably 12–18 min, and even more preferably 14–16 min. The temperature of the second pre-oxidation is preferably 220–260°C, more preferably 230–255°C, and even more preferably 240–250°C. The time of the second pre-oxidation is preferably 25–90 min, more preferably 35–85 min, and even more preferably 50–80 min. The temperature of the third pre-oxidation is preferably 280–320°C, more preferably 290–315°C, and even more preferably 300–310°C. The time of the third pre-oxidation is preferably 30–60 min, more preferably 35–55 min, and even more preferably 40–50 min.

[0059] In this invention, the heating rate from room temperature to 170-200°C is preferably 3-8°C / min, more preferably 4-7°C / min, and even more preferably 5-6°C / min; the heating rate from 170-200°C to 220-260°C is preferably 0.5-2°C / min, more preferably 1.1-1.8°C / min, and even more preferably 1.3-1.7°C / min; and the heating rate from 220-260°C to 280-320°C is preferably 4-8°C / min, more preferably 4.5-6.5°C / min, and even more preferably 5-6°C / min.

[0060] In this invention, the pre-oxidation atmosphere of the nonwoven felt is air.

[0061] In this invention, the mass fraction of the resin solution in step 3) is preferably 5-18%, more preferably 8-12%, and even more preferably 10%; the resin in the resin solution is preferably boron phenolic resin, and the solvent is preferably methanol and / or ethanol; the impregnation time in the resin solution is preferably 10-80 min, more preferably 20-70 min, and even more preferably 30-60 min; the impregnation method of the boron phenolic resin solution is vacuum impregnation or atmospheric pressure impregnation, and the vacuum degree of vacuum impregnation is preferably 100-150 Pa, more preferably 110-130 Pa, and even more preferably 115-125 Pa.

[0062] In this invention, the boron phenolic resin is prepared using a method known in the art, and the boron phenolic resin is a resin with a high carbon residue rate. The boron phenolic resin can improve the bonding at the intersections between monofilament fibers, which can stabilize the mechanical properties of carbon fiber paper and ensure good electron transport properties.

[0063] In this invention, the drying temperature in step 3) is preferably 50-100℃, more preferably 60-90℃, and even more preferably 70-80℃; the drying time is preferably 20-60 min, more preferably 30-50 min, and even more preferably 40 min; the hot-press curing temperature is preferably 130-170℃, more preferably 140-160℃, and even more preferably 150℃; the hot-press curing pressure is preferably 5-13 MPa, more preferably 7-11 MPa, and even more preferably 8-10 MPa; and the hot-press curing time is preferably 10-25 min, more preferably 15-20 min, and even more preferably 16-18 min.

[0064] In this invention, the carbonization temperature in step 3) is preferably 800–1400°C, more preferably 900–1300°C, and even more preferably 1000–1200°C; the carbonization time is preferably 5–30 min, more preferably 10–25 min, and even more preferably 15–20 min; the graphitization temperature is preferably 2000–2800°C, more preferably 2200–2600°C, and even more preferably 2300–2500°C; the graphitization time is preferably 5–20 min, more preferably 8–18 min, and even more preferably 10–15 min; the heating rate from room temperature to carbonization temperature and the heating rate from carbonization temperature to graphitization temperature are independently preferably 3–10°C / min, more preferably 5–8°C / min, and even more preferably 6–7°C / min; carbonization and graphitization are preferably carried out under a protective atmosphere, preferably high-purity nitrogen or high-purity argon.

[0065] In this invention, the carbonization and graphitization process is preferably carried out in a one-step carbonization and graphitization process in a multi-stage distributed temperature-controlled tube furnace.

[0066] The present invention also provides carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt prepared by the aforementioned preparation method, wherein the carbon fiber paper has a resistivity of 3-8 mΩ·cm, a thickness of 0.05-0.12 mm, and an air permeability of 1500-2200 mL·mm / (cm). 2 ·hr·mmAq).

[0067] In this invention, the resistivity of the carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt is preferably 3.2–6 mΩ·cm, more preferably 4–5 mΩ·cm; the thickness is preferably 0.06–0.10 mm, more preferably 0.07–0.09 mm; and the air permeability is preferably 1700–2100 mL·mm / (cm²). 2 ·hr·mmAq), more preferably 1800~2000mL·mm / (cm 2 ·hr·mmAq).

[0068] The present invention also provides the application of the aforementioned carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt in the gas diffusion layer of a proton exchange membrane fuel cell.

