Preparation method and application process of multi-material wooden barrel for brewing wine
By using a multi-material wooden barrel preparation method, gradient particle size crushing and functionalization treatment, combined with microwave activation and stamping, the problems of traditional wooden barrels such as single flavor, low process efficiency and poor stability are solved, achieving flavor diversity and structural stability, and reducing production costs.
Patent Information
- Application Number
- CN202510615059.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-05-14
AI Technical Summary
Existing brewing barrels have limited flavor profiles, complex processes, and high costs. They also lack sufficient sealing and durability, making it impossible to effectively control the release rate and synergistic effects of flavor compounds.
The preparation method of multi-material wooden barrels is adopted. Oak, cherry and chestnut wood are crushed by gradient particle size, combined with microwave treatment, nitrogen protection, microwave activation, stamping and molding and functional adhesive design to form a dense and breathable composite structure. Combined with nano magnetic powder and β-glucan slow release network, flavor diversity and structural stability are achieved.
It enhances the flavor profile and release control of the barrels, improves their compressive strength and leakage rate, shortens the aging period, reduces production costs, and meets food safety and environmental protection standards.
Smart Images

Figure CN120481015B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of food brewing technology, and in particular to a method for preparing and applying a multi-material wooden barrel for brewing. Background Technology
[0002] In the winemaking process, wooden barrels, as traditional aging containers, play an irreplaceable role in the formation of flavor and the enhancement of quality. Currently, most commercially available winemaking barrels are made from a single type of wood (such as oak). Through the slow interaction between the natural components of the wood (such as tannins and lignin derivatives) and the wine, specific aromas and flavors are imparted to the spirit. However, the limitations of single-wood barrels are becoming increasingly apparent: firstly, the flavor profile is limited, making it difficult to satisfy consumers' pursuit of complex tastes; secondly, traditional barrels rely on handcrafting, which is cumbersome and costly, making large-scale production difficult; thirdly, the barrels lack sufficient sealing and durability, making them prone to leakage or microbial contamination, affecting product stability. Furthermore, existing technologies lack systematic research on wood pretreatment and functional modification, making it impossible to effectively control the release rate and synergistic effects of flavor compounds.
[0003] To address the aforementioned issues, there is an urgent need for a novel method for preparing wooden barrels that combines flavor diversity, high process efficiency, and structural stability, while ensuring the environmental friendliness of the production process and the safety of the wine. This invention, through innovative material selection, synergistic pretreatment processes, and functional design, effectively overcomes the bottlenecks of traditional technologies, providing technical support for quality upgrading in the brewing industry. Summary of the Invention
[0004] In view of this, the present invention proposes a novel stamping preparation method and application process for multi-material wooden barrels, which effectively combines the unique flavors of different woods and improves the quality of aged products.
[0005] The technical solution of this invention is achieved as follows: This invention provides a method for preparing a multi-material wooden barrel for brewing, comprising the following steps:
[0006] Step 1: Crush oak, cherry wood and chestnut wood separately to obtain oak with an average particle size of 3-5mm, cherry wood with an average particle size of 2-3mm and chestnut wood with an average particle size of 1-2mm;
[0007] Step 2: Mix oak, cherry and chestnut wood particles in a weight ratio of (5-7):(2-3):(1-2). Microwave the mixed wood under a nitrogen atmosphere for 5-10 minutes at a microwave power of 800W. Then add natural plant binder, which accounts for 5-10% of the mixed wood.
[0008] Step 3: Press the mixture from Step 2 into a barrel shape using a stamping press with a pressure of 200-350 tons;
[0009] Step 4: Heat the formed barrel-shaped structure to 50-80℃ and keep it warm for 6-12 hours to obtain a multi-material wooden barrel for brewing.
[0010] The technical solution of this invention enhances the function of brewing barrels through the synergistic treatment and structural optimization of multiple types of wood. Its core principle is as follows: First, oak, cherry, and chestnut are pulverized into gradient particle sizes of 3-5mm, 2-3mm, and 1-2mm, respectively, forming a dense and breathable composite substrate through physical gradation. Second, microwave treatment under nitrogen protection eliminates volatile impurities in the wood while activating surface hydroxyl groups, enhancing the bonding force with natural adhesives. Subsequently, high-pressure stamping at 200-350 tons is used to form a seamless barrel structure, utilizing the elastic deformation of wood fibers and the penetration and curing of the adhesive. Finally, a heat treatment at 50-80℃ promotes the cross-linking and curing of the adhesive, forming a composite coating that combines mechanical strength and slow-release function. The tannins of oak, the fruity aroma of cherry, and the sweetness of chestnut are released in stages through the particle size gradient, increasing flavor complexity. The stamping process improves production efficiency and reduces costs, while microwave treatment activates surface hydroxyl groups and removes volatile impurities.
