An electrochemical device and an electronic device including the same

By using ternary materials of nickel-cobalt-manganese lithium oxide with different cobalt contents, and by controlling their chemical composition and particle size, a dense conductive network is formed, which solves the problem of poor low-temperature and low-SOC discharge performance of lithium-ion batteries. This achieves the characteristics of high discharge voltage and smooth discharge curve, improves low-temperature discharge capability and reduces cost.

CN120457550BActive Publication Date: 2026-11-24NINGDE AMPEREX TECHNOLOGY LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202480006118.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2026-11-24
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing lithium-ion batteries exhibit significantly degraded discharge performance under low temperature and low charge conditions, making it difficult to meet practical application requirements, and the use of lithium cobalt oxide materials is costly.

Method used

By employing two or more ternary materials of lithium nickel cobalt manganese oxide with different cobalt contents, and by controlling their chemical composition and particle size, combined with doping or coating elements, a dense conductive network is formed, the specific surface area is reduced, and a passivation film is formed, thereby improving the kinetic performance and discharge performance of the electrochemical device.

Benefits of technology

At low temperature and low SOC conditions, the discharge performance of lithium-ion batteries is improved, the discharge time is extended, and the impedance and cost of electrochemical devices are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

An electrochemical device includes a positive electrode, which comprises a positive electrode material layer, and the positive electrode material layer comprises a positive electrode active material. The positive electrode active material comprises two or more lithium nickel cobalt manganese oxide ternary materials. The two or more lithium nickel cobalt manganese oxide ternary materials are divided into two groups, and the first group of lithium nickel cobalt manganese oxide ternary materials has the chemical formula Li. n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.15≤y1≤0.60, the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, x2+y2+z2+m2=1, satisfying 0<y2≤0.14; based on the total mass of lithium nickel cobalt manganese oxide ternary materials, the mass percentage of the first group of lithium nickel cobalt manganese oxide ternary materials is 'a', and the mass percentage of the second group of lithium nickel cobalt manganese oxide ternary materials is 'b', 10%≤a≤80%, 20%≤b≤90%. By controlling the type and content of the positive electrode active material within the scope of this application, the discharge performance of NCM lithium batteries under low temperature and low SOC conditions can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrochemical technology, and in particular to an electrochemical device and its preparation method. Background Technology

[0002] The positive electrode active materials for lithium-ion batteries include ternary materials such as lithium nickel cobalt manganese oxide (NCM) and lithium cobalt oxide. Lithium batteries using NCM as the positive electrode active material have the advantages of low cost, high specific capacity, and good safety.

[0003] However, currently, NCM lithium batteries quickly reach the discharge cutoff voltage (3.0V) when discharging at low temperature and low state of charge (SOC), resulting in a significant deterioration in low-temperature, low-SOC discharge performance, which is difficult to meet the needs of practical product applications. Lithium batteries using lithium cobalt oxide as the cathode material can meet the requirements for low-temperature, low-SOC discharge, but lithium cobalt oxide materials require the consumption of cobalt metal resources, which are relatively scarce, resulting in higher costs and hindering the reduction of cell costs. Summary of the Invention

[0004] The purpose of this application is to provide an electrochemical device and an electronic device comprising the same, so as to improve the discharge performance of the electrochemical device under low temperature and low SOC conditions.

[0005] It should be noted that while this application uses lithium-ion batteries as an example of an electrochemical device to explain the invention, the electrochemical device described herein is not limited to lithium-ion batteries. The specific technical solution is as follows:

[0006] The first aspect of this application provides an electrochemical device, including a positive electrode sheet, the positive electrode sheet including a positive electrode material layer, the positive electrode material layer including a positive electrode active material, wherein the positive electrode active material includes two or more lithium nickel cobalt manganese oxide ternary materials; the two or more lithium nickel cobalt manganese oxide ternary materials are divided into two groups, the first group of lithium nickel cobalt manganese oxide ternary materials having the chemical formula Li n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.15≤y1≤0.60; the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, x2+y2+z2+m2=1, satisfying 0<y2≤0.14. By using two or more ternary materials of lithium nickel cobalt manganese oxide with different cobalt contents, the discharge performance of electrochemical devices under low temperature and low SOC conditions can be improved.

[0007] In one embodiment of this application, based on the total mass of the lithium nickel cobalt manganese oxide ternary materials, the mass percentage of the first group of lithium nickel cobalt manganese oxide ternary materials is 'a', and the mass percentage of the second group of lithium nickel cobalt manganese oxide ternary materials is 'b', with 10%≤a≤80% and 20%≤b≤90%; preferably, 30%≤a≤60% and 40%≤b≤70%; more preferably, 40%≤a≤60% and 40%≤b≤60%. By adjusting the content of lithium nickel cobalt manganese oxide ternary materials with different cobalt contents within the scope of this application, the discharge performance of the electrochemical device under low temperature and low SOC conditions can be improved.