[0069] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0070] The multi-stage step-by-step temperature-controlled tube furnace used in the examples and comparative examples is model KSL-1700X-GS.

[0071] The preparation process of the acrylonitrile-itaconic acid copolymer solution is as follows: acrylonitrile and itaconic acid are added to the solvent N,N-dimethylformamide at a mass ratio of 98:2, and stirred for 60 min under a nitrogen atmosphere and a 35°C water bath; the initiator azobisisoheptanenitrile (the mass of the initiator is 0.8% of the total mass of acrylonitrile and itaconic acid monomers) is added and fully dissolved in the solvent, and reacted at a water bath temperature of 50°C and a rotation speed of 130 rpm for 20 h; after removing unreacted monomers (the equipment automatically removes unreacted monomers) and degassing, a certain mass fraction of acrylonitrile-itaconic acid copolymer solution is obtained.

[0072] The ultrasonic frequency for ultrasonic-assisted solvent extraction was 45 kHz, the vacuum degree for vacuum rotary evaporation was 0.08 MPa, and the vacuum degree for vacuum degassing was -0.7 bar.

[0073] Example 1

[0074] Naphthalene pitch was thoroughly ground in a pulverizer and sieved through a 100-mesh sieve. The resulting powder was mixed with quinoline at a mass ratio of 1:5. The mixture was subjected to ultrasonic-assisted solvent extraction at 35°C for 12 hours. After extraction, the mixture was transferred to a centrifuge tube and centrifuged at 6000 rpm for 10 minutes. After filtration, the extract was subjected to vacuum rotary evaporation at 135 rpm and a water bath temperature of 90°C. The precipitated soluble pitch was dried in a forced-air drying oven at 60°C for 24 hours to obtain the pitch extract. The pitch extract was then mixed evenly with quinoline to obtain a 15% (w / w) soluble pitch solution.

[0075] N,N-dimethylformamide (0.4 mL N,N-dimethylformamide per mL of soluble asphalt solution) was added to the soluble asphalt solution and stirred at 500 rpm for 60 min. Then, an acrylonitrile-itaconic acid copolymer solution (20% by mass and a mass ratio of 1:0.15 between the acrylonitrile-itaconic acid copolymer solution and the soluble asphalt solution) was slowly added to the system in three portions. The mixture was stirred at 60 °C and 300 rpm for 6 h and then degassed under vacuum at 60 °C for 5 h to obtain the asphalt / polyacrylonitrile spinning solution.

[0076] Electrospinning technology was used with a positive voltage of 13kV, a negative voltage of -1.5kV, a receiving distance of 15cm, and a flow rate of 1.5mL / h. The spinning solution was uniformly sprayed onto the roller collector by a Taylor cone formed by the polarization of the spinning solution at the tip of the needle. The spinning time was 4h, and a nonwoven felt with a thickness of 0.22mm was obtained. It was then dried in a 65℃ forced-air drying oven for 2h.

[0077] Nonwoven felt was placed in a multi-stage, stepwise, temperature-controlled tube furnace with an air flow rate of 0.4 L / min. The temperature was increased from room temperature to 180℃ at a rate of 5℃ / min and held for 15 min; then increased from 180℃ to 250℃ at a rate of 1.2℃ / min and held for 50 min; finally, increased from 250℃ to 300℃ at a rate of 5℃ / min and held for 45 min to obtain pre-oxidized felt. The pre-oxidized felt was slowly immersed in a methanol solution of boron phenolic resin (the mass fraction of boron phenolic resin in the methanol solution was 12%) and vacuum impregnated at 120 Pa for 60 min. After impregnation, it was transferred to a 70℃ forced-air drying oven for 45 min; subsequently, it was hot-pressed and cured for 18 min at a flat vulcanizing machine with an upper and lower plate temperature of 150℃ and a pressure of 8 MPa to obtain resin-impregnated pre-oxidized felt.

[0078] The resin-impregnated pre-oxidized felt was transferred into a multi-stage stepwise temperature-controlled tube furnace and heated from room temperature to 1000℃ at a rate of 5℃ / min under a high-purity nitrogen atmosphere, and held for 20 min. Then, under a high-purity argon atmosphere, the temperature was increased from 1000℃ to 2300℃ at a rate of 7℃ / min and held for 15 min to obtain carbon fiber paper based on pitch / polyacrylonitrile.

[0079] The carbon fiber paper in this embodiment has a resistivity of 4.3 mΩ·cm, a thickness of 0.11 mm, and an air permeability of 1800 mL·mm / (cm). 2 ·hr·mmAq).