[0011] In some embodiments, the oak is softened by steam treatment before pulverization, with the steam treatment temperature being 100-120°C and the treatment time being 2-4 hours.
[0012] Steam softening treatment of oak involves high-temperature steam penetrating the wood fibers, reducing the rigidity of lignin and partially degrading hemicellulose, thereby improving the wood's plasticity. Softened oak is more likely to form uniform particles during pulverization, while reducing internal stress concentration caused by fiber breakage, enhancing the structural stability of subsequent stamping. Softened oak particles bind more tightly with cherry and chestnut wood particles during stamping, reducing the release rate of oak tannins and preventing excessive astringency in the initial taste of the wine, resulting in a smoother flavor. Steam treatment removes some volatile impurities from the oak, reducing negative flavor interference in the wine. The increased porosity of softened oak allows for a more complete interaction with the fruity aromas of cherry and the sweetness of chestnut, leading to improved sensory evaluation scores.
[0013] In some embodiments, the cherry wood is soaked in a lactic acid bacteria fermentation liquid with a pH of 4.5-5.5 before being crushed, and the soaking time is 24-48 hours.
[0014] Cherry wood is treated with lactic acid bacteria fermentation broth. Through the metabolic activity of lactic acid bacteria, lignin and hemicellulose in the wood are degraded, releasing fruit aroma precursors and generating organic acids such as lactic acid to regulate the wood's microenvironment. The acidic conditions inhibit the growth of unwanted microorganisms while promoting the hydrolysis of fruit aroma components in the cherry wood, forming soluble flavor compounds. After fermentation, the content of fruit aroma compounds (esters and aldehydes) in the cherry wood increases, giving the wine a more pronounced cherry and almond flavor. Lactic acid produced by lactic acid bacteria metabolism reacts with ethanol in the wine through esterification, generating aromatic esters such as ethyl acetate, improving sensory evaluation scores. Partial degradation of lignin increases the porosity of cherry wood particles, expanding the bonding area with oak and chestnut wood particles, thus improving the barrel's compressive strength. Fermentation treatment reduces the wood's hardness, minimizing internal stress cracks during stamping and reducing leakage.
[0015] In some embodiments, the chestnut wood is ultrasonically treated before being crushed, with an ultrasonic frequency of 40-60 kHz and an ultrasonic time of 1-2 hours.
[0016] Ultrasonic treatment of chestnut wood utilizes the cavitation effect and mechanical vibration of ultrasound to disrupt the cell wall structure, increase porosity, and release internally bound polysaccharides, phenols, and other flavor compounds. High-frequency vibration precisely targets weak areas of the chestnut wood fibers, avoiding damage to the overall structure, while simultaneously promoting the penetration of subsequent adhesives and the uniform bonding of wood powder particles. After ultrasonic treatment, the dissolution of sweet substances in chestnut wood increases, imparting a more pronounced sweetness to the wine. Increased porosity enhances the interaction area between the wine and the wood, shortening the flavor transfer cycle. Ultrasonic pretreatment also reduces the hardness of chestnut wood, improves particle uniformity after crushing, results in tighter wood powder bonding during molding, and increases the compressive strength of the barrels.
[0017] In some embodiments, the natural plant adhesive is a mixture of modified gum arabic and lignin, wherein the mass ratio of gum arabic to lignin is (6-8):(2-4).
[0018] A mixture of modified gum arabic and lignin is used as a natural plant-based binder, achieving a balance between adhesive strength and flavor compatibility through the complementary functions of the two. Modified gum arabic: Carboxymethylation introduces hydrophilic groups, enhancing wettability and dispersibility with wood particles; lignin: As a natural hydrophobic component, it provides water resistance and mechanical support, reducing binder swelling caused by wine penetration. The film-forming properties of gum arabic delay the rapid release of flavor compounds, reducing tannin dissolution in the early stages of barrel aging; the phenolic compounds in lignin undergo slow esterification with alcohols in the wine, generating additional flavor components such as vanillin, thus increasing the complexity score in sensory evaluation.