[0008] In one embodiment of this application, the lithium nickel cobalt manganese oxide ternary material may include doping or coating elements, and the materials M1 and M2 are each independently selected from at least one of Ag, Sn, Zn, Al, Mo, Cu, B, Ti, and Fe. Adding the above-mentioned doping or coating elements to the positive electrode active material can make the conductive network on the surface of the positive electrode active material particles more compact, improving the kinetic performance of the electrochemical device; on the other hand, it can reduce the specific surface area of ​​the positive electrode active material, reducing side reactions between the positive electrode active material and the electrolyte; furthermore, it facilitates the formation of a passivation film on the surface of the positive electrode active material particles, improving the initial efficiency and reversible capacity of the electrochemical device. It should be noted that Li... n1 Ni x1 Co y1 Mn z1 M1 m1 O2 and Li n2 Ni x2 Co y2 Mn z2 M2 m2 In O2, m1 and m2 can be 0, meaning that nickel-cobalt-manganese ternary materials may not include doped or coated elements.

[0009] In one embodiment of this application, two or more lithium nickel cobalt manganese oxide ternary materials are divided into two groups according to their y-values. The first group of lithium nickel cobalt manganese oxide ternary materials satisfies 0.15≤y1≤0.50, and the second group of lithium nickel cobalt manganese oxide ternary materials satisfies 0.02≤y2≤0.10. By adjusting the molar amount of cobalt in the lithium nickel cobalt manganese oxide ternary materials within the range of this application, the impedance of the electrochemical device can be reduced, and the discharge voltage platform of the electrochemical device can be stabilized, which is beneficial to extending the low-temperature discharge time of the electrochemical device.

[0010] In one embodiment of this application, the particle size of the first group of lithium nickel cobalt manganese oxide ternary materials is D. V1 50, 1μm≤D V1 50≤10μm, preferably, 2μm≤D V150≤9μm. By controlling the particle size of lithium nickel cobalt manganese oxide material within the scope of this application, the lithium-ion transport distance during charging and discharging of the electrochemical device can be improved, thereby extending the discharge time of the electrochemical device in low-temperature environments.

[0011] In one embodiment of this application, the particle size of the second group of lithium nickel cobalt manganese oxide ternary materials is D. V2 50, 1μm≤D V2 50≤15μm, optionally, 2μm≤D V2 50≤10μm. By controlling the particle size of lithium nickel cobalt manganese oxide material within the scope of this application, the lithium-ion transport distance during charging and discharging of the electrochemical device can be improved, thereby extending the discharge time of the electrochemical device in low-temperature environments.

[0012] In one embodiment of this application, the first group of lithium nickel cobalt manganese oxide ternary materials has the chemical formula Li n1 Ni x1 Co y1 Mn z1 M1 m1 O2, where 0.95≤n1≤1.05, 0.3≤x1≤0.84, 0.01≤z1≤0.7, 0≤m1≤0.2; the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, where 0.95≤n2≤1.05, 0.3≤x2≤0.9, 0.01≤z2≤0.7, and 0≤m2≤0.2.

[0013] In one embodiment of this application, the positive electrode active material includes two ternary nickel-cobalt-manganese oxide materials, NCM-1 and NCM-2. NCM-1 satisfies: 0.15 ≤ y1 ≤ 0.60, and NCM-2 satisfies: 0 < y2 ≤ 0.14. By controlling the range of cobalt content y in the ternary nickel-cobalt-manganese oxide materials within the scope of this application, it is preferable to use two ternary nickel-cobalt-manganese oxide materials. This can reduce the impedance of the electrochemical device while increasing the discharge voltage platform of the electrochemical device, thereby improving the discharge capability of the electrochemical device in low-temperature environments.

[0014] In one embodiment of this application, the positive electrode material layer further includes a conductive agent and a binder. The conductive agent is selected from at least one of conductive carbon black and carbon nanotubes, and the binder is selected from at least one of polyacrylate, polyimide, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene-butadiene copolymer, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, sodium hydroxymethyl cellulose, and potassium hydroxymethyl cellulose.

[0015] In one embodiment of this application, the mass percentage of the conductive agent is 1% to 8% and the mass percentage of the binder is 1% to 3%, based on the mass of the positive electrode material layer.

[0016] A second aspect of this application provides a method for preparing the electrochemical device in any of the foregoing embodiments, comprising:

[0017] Preparation of positive electrode sheet: Two or more lithium nickel cobalt manganese oxide ternary materials are mixed to obtain positive electrode active material; wherein, the two or more lithium nickel cobalt manganese oxide ternary materials used are divided into two groups, and the chemical formula of the first group of lithium nickel cobalt manganese oxide ternary materials is Li n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.15≤y1≤0.60, the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, x2+y2+z2+m2=1, satisfying 0<y2≤0.14; the positive electrode active material is disposed on at least one surface in the thickness direction of the positive electrode current collector to obtain a positive electrode sheet. By adjusting the preparation method of the electrochemical device within the above range, the electrochemical device provided in this application can have good discharge performance under low temperature and low SOC conditions.

[0018] A third aspect of this application provides an electronic device that includes the electrochemical device in any of the foregoing embodiments.

[0019] The beneficial effects of this application are:

[0020] This application provides an electrochemical device, which includes a positive electrode sheet, a positive electrode material layer, and a positive electrode active material. The positive electrode active material includes two or more lithium nickel cobalt manganese oxide ternary materials, which are divided into two groups. The first group of lithium nickel cobalt manganese oxide ternary materials has the chemical formula Li. n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.15≤y1≤0.60, the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2O2, x2+y2+z2+m2=1, satisfying 0<y2≤0.14. By adjusting the type and content of the positive electrode active material within the scope of this application, the discharge performance of the electrochemical device under low temperature and low SOC conditions can be improved.