[0080] The surface scanning electron microscope image of the resin-impregnated pre-oxidized felt in this embodiment is shown below. Figure 1 As shown, by Figure 1The morphology and microstructure show that the fibers inside the pre-oxidized felt are interwoven, especially at the overlap, where the resin tightly bonds the two fibers together, while the original pore structure of the pre-oxidized felt is preserved.

[0081] Example 2

[0082] The mass ratio of acrylonitrile-itaconic acid copolymer solution to soluble asphalt solution in Example 1 was changed to 1:0.30, while other conditions remained the same as in Example 1.

[0083] The carbon fiber paper in this embodiment has a resistivity of 3.9 mΩ·cm, a thickness of 0.12 mm, and an air permeability of 1730 mL·mm / (cm). 2 ·hr·mmAq).

[0084] The surface scanning electron microscope image of the carbon fiber paper in this embodiment is shown below. Figure 2 As shown, by Figure 2 The surface morphology shows that after one step of carbonization and graphitization, the resin carbon is tightly bonded to the fiber overlap, and there is no situation where the pore structure is blocked due to the cracking of the resin carbon, effectively connecting the overlap of the monofilament fibers.

[0085] Example 3

[0086] The solvent for extracting asphalt in Example 1 was changed from quinoline to dimethyl sulfoxide, while other conditions remained the same as in Example 1.

[0087] The carbon fiber paper in this embodiment has a resistivity of 5.1 mΩ·cm, a thickness of 0.10 mm, and an air permeability of 2000 mL·mm / (cm). 2 ·hr·mmAq).

[0088] The cross-sectional scanning electron microscope image of the resin-impregnated pre-oxidized felt in this embodiment is shown below. Figure 3 As shown, by Figure 3 The cross-sectional morphology shows that the resin penetrates well into the interior of the pre-oxidized felt along the thickness direction. Especially at the overlap, the intersection of the monofilament fibers is tightly bonded together by the resin, while the original pore structure is well preserved.

[0089] Example 4

[0090] The spinning time in Example 1 was changed from 4 hours to 2 hours, while other conditions remained the same as in Example 1.

[0091] The carbon fiber paper in this embodiment has a resistivity of 4.0 mΩ·cm, a thickness of 0.06 mm, and an air permeability of 2100 mL·mm / (cm). 2 ·hr·mmAq).

[0092] The cross-sectional scanning electron microscope image of the carbon fiber paper in this embodiment is shown below. Figure 4 As shown, by Figure 4 The cross-sectional morphology shows that along the thickness direction of the carbon fiber paper, the overlapping and crossing points of the monofilament fibers are tightly bonded by the resin carbon, and there is no phenomenon of resin carbon falling off and causing blockage of the pore structure; along the horizontal direction of the carbon fiber paper, the fibers are well dispersed and the thickness is uniform.

[0093] Example 5

[0094] Petroleum asphalt was thoroughly ground in a pulverizer and sieved through a 100-mesh sieve. The resulting powder was mixed with tetrahydrofuran at a mass ratio of 1:6. The mixture was subjected to ultrasonic-assisted solvent extraction at 35°C for 12 hours. After extraction, it was transferred to a centrifuge tube and centrifuged at 6000 rpm for 10 minutes. After filtration, the extract was subjected to vacuum rotary evaporation at 135 rpm and a water bath temperature of 50°C. The precipitated soluble asphalt was dried in a forced-air drying oven at 60°C for 24 hours to obtain asphalt extract. The asphalt extract was mixed evenly in tetrahydrofuran to obtain a 15% soluble asphalt solution.

[0095] N,N-dimethylformamide (0.5 mL N,N-dimethylformamide per mL of soluble asphalt solution) was added to the soluble asphalt solution and stirred at 500 rpm for 60 min. Then, an acrylonitrile-itaconic acid copolymer solution (22% by mass and a mass ratio of 1:0.20 to the soluble asphalt solution) was slowly added to the system in three portions. The mixture was stirred at 60 °C and 300 rpm for 6 h and then degassed under vacuum at 60 °C for 5 h to obtain the asphalt / polyacrylonitrile spinning solution.

[0096] Electrospinning technology was used with a positive voltage of 13kV, a negative voltage of -1.5kV, a receiving distance of 15cm, and a flow rate of 1.8mL / h. The spinning solution was uniformly sprayed onto the roller collector by a Taylor cone formed by the polarization of the spinning solution at the tip of the needle. The spinning time was 2.5h, resulting in a nonwoven felt with a thickness of 0.17mm. The felt was then dried in a 65℃ forced-air drying oven for 2h.