[0021] Of course, implementing any product or method of this application does not necessarily require achieving all of the advantages described above at the same time. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this application clearer, the following embodiments are provided to further illustrate this application in detail. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.

[0023] It should be noted that, in the specific embodiments of this application, a lithium-ion battery is used as an example of a secondary battery to explain this application; however, the secondary battery in this application is not limited to lithium-ion batteries. The specific technical solution is as follows:

[0024] This application provides an electrochemical device comprising a positive electrode, a positive electrode material layer, and a positive electrode active material. The positive electrode active material comprises two or more lithium nickel cobalt manganese oxide ternary materials, wherein the lithium nickel cobalt manganese oxide ternary materials have a layered structure. The chemical formula of the lithium nickel cobalt manganese oxide ternary material is Li. n Ni x Co y Mn z M m O2, x+y+z+m=1; the molar amount of cobalt atoms in lithium nickel cobalt manganese oxide ternary materials is y. Two or more lithium nickel cobalt manganese oxide ternary materials are divided into two groups according to the value of y. The chemical formula of the first group of lithium nickel cobalt manganese oxide ternary materials is Li. n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.15≤y1≤0.60, the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2O2, x2+y2+z2+m2=1, satisfying 0<y2≤0.14, preferably 0.15≤y1≤0.50, 0.02≤y2≤0.10. For example, y1 can be 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60 or any range of any two of the above values, and y2 can be 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14 or any range of any two of the above values.

[0025] The inventors discovered that when lithium nickel cobalt manganese oxide (LCO) ternary materials are used as positive electrode active materials, they quickly reach the discharge cutoff voltage (3.0V) under low-temperature, low-SOC discharge conditions, resulting in a significant deterioration in low-temperature, low-SOC discharge performance, which fails to meet the requirements of practical product applications. While lithium cobalt oxide is commonly used as a substitute for LCO to achieve satisfactory discharge performance under low-temperature, low-SOC conditions, it requires the use of cobalt metal resources, which are relatively scarce, leading to higher costs and hindering cost reduction. When the cobalt content in the LCO ternary material is high (e.g., 0.15≤y≤0.60), the discharge voltage is lower and the discharge curve is flatter; conversely, when the cobalt content is low (e.g., 0<y≤0.14), the discharge voltage is higher and the slope of the discharge curve is steeper. Mixing two or more LCO ternary materials that meet these ranges can simultaneously achieve both high discharge voltage and a flat discharge curve, thereby improving low-temperature discharge capability. Increasing the cobalt content in ternary materials can reduce the impedance of electrochemical devices and lower the discharge voltage plateau. Lower impedance helps extend the low-temperature discharge time of electrochemical devices, but lower discharge voltage shortens the low-temperature discharge time of batteries. Therefore, by using two or more nickel-cobalt-manganese lithium ternary materials with different cobalt contents, the discharge performance of electrochemical devices under low temperature and low SOC conditions can be improved.

[0026] Based on the total mass of the lithium nickel cobalt manganese oxide ternary material, the mass percentage of the first group of lithium nickel cobalt manganese oxide ternary material is 'a', and the mass percentage of the second group of lithium nickel cobalt manganese oxide ternary material is 'b', where 10%≤a≤80%, 20%≤b≤90%, preferably 30%≤a≤60%, 40%≤b≤70%, and more preferably 40%≤a≤60%, 40%≤b≤60%. For example, 'a' can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or a range of any two of the above values, and 'b' can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, or a range of any two of the above values. When two or more lithium nickel cobalt manganese oxide (LCO) ternary materials are mixed, if the mass percentages (a and b) of the two LCO ternary materials with higher and lower cobalt contents based on the total mass of the positive electrode active material are appropriately valued (e.g., a=80%, b=20%), the mixed LCO ternary material can exhibit both a high discharge voltage and a relatively smooth discharge curve. Therefore, by controlling the type and content of LCO ternary materials within the aforementioned range, the discharge performance of the electrochemical device under low temperature and low state of charge (SOC) conditions can be improved.

[0027] In one embodiment of this application, the lithium nickel cobalt manganese oxide ternary material may include doping or coating elements, and the materials M1 and M2 are each independently selected from at least one of Ag, Sn, Zn, Al, Mo, Cu, B, Ti, and Fe. Adding the above-mentioned doping or coating elements to the positive electrode active material can make the conductive network on the surface of the positive electrode active material particles more compact, improving the kinetic performance of the electrochemical device; on the other hand, it can reduce the specific surface area of ​​the positive electrode active material, reducing side reactions between the positive electrode active material and the electrolyte; furthermore, it facilitates the formation of a passivation film on the surface of the positive electrode active material particles, improving the initial efficiency and reversible capacity of the electrochemical device. It should be noted that Li... n1 Ni x1 Co y1 Mn z1 M1 m1 O2 and Li n2 Ni x2 Co y2 Mn z2 M2 m2 In O2, m1 and m2 can be 0, meaning that nickel-cobalt-manganese ternary materials may not include doped or coated elements.

[0028] In one embodiment of this application, the particle size of the first group of lithium nickel cobalt manganese oxide ternary materials is D. V1 50, 1μm≤DV1 50≤10μm, preferably, 2μm≤D V1 50≤9μm, for example, D V1 50 can be 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, 10μm, or a range of any two of the above values. The particle size of the second group of lithium nickel cobalt manganese oxide ternary materials is D. V2 50, 1μm≤D V2 50≤15μm, preferably, 2μm≤D V2 50≤10μm, for example, D V2 The particle size 50 can be 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm, 15 μm, or a range of any two of the above values. The particle size of lithium nickel cobalt manganese oxide ternary materials affects the lithium-ion transport distance during battery charging and discharging, thus affecting the discharge time at low temperatures. By controlling the particle size of lithium nickel cobalt manganese oxide materials within the range of this application, the lithium-ion transport distance during the charging and discharging of the electrochemical device can be improved, thereby extending the discharge time of the electrochemical device in low-temperature environments.

[0029] In one embodiment of this application, the first group of lithium nickel cobalt manganese oxide ternary materials has the chemical formula Li n1 Ni x1 Co y1 Mn z1 M1 m1 O2, where 0.95≤n1≤1.05, 0.3≤x1≤0.84, 0.01≤z1≤0.7, 0≤m1≤0.2; the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, wherein 0.95≤n2≤1.05, 0.3≤x2≤0.9, 0.01≤z2≤0.7, 0≤m2≤0.2. By selecting the above-mentioned nickel-cobalt-manganese ternary materials, the discharge performance of the electrochemical device under low temperature and low SOC conditions can be improved.

[0030] In one embodiment of this application, the positive electrode active material includes two ternary nickel-cobalt-manganese oxide lithium materials, grouped according to the cobalt content y, into NCM-1 and NCM-2. NCM-1 satisfies: 0.15 ≤ y1 ≤ 0.60. For example, y1 can be 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or a range of any two of the above values. NCM-2 satisfies: 0 < y2 ≤ 0. 14. For example, y2 can be 0.02, 0.04, 0.06, 0.08, 0.10, 0.12, 0.14 or any two of the above values. By adjusting the cobalt content y1 and y2 of the two nickel cobalt manganese ternary materials within the scope of this application, it is preferred to use two nickel cobalt manganese ternary materials. This can reduce the impedance of the electrochemical device while increasing the discharge voltage platform of the electrochemical device, thereby improving the discharge capability of the electrochemical device in a low-temperature environment and simplifying the production process.

[0031] In this application, there are no particular limitations on the preparation method of the lithium nickel cobalt manganese oxide ternary material, as long as it can achieve the purpose of this invention. For example, the following methods can be used for preparation:

[0032] Ni, Co, and Mn nitrates, sulfates, or chlorides are co-precipitated in the presence of ammonia or ammonium bicarbonate complexing agents to prepare NCM carbonate or hydroxide precursors. The precursors are then sintered with lithium hydroxide or lithium carbonate at 700℃~1000℃ to obtain lithium nickel cobalt manganese oxide ternary materials.

[0033] In this application, the positive electrode material layer further includes a conductive agent and a binder. The conductive agent is selected from at least one of conductive carbon black and carbon nanotubes. Exemplarily, the conductive carbon black may include, but is not limited to, at least one of acetylene black or Ketjen black, and the carbon nanotubes may include, but are not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The binder is selected from at least one of polyacrylate, polyimide, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene-butadiene copolymer, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, sodium carboxymethyl cellulose, and potassium carboxymethyl cellulose.

[0034] In one embodiment of this application, based on the mass of the positive electrode material layer, the mass percentage content of the conductive agent is 1% to 8%. Exemplarily, the mass percentage content of the conductive agent can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, or any range of two of the above values. The mass percentage content of the binder is 1% to 3%. Exemplarily, the mass percentage content of the binder can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, or any range of two of the above values. By controlling the type and content of the conductive agent and binder within the above ranges, the discharge performance of the electrochemical device under low temperature and low SOC conditions can be improved.

[0035] The positive electrode sheet of this application also includes a positive current collector. This application does not have any particular restrictions on the positive current collector, as long as it can achieve the purpose of this application. For example, it may include aluminum foil, aluminum alloy foil or composite current collector (such as aluminum-carbon composite current collector), etc.

[0036] This application does not impose any particular limitations on the thickness of the positive electrode current collector and the positive electrode material layer, as long as the purpose of this application can be achieved. For example, the thickness of the positive electrode current collector can be 5 μm to 20 μm, and the thickness of the positive electrode material layer can be 30 μm to 120 μm.

[0037] In this application, the electrochemical device further includes a negative electrode sheet, which comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector. The phrase "the negative electrode material layer is disposed on at least one surface of the negative electrode current collector" means that the negative electrode material layer can be disposed on one surface of the negative electrode current collector along its thickness direction, or on two surfaces of the negative electrode current collector along its thickness direction. It should be noted that the term "surface" here can refer to the entire surface area of ​​the negative electrode current collector, or only a portion thereof; this application does not impose any particular limitation, as long as the purpose of this application is achieved.

[0038] This application does not impose any particular restrictions on the negative electrode current collector, as long as it can achieve the purpose of this application. For example, it may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or composite current collector. For example, the composite current collector may be lithium copper composite current collector, carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector, etc.