[0097] Nonwoven felt was placed in a multi-stage, stepwise, temperature-controlled tube furnace with an air flow rate of 0.4 L / min. The temperature was increased from room temperature to 185°C at a rate of 5°C / min and held for 15 min; then increased from 185°C to 240°C at a rate of 1.2°C / min and held for 50 min; finally, increased from 240°C to 300°C at a rate of 5°C / min and held for 50 min to obtain pre-oxidized felt. The pre-oxidized felt was slowly immersed in a methanol solution of boron phenolic resin (the mass fraction of boron phenolic resin in the methanol solution was 10%) and vacuum impregnated at 120 Pa for 50 min. After impregnation, it was transferred to a 70°C forced-air drying oven for 45 min; then hot-pressed for 15 min. The upper and lower plates of the flat vulcanizing machine were at a temperature of 150°C and a pressure of 10 MPa to obtain resin-impregnated pre-oxidized felt.

[0098] The resin-impregnated pre-oxidized felt was transferred into a multi-stage stepwise temperature-controlled tube furnace and heated from room temperature to 1000℃ at a rate of 5℃ / min under a high-purity nitrogen atmosphere, and held for 20 min. Then, under a high-purity argon atmosphere, the temperature was increased from 1000℃ to 2200℃ at a rate of 7℃ / min and held for 15 min to obtain carbon fiber paper based on pitch / polyacrylonitrile.

[0099] The carbon fiber paper in this embodiment has a resistivity of 3.9 mΩ·cm, a thickness of 0.09 mm, and an air permeability of 1900 mL·mm / (cm). 2 ·hr·mmAq).

[0100] Example 6

[0101] Coal tar pitch was thoroughly ground in a pulverizer and sieved through a 100-mesh sieve. The resulting powder was mixed with pyridine at a mass ratio of 1:5. The mixture was subjected to ultrasonic-assisted solvent extraction at 35°C for 12 hours. After extraction, the mixture was transferred to a centrifuge tube and centrifuged at 6000 rpm for 10 minutes. After filtration, the extract was subjected to vacuum rotary evaporation at 135 rpm and a water bath temperature of 90°C. The precipitated soluble asphalt was dried in a forced-air drying oven at 60°C for 24 hours to obtain asphalt extract. The asphalt extract was then mixed evenly with pyridine to obtain a soluble asphalt solution with a mass fraction of 25%.

[0102] N,N-dimethylformamide (0.7 mL N,N-dimethylformamide per mL of soluble asphalt solution) was added to the soluble asphalt solution and stirred at 500 rpm for 60 min. Then, an acrylonitrile-itaconic acid copolymer solution (22% by mass and a mass ratio of 1:0.40 to the soluble asphalt solution) was slowly added to the system in three portions. The mixture was stirred at 60 °C and 300 rpm for 6 h and then degassed under vacuum at 60 °C for 5 h to obtain the asphalt / polyacrylonitrile spinning solution.

[0103] Electrospinning technology was used with a positive voltage of 13kV, a negative voltage of -1.5kV, a receiving distance of 15cm, and a flow rate of 1.6mL / h. The spinning solution was uniformly sprayed onto the roller collector by a Taylor cone formed by the polarization of the spinning solution at the tip of the needle. The spinning time was 3h, and a nonwoven felt with a thickness of 0.17mm was obtained. It was then dried in a 65℃ forced-air drying oven for 2h.

[0104] Nonwoven felt was placed in a multi-stage, stepwise, temperature-controlled tube furnace with an air flow rate of 0.4 L / min. The temperature was increased from room temperature to 180℃ at a rate of 5.5℃ / min and held for 15 min; then increased from 180℃ to 260℃ at a rate of 1.5℃ / min and held for 80 min; finally, increased from 260℃ to 320℃ at a rate of 4.5℃ / min and held for 50 min to obtain pre-oxidized felt. The pre-oxidized felt was slowly immersed in a methanol solution of boron phenolic resin (the mass fraction of boron phenolic resin in the methanol solution was 9%) and vacuum impregnated at 120 Pa for 60 min. After impregnation, it was transferred to a 70℃ forced-air drying oven for 45 min; then hot-pressed for 20 min. The upper and lower plates of the flat vulcanizing machine were at a temperature of 140℃ and a pressure of 9 MPa to obtain resin-impregnated pre-oxidized felt.

[0105] The resin-impregnated pre-oxidized felt was transferred into a multi-stage stepwise temperature-controlled tube furnace and heated from room temperature to 1200°C at a rate of 7°C / min under a high-purity nitrogen atmosphere, and held for 20 min. Then, under a high-purity argon atmosphere, the temperature was increased from 1200°C to 2200°C at a rate of 7°C / min and held for 20 min to obtain carbon fiber paper based on pitch / polyacrylonitrile.

[0106] The carbon fiber paper in this embodiment has a resistivity of 3.5 mΩ·cm, a thickness of 0.10 mm, and an air permeability of 1730 mL·mm / (cm). 2 ·hr·mmAq).

[0107] Comparative Example 1

[0108] The soluble asphalt solution of Example 1 was replaced with the same mass of solvent quinoline. N,N-dimethylformamide was added to the quinoline (0.4 mL of N,N-dimethylformamide per mL of quinoline), and the mixture was stirred at 500 rpm for 60 min. The acrylonitrile-itaconic acid copolymer solution (20% by mass and a mass ratio of acrylonitrile-itaconic acid copolymer solution to quinoline of 1:0.15) was slowly added to the system in three portions. Other process conditions were the same as in Example 1.

[0109] The carbon fiber paper in this comparative example has a resistivity of 10.3 mΩ·cm, a thickness of 0.09 mm, and an air permeability of 1500 mL·mm / (cm). 2·hr·mmAq).

[0110] In-situ X-ray diffraction patterns of carbonized carbon fiber paper in Example 5 and carbonized carbon fiber paper in Comparative Example 1 are shown below. Figure 5 As shown, by Figure 5 It can be seen that, under the same preparation and processing conditions, the introduction of soluble bitumen in Example 5 is beneficial to reducing the interlayer spacing of microcrystals in carbon fibers and increasing the crystallite size. The polyacrylonitrile-based carbon fibers in Comparative Example 1 have a larger interlayer spacing and smaller crystallite size.

[0111] Comparative Example 2

[0112] Carbon fiber paper was prepared using a traditional wet papermaking process. Commercially available short-cut polyacrylonitrile-based carbon fibers (T700, 8 mm) were placed in a fiber dissociator and slowly added to an aqueous solution of surfactants. The surfactants were hydroxymethyl cellulose with a viscosity of 100,000 and polyethylene oxide with a viscosity-average molecular weight of 5 million. The mass fraction of both hydroxymethyl cellulose and polyethylene oxide was 0.1%. The mixture was stirred at 500 rpm for 3 minutes to obtain a dispersion of short-cut carbon fibers.

[0113] The dispersion was transferred to a paper forming apparatus and dehydrated under a vacuum of 0.05 MPa for 80 seconds. The chopped carbon fiber dispersion was then passed through a stainless steel filter screen, forming a 20 cm × 20 cm carbon fiber base paper with a thickness of 0.16 mm on the filter screen surface. This base paper was then slowly immersed in a methanol solution of boron phenolic resin (the mass fraction of boron phenolic resin in the methanol solution was 12%) and vacuum impregnated at 120 Pa for 60 min. It was then transferred to a 70 °C forced-air drying oven for 45 min and dried. After that, it was hot-pressed and cured for 18 min at a flat vulcanizing machine with the upper and lower plates at a temperature of 150 °C and a pressure of 8 MPa to obtain the resin-impregnated carbon fiber base paper. This base paper was then transferred to a multi-stage stepwise temperature-controlled tube furnace and heated from room temperature to 1000 °C at a rate of 5 °C / min under a high-purity nitrogen atmosphere, and held at that temperature for 20 min. Then, under a high-purity argon atmosphere, the temperature was increased from 1000 °C to 2300 °C at a rate of 7 °C / min and held at that temperature for 15 min to obtain the carbon fiber paper.

[0114] The carbon fiber paper in this comparative example has a resistivity of 12.6 mΩ·cm, a thickness of 0.19 mm, and an air permeability of 1380 mL·mm / (cm). 2 ·hr·mmAq).

[0115] As can be seen from the examples and comparative examples, the carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt prepared by the present invention has significantly reduced resistivity, uniform thickness, and is easy to prepare into ultrathin sheets. It also has excellent air permeability and achieves simultaneous and precise control of conductivity, thickness control, and ultrathinness. This provides a new design idea for the preparation of functional carbon fiber paper materials for PEMFC. At the same time, the preparation process is simple, energy consumption is low, and cost is low, which has a good foundation for industrial promotion.