[0039] The negative electrode material layer includes a negative electrode active material. This application does not impose any particular limitation on the negative electrode active material, as long as it can achieve the purpose of this application. For example, the negative electrode active material may include, but is not limited to, natural graphite, artificial graphite, mesophase micro carbon spheres, hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, and spinel-structured lithiated TiO2-Li4Ti5O. 12 Or at least one of Li-Al alloys.

[0040] In some embodiments of this application, the negative electrode material layer may further include a conductive agent and a binder. This application does not impose any particular restrictions on the types of conductive agents and binders, as long as they achieve the purpose of this application. For example, it may be at least one of the aforementioned conductive agents and binders. This application does not impose any particular restrictions on the mass ratio of the negative electrode active material, conductive agent, and binder in the negative electrode material layer. Those skilled in the art can select according to actual needs, as long as the purpose of this application is achieved.

[0041] This application does not impose any particular limitation on the thickness of the negative electrode material layer, as long as it can achieve the purpose of this application. For example, the thickness of the negative electrode material layer is 30 μm to 120 μm.

[0042] This application does not impose any particular limitation on the thickness of the negative electrode current collector, as long as it can achieve the purpose of this application. For example, the thickness of the negative electrode current collector is 4 μm to 15 μm.

[0043] Optionally, the negative electrode sheet may further include a conductive layer located between the negative electrode current collector and the negative electrode material layer. This application does not impose any particular limitation on the composition of the conductive layer, which can be a conductive layer commonly used in the art. For example, the conductive layer may include a conductive agent and a binder. This application does not impose any particular limitation on the conductive agent and binder in the conductive layer; for example, it can be at least one of the aforementioned conductive agents and binders.

[0044] In this application, the electrochemical device also includes a diaphragm. This application does not impose any particular limitation on the diaphragm, as long as it achieves the purpose of this application. For example, the diaphragm material may include, but is not limited to, at least one of polyethylene (PE), polyolefins (PO) primarily composed of polypropylene (PP), polyester (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex, or aramid. The type of diaphragm may include at least one of woven membrane, nonwoven membrane, microporous membrane, composite membrane, rolled membrane, or spun membrane.

[0045] In some embodiments of this application, the diaphragm may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, membrane, or composite membrane with a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate, or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane may be used.

[0046] Optionally, a surface treatment layer is provided on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing polymers and inorganic substances.

[0047] In some embodiments of this application, the inorganic layer comprises inorganic particles and a binder. This application does not particularly limit the inorganic particles; for example, the inorganic particles may include at least one selected from alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. This application does not particularly limit the binder; for example, the binder may be at least one of the binders described above. In some embodiments of this application, the polymer layer comprises a polymer, the polymer material of which includes at least one selected from polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, or polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene).

[0048] In this application, there is no particular limitation on the thickness of the diaphragm, as long as it can achieve the purpose of this application. For example, the thickness of the diaphragm can be from 3 μm to 30 μm.

[0049] A second aspect of this application provides a method for preparing the electrochemical device in any of the foregoing embodiments, comprising:

[0050] Preparation of positive electrode sheet: Two or more lithium nickel cobalt manganese oxide ternary materials are mixed to obtain positive electrode active material; wherein, the two or more lithium nickel cobalt manganese oxide ternary materials used are divided into two groups, and the chemical formula of the first group of lithium nickel cobalt manganese oxide ternary materials is Li n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.15≤y1≤0.60, the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2O2, x2+y2+z2+m2=1, satisfying 0<y2≤0.14; the positive electrode active material is disposed on at least one surface in the thickness direction of the positive electrode current collector to obtain the positive electrode sheet.

[0051] A third aspect of this application provides an electronic device that includes the electrochemical device in any of the foregoing embodiments. The electronic device provided by this application has good performance. This application does not particularly limit the type of electronic device, which can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, laptops, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, household large-capacity batteries, and lithium-ion capacitors, etc.

[0052] Example

[0053] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.

[0054] Test methods and equipment:

[0055] Cobalt content test:

[0056] Using scanning electron microscopy (SEM), NCM material particles were selected, and elemental analysis was performed on the selected NCM particles using energy dispersive spectroscopy (EDS). It should be noted that the EDS test yields the mass of each element. To obtain the molar mass of each element's atoms, the following formula needs to be used: n' = m' / M', where n' is the molar mass of each element's atoms, m' is the mass of each element measured by EDS, and M' is the molar mass of each element. Therefore, the molar mass of cobalt atoms in the lithium nickel cobalt manganese oxide ternary material is n'(Co) = m'(Co) / M'(Co).

[0057] Testing of the content of each component in the positive electrode active material layer:

[0058] The prepared positive electrode sheet was calcined at 500℃ for 4 hours under oxygen-permeable conditions to remove carbon conductive agent and organic binder components. The powder after high-temperature treatment was evenly dispersed in water, and 1 mL of suspension was dried to prepare a sample. SEM and EDS were used for observation at 1000x magnification. The composition and number of all NCM particles in the random field of view were counted, and the content of each component was counted based on the composition and number of particles.

[0059] Particle size testing:

[0060] The above suspension was dried and sampled. When observed using SEM and EDS, in addition to counting the composition and number of particles, the particle size was also counted to obtain the Dv50 of different components.