[0116] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing carbon fiber paper based on pitch / polyacrylonitrile-based nonwoven felt, characterized in that, It includes the following steps: 1) The soluble asphalt solution and the acrylonitrile-itaconic acid copolymer solution are stirred, mixed, and degassed in sequence to obtain the electrospinning solution; 2) Electrospin the electrospinning solution to obtain pitch / polyacrylonitrile-based nonwoven felt; the pitch / polyacrylonitrile-based nonwoven felt is then dried and pre-oxidized in sequence to obtain pre-oxidized felt; 3) The pre-oxidized felt is impregnated in a resin solution, and then successively dried, hot-pressed, cured, carbonized, and graphitized to obtain carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt; In the preparation process of the acrylonitrile-itaconic acid copolymer solution, the mass ratio of acrylonitrile to itaconic acid is 98:2; Step 1) The soluble asphalt solution contains asphalt extract and organic solvent; The preparation method of bitumen extract is as follows: bitumen and organic solvent are mixed, and the mixture is sequentially extracted, centrifuged, rotary evaporated and dried to obtain bitumen extract; The asphalt is petroleum asphalt and / or coal tar pitch; The organic solvent comprises one or more of n-heptane, quinoline, pyridine, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide; The mass ratio of the asphalt to the organic solvent is 1:4~8; Step 2) The drying temperature is 60~100°C and the drying time is 1~3h; the pre-oxidation procedure includes three pre-oxidations: the first pre-oxidation temperature is 170~200°C and the time is 10~20min; the second pre-oxidation temperature is 220~260°C and the time is 25~90min; the third pre-oxidation temperature is 280~320°C and the time is 30~60min. Step 3) The resin solution has a mass fraction of 5-18%, the resin is boron phenolic resin, and the solvent is methanol and / or ethanol; the impregnation time in the resin solution is 10-80 min; the drying temperature is 50-100℃ and the time is 20-60 min; the hot pressing curing temperature is 130-170℃, the pressure is 5-13 MPa, and the time is 10-25 min.

2. The method for preparing carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt according to claim 1, characterized in that, The mass fraction of soluble asphalt solution is 5-35%; The mass fraction of the acrylonitrile-itaconic acid copolymer solution is 12-30%. The mass ratio of acrylonitrile-itaconic acid copolymer solution to soluble asphalt solution is 1:0.10~0.

65.

3. The method for preparing carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt according to claim 2, characterized in that, The extraction method is one or more of ultrasound-assisted extraction, Soxhlet extraction and magnetic stirring. The stirring and mixing temperature and the degassing temperature are independently 40~90℃, and the stirring and mixing time and the degassing time are independently 3~12h.

4. The method for preparing carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt according to claim 1 or 2, characterized in that, Step 2) The electrospinning flow rate is 0.8~2.2mL / h, and the electrospinning time is 2~6h; the thickness of the pitch / polyacrylonitrile-based nonwoven felt is 0.14~0.30mm.

5. The method for preparing carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt according to claim 4, characterized in that, Step 3) The carbonization temperature is 800~1400℃ and the time is 5~30min; the graphitization temperature is 2000~2800℃ and the time is 5~20min; the heating rate from room temperature to carbonization temperature and the heating rate from carbonization temperature to graphitization temperature are independently 3~10℃ / min; carbonization and graphitization are carried out under a protective atmosphere.

6. The carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt prepared by the preparation method according to any one of claims 1 to 5, characterized in that, The carbon fiber paper has a resistivity of 3~8 mΩ·cm, a thickness of 0.05~0.12 mm, and an air permeability of 1500~2200 mL·mm / (cm). 2 ·hr·mmAq).

7. The application of the carbon fiber paper based on pitch / polyacrylonitrile nonwoven felt as described in claim 6 in the gas diffusion layer of a proton exchange membrane fuel cell.

Citation Information

Patent Citations

  • Carbon fiber paper preparation method

    CN108914681A

  • Preparation method of carbon fiber paper

    CN113584940A

  • A continuous production process for carbon fiber paper used in fuel cell gas diffusion layers

    CN114976048B

  • Carbon fiber paper as well as preparation method and application thereof

    CN116479545A

  • Preparation method of two-phase carbon nanofibers andactivated carbon nanofibers by electrospinning frompolyacrylonitrile / pitch blend solutions

    KR100759102B1