[0061] Low-temperature discharge performance test

[0062] The battery was subjected to a low temperature and low SOC discharge test: the battery was discharged to 3.0V at a discharge rate of 0.2C, and then charged at a rate of 0.2C for 0.5H. The battery was placed at a low temperature of 0℃ and discharged at a rate of 1C and 0.5C respectively. The duration of discharge to 3.0V was recorded.

[0063] Example 1-1

[0064] <Preparation of the positive electrode>

[0065] LiNi with a mass ratio of 1:1 0.5 Co 0.4 Mn 0.09 Al 0.01 O2 and LiNi 0.5 Co 0.05 Mn 0.44 Al 0.01 O2 was mixed with conductive carbon black (Super P), CNTs, and polyvinylidene fluoride (PVDF) in a weight ratio of 96.5:1.0:1.0:1.5. N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 75 wt%, and the mixture was stirred until homogeneous to obtain the positive electrode slurry. The positive electrode slurry was then uniformly coated onto one surface of a 10 μm thick aluminum foil used as the positive electrode current collector. The coating weight of the positive electrode active material layer on the positive electrode sheet was 180 g / m². 2 The aluminum foil was dried at 90℃ to obtain a positive electrode sheet with a single-sided coating of positive active material. The above steps were then repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of positive active material. After coating, the positive electrode sheet was cold-pressed to a compaction density of 4.1 g / cm³. 3 After cutting and welding the tabs, a positive electrode sheet with a size of 74mm×867mm is obtained for later use.

[0066] <Preparation of Negative Electrode Sheets>

[0067] Artificial graphite, conductive carbon black (Super P), and polyacrylic acid, the negative electrode active materials, were mixed in a weight ratio of 97.3:1.5:1.2. Deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 70wt%, and the mixture was stirred evenly to obtain the negative electrode slurry. The negative electrode slurry was uniformly coated on one surface of a 10μm thick copper foil for the negative electrode current collector. The coating weight of the negative electrode active material layer on the negative electrode sheet was 95g / m². 2 The copper foil was dried at 110℃ to obtain a negative electrode sheet with a single-sided coating of the negative electrode active material layer. The above steps were then repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of the negative electrode active material layer. After coating, the negative electrode sheet was cold-pressed to a compaction density of 1.7 g / cm³. 3 After cutting and welding the tabs, a negative electrode sheet with dimensions of 78mm × 875mm is obtained for later use. The artificial graphite used as the negative electrode active material has a Dv50 of 10μm and a specific surface area of ​​1.6m² achieved by adjusting the ball milling time. 2 / g.

[0068] <Preparation of Electrolyte>

[0069] In an argon-atmospheric glove box with a water content of less than 10 ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed uniformly at a mass ratio of EC:EMC:DEC = 3:5:2 to obtain a base solvent. Then, lithium hexafluorophosphate (LiPF6) was added to the base solvent and mixed uniformly to obtain an electrolyte. The lithium salt content was 12.5% ​​by mass, with the remainder being the base solvent.

[0070] <Septum>

[0071] A polyethylene film with a thickness of 9μm was selected as the diaphragm.

[0072] <Preparation of Lithium-ion Batteries>

[0073] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. The electrode assembly is then wound up. The electrode assembly is placed in an outer packaging foil and then injected with the prepared electrolyte. After formation, degassing, and edge trimming, a lithium-ion battery is obtained.

[0074] Examples 1-2 to 1-32

[0075] Except for changing the preparation parameters according to Table 1, the rest is the same as in Example 1-1.

[0076] Examples 1-33

[0077] LiNi with a mass ratio of 25%:25%:50% 0.5 Co 0.4 Mn 0.09 Al 0.01 O2, LiNi 0.4 Co 0.5 Mn 0.09 Al 0.01 O2 and LiNi 0.5 Co 0.05 Mn 0.44 Al 0.01 O2 was mixed with conductive carbon black (Super P), CNTs, and polyvinylidene fluoride (PVDF) in a weight ratio of 96.5:1.0:1.0:1.5. N-methylpyrrolidone (NMP) was then added as a solvent to prepare a slurry with a solid content of 75 wt%, which was stirred until homogeneous to obtain the positive electrode slurry. The positive electrode slurry was then uniformly coated onto one surface of a 10 μm thick aluminum foil used as the positive electrode current collector. The coating weight of the positive electrode active material layer on the positive electrode sheet was 180 g / m². 2 The electrode was dried at 90°C to obtain a positive electrode sheet with a single-sided coating of positive active material. The rest of the process was the same as in Example 1-1, and low-temperature discharge performance testing was performed.

[0078] Examples 1-34

[0079] LiNi with a mass ratio of 50%:25%:25% 0.5 Co 0.4 Mn 0.09 Al 0.01 O2, LiNi 0.5 Co 0.05 Mn 0.44 Al 0.01 O2 and LiNi 0.5 Co 0.1 Mn 0.39 Al 0.01 O2 was mixed with conductive carbon black (Super P), CNTs, and polyvinylidene fluoride (PVDF) in a weight ratio of 96.5:1.0:1.0:1.5. N-methylpyrrolidone (NMP) was then added as a solvent to prepare a slurry with a solid content of 75 wt%, which was stirred until homogeneous to obtain the positive electrode slurry. The positive electrode slurry was then uniformly coated onto one surface of a 10 μm thick aluminum foil used as the positive electrode current collector. The coating weight of the positive electrode active material layer on the positive electrode sheet was 180 g / m². 2 The electrode was dried at 90°C to obtain a positive electrode sheet with a single-sided coating of positive active material. The rest of the process was the same as in Example 1-1, and low-temperature discharge performance testing was performed.

[0080] Examples 1-35

[0081] LiNi with a mass ratio of 25%:25%:25%:25% 0.5 Co 0.4 Mn 0.09 Al 0.01 O2, LiNi 0.5 Co 0.05 Mn 0.44 Al 0.01 O2, LiNi 0.4 Co 0.5 Mn 0.09 Al 0.01 O2 and LiNi 0.5 Co 0.1 Mn 0.39 Al 0.01 O2 was mixed with conductive carbon black (Super P), CNTs, and polyvinylidene fluoride (PVDF) in a weight ratio of 96.5:1.0:1.0:1.5. N-methylpyrrolidone (NMP) was then added as a solvent to prepare a slurry with a solid content of 75 wt%, which was stirred until homogeneous to obtain the positive electrode slurry. The positive electrode slurry was then uniformly coated onto one surface of a 10 μm thick aluminum foil used as the positive electrode current collector. The coating weight of the positive electrode active material layer on the positive electrode sheet was 180 g / m². 2 The electrode was dried at 90°C to obtain a positive electrode sheet with a single-sided coating of positive active material. The rest of the process was the same as in Example 1-1, and low-temperature discharge performance testing was performed.

[0082] Comparative Example 1

[0083] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as in Example 1-1.

[0084] Table 1

[0085] Table 2

[0086] As can be seen from Examples 1-1 to 1-11 and Comparative Example 1, by adjusting the cobalt content y1 and y2 in the two sets of lithium nickel cobalt manganese oxide ternary materials within the scope of this application, the discharge time of the secondary battery at 0°C and discharge rates of 1C and 0.5C was improved, indicating that the discharge performance of the lithium-ion battery at low temperature and low SOC was improved. Based on the discharge times of Examples 1-1 to 1-11 at 0°C and discharge rates of 1C and 0.5C, it can be concluded that the cobalt content y1 and y2 have a preferred range.

[0087] Based on the total mass of the positive electrode active material, the mass percentage of the two sets of lithium nickel cobalt manganese oxide ternary materials affects the low-temperature discharge performance of the secondary battery. As can be seen from Examples 1-1, 1-12 to 1-16 and Examples 1-31 and 1-32, by adjusting the mass percentages a and b of the two sets of lithium nickel cobalt manganese oxide ternary materials to satisfy: 10%≤a≤80% and 20%≤b≤90%, the discharge time of the secondary battery at 0℃ low temperature conditions at 1C and 0.5C rates is improved, thus indicating that the discharge performance of lithium-ion batteries at low temperature and low SOC conditions is improved. Based on the discharge times of Examples 1-1, 1-12 to 1-16, and 1-31 and 1-32 under 0°C low-temperature conditions at discharge rates of 1C and 0.5C, it can be concluded that the mass percentages a and b of the lithium nickel cobalt manganese oxide ternary material show a trend of first increasing and then decreasing with the increase of a. This indicates that the mass percentages a and b of the lithium nickel cobalt manganese oxide ternary material have a preferred range: 30% ≤ a ≤ 60%, 40% ≤ b ≤ 70%. Furthermore, a and b have a more preferred range: 40% ≤ a ≤ 60%, 40% ≤ b ≤ 60%.

[0088] The particle size of the two sets of lithium nickel cobalt manganese oxide ternary materials affects the low-temperature discharge performance of the secondary battery. As can be seen from Examples 1-1, 1-17 to 1-28 and Comparative Example 1, the low-temperature discharge performance of the secondary battery can be affected by adjusting the particle size D of the two sets of lithium nickel cobalt manganese oxide ternary materials. V1 50 and D V2 50. Within the scope of this application, the discharge time of the secondary battery at 0°C and discharge rates of 1C and 0.5C is improved, indicating that the discharge performance of the lithium-ion battery at low temperature and low SOC is improved. From the discharge times of Examples 1-1, 1-17 to 1-28 at 0°C and discharge rates of 1C and 0.5C, it can be concluded that the particle size D of the lithium nickel cobalt manganese oxide ternary material... V1 50 has a significant impact on discharge time, D V2 The influence of 50 is relatively small, which indicates that the particle size of the cobalt-manganese ternary material has an optimal range.

[0089] The content of conductive agent affects the low-temperature discharge performance of secondary batteries. As can be seen from Examples 1-1, 1-29, 1-30 and Comparative Example 1, by adjusting the content of conductive agent within the scope of this application, the discharge time of secondary batteries at 0°C low temperature conditions at 1C and 0.5C rates is improved, thus indicating that the discharge performance of lithium-ion batteries at low temperature and low SOC is improved.

[0090] Table 2 shows the secondary batteries made by mixing two or more lithium nickel cobalt manganese oxide ternary materials. As can be seen from Examples 1-1, 1-33 to 1-35 and Comparative Example 1, by adjusting the types and contents of two or more lithium nickel cobalt manganese oxide ternary materials within the scope of this application, the discharge time of the secondary battery at 0°C low temperature conditions at 1C and 0.5C rates is improved. Comparing Examples 1-33 with Example 1-1, Example 1-33 added a set of ternary materials with high cobalt content (0.15≤y≤0.60). The increased cobalt content lowered the discharge voltage plateau and improved the material impedance, resulting in improved discharge performance. Comparing Examples 1-34 with Example 1-1, Example 1-34 added a set of ternary materials with low cobalt content (0<y≤0.14), which lowered the discharge voltage, but had a smaller improvement on the material impedance, thus having a certain impact on discharge performance. Comparing Examples 1-35 with Example 1-1, Example 1-35 added both a set of ternary materials with high cobalt content and a set with low cobalt content. The increased cobalt content lowered the discharge voltage plateau and improved the material impedance, thereby improving discharge performance.

[0091] It should be noted that, in this document, the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0092] The various embodiments in this specification are described in a related manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.

[0093] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.

Claims

1. An electrochemical device comprising a positive electrode, said positive electrode comprising a positive electrode material layer, said positive electrode material layer comprising a positive electrode active material, wherein, The positive electrode active material comprises two or more than two lithium nickel cobalt manganese ternary materials; the two or more than two lithium nickel cobalt manganese ternary materials are divided into two groups, the chemical formula of the first group of lithium nickel cobalt manganese ternary materials is Li n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, 0.33<=x1<=0.5, 0.15<=y1<=0.60, the chemical formula of the second group of lithium nickel cobalt manganese ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, x2+y2+z2+m2=1, x2=0.5, 0 2. The electrochemical device according to claim 1, wherein, Based on the total mass of the lithium nickel cobalt manganese oxide ternary materials, the mass percentage of the first group of lithium nickel cobalt manganese oxide ternary materials is a, and the mass percentage of the second group of lithium nickel cobalt manganese oxide ternary materials is b, where 10%≤a≤80% and 20%≤b≤90%.

3. The electrochemical device according to claim 1, wherein, The materials of M1 and M2 are each independently selected from at least one of Ag, Sn, Zn, Al, Mo, Cu, B, Ti and Fe.

4. The electrochemical device according to claim 2, wherein, 30%≤a≤60%, 40%≤b≤70%.

5. The electrochemical device according to claim 4, wherein, 40%≤a≤60%, 40%≤b≤60%.

6. The electrochemical device according to claim 1, wherein, 0.15≤y1≤0.50, 0.02≤y2≤0.

10.

7. The electrochemical device according to claim 1, wherein, The particle size of the first group of lithium nickel cobalt manganese oxide ternary materials is D. V1 50, 1μm≤D V1 50≤10μm.

8. The electrochemical device according to claim 7, wherein, 2μm≤D V1 50≤9μm。 9. The electrochemical device according to claim 1, wherein, The particle size of the second group of lithium nickel cobalt manganese oxide ternary materials is D. V2 50, 1μm≤D V2 50≤15μm.

10. The electrochemical device according to claim 9, wherein, 2μm≤D V2 50≤10μm。 11. The electrochemical device according to claim 1, wherein, 0.95≤n1≤1.05, 0.01≤z1≤0.7, 0≤m1≤0.2; 0.95≤n2≤1.05, 0.01≤z2≤0.7, 0≤m2≤0.

2.

12. The electrochemical device according to claim 1, wherein, The positive electrode active material includes two ternary materials, NCM-1 and NCM-2, of lithium nickel cobalt manganese oxide. NCM-1 satisfies: 0.15≤y1≤0.60, and NCM-2 satisfies: 0<y2≤0.

14.

13. The electrochemical device according to any one of claims 1 to 12, wherein, The positive electrode material layer further includes a conductive agent and a binder. The conductive agent is selected from at least one of conductive carbon black and carbon nanotubes. The binder is selected from at least one of polyacrylate, polyimide, polyamide, polyamide-imide, polyvinylidene fluoride, polystyrene-butadiene copolymer, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, sodium hydroxymethyl cellulose, and potassium hydroxymethyl cellulose.

14. The electrochemical device according to claim 13, wherein, Based on the mass of the positive electrode material layer, the mass percentage of the conductive agent is 1% to 8%, and the mass percentage of the binder is 1% to 3%.

15. A method for preparing an electrochemical device as described in any one of claims 1 to 14, comprising: Preparation of the positive electrode sheet: The two or more lithium nickel cobalt manganese oxide ternary materials are mixed to obtain the positive electrode active material; wherein the two or more lithium nickel cobalt manganese oxide ternary materials used are divided into two groups, and the first group of lithium nickel cobalt manganese oxide ternary materials has the chemical formula Li. n1 Ni x1 Co y1 Mn z1 M1 m1 O2, x1+y1+z1+m1=1, satisfying 0.33≤x1≤0.5, 0.15≤y1≤0.60, the chemical formula of the second group of lithium nickel cobalt manganese oxide ternary materials is Li n2 Ni x2 Co y2 Mn z2 M2 m2 O2, x2+y2+z2+m2=1, satisfying x2=0.5, 0<y2≤0.14; the positive electrode active material is disposed on at least one surface in the thickness direction of the positive electrode current collector to obtain a positive electrode sheet.

16. An electronic device comprising the electrochemical device according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Fully-sealed Li-ion storage battery based on ternary cathode material and preparation method of fully-sealed Li-ion storage battery

    CN105336942A

  • Positive pole piece and preparation method thereof and lithium ion secondary battery

    CN111640912A