[0019] Methods for preparing modified gum arabic include:
[0020] Gum arabic raw material is pulverized to a particle size of 50-100 μm. A 60-80% volume concentration isopropanol solution is used as the dispersion medium to adjust the gum arabic to a latex concentration of 20-30 wt%. Sodium hydroxide solution (40-50% concentration) is added, at a volume of 100-150% of the gum arabic mass. The mixture is stirred at 25-40℃ for 1-2 hours. Chloroacetic acid is used as the etherifying agent, with a molar ratio of gum arabic:chloroacetic acid = 1:0.8-1.2. The temperature is controlled at 50-70℃, and the reaction time is 3-5 hours. The pH is maintained at 10-12 to promote the carboxymethyl substitution reaction. After the reaction, the pH is adjusted to 6.5-7.5 with glacial acetic acid to terminate the reaction and precipitate the product. The product is washed 3-5 times with 70-85% ethanol to remove unreacted reagents and salts. After vacuum drying at 60-80℃, the product is pulverized and sieved.
[0021] In some embodiments, the natural plant adhesive also includes β-glucan, with the amount of β-glucan added being 1-3% of the total weight of the adhesive.
[0022] Adding β-glucan to natural plant binders allows it to form a complex network with modified gum arabic and lignin through its unique polysaccharide structure. The microporous structure of β-glucan adsorbs flavor molecules, slowing their release rate and preventing initial flavor overload in the wine. The linear chains of β-glucan cross-link with the branched structure of gum arabic, improving the binder's flexibility and reducing brittle cracking during stamping. The strong hydrophilicity of β-glucan maintains a balanced humidity environment within the barrel, reducing the risk of leakage due to wood shrinkage. The slow-release effect of β-glucan results in a higher ester content and more persistent flavor profile in the wine after 6 months of aging compared to the unadded group. The synergistic effect of lignin and β-glucan generates vanillin-like derivatives, improving the sweetness score in sensory evaluation.
[0023] In some embodiments, step two, when mixing wood particles, also includes adding food-grade magnetic powder, the amount of which is 3-6% of the weight of the wood, and the particle size of the food-grade magnetic powder does not exceed 100 nm.
[0024] Nanoparticles create a localized magnetic field within the wooden barrel, accelerating the directional movement of charged particles in the wine, promoting esterification and oxidation reactions, and shortening the aging period. The magnetic field induces the orderly arrangement of wine molecules, reducing the formation of off-flavors and enhancing flavor purity. The high specific surface area of the nanoparticles strengthens interfacial bonding, reducing internal stress cracks during stamping and lowering leakage. Under the magnetic field environment, the ethyl acetate content in the wine increases, resulting in enhanced fruit aroma intensity in sensory evaluation.
[0025] In some embodiments, the food-grade magnetic powder is surface-grafted using a silane coupling agent.
[0026] Silane coupling agents (such as KH-550 or KH-560) generate silanol groups (Si-OH) through hydrolysis, which form covalent bonds with hydroxyl groups (Fe-OH or rare earth oxide-OH) on the magnetic powder surface, while simultaneously introducing organic functional groups such as amino or epoxy groups onto the magnetic powder surface. The grafted organic groups on the magnetic powder surface form hydrogen bonds or covalent bonds with wood particles or adhesives, improving interfacial bonding strength. The silane layer reduces the surface energy of the magnetic powder, inhibiting nanoparticle agglomeration and improving the uniformity of magnetic powder dispersion in the mixture.
[0027] Secondly, the present invention also provides a multi-material wooden barrel for brewing prepared by the above method.
[0028] Thirdly, the present invention also provides an application process for the above-mentioned multi-material wooden barrels for brewing, including: maintaining the internal temperature of the container at 15-20°C and the relative humidity at 70%-80% during the aging process in the multi-material wooden barrels for brewing.
[0029] The present invention has the following advantages over the prior art:
[0030] This invention significantly enhances the flavor complexity and release controllability of wooden barrels through multi-gradient wood particle size ratios, bio-physical synergistic pretreatment, and functionalized adhesive design. Oak tannins, cherry fruit aromas, and chestnut sweetness are released in stages, increasing sensory complexity. Combining high-pressure stamping and nano-magnetic powder reinforcement technology, the barrels achieve increased compressive strength and reduced leakage rate, while the magnetic field response characteristics can dynamically regulate the flavor release rate. In terms of process, microwave activation and nitrogen protection reduce volatile impurities. Combined with food-grade magnetic powder silane modification and β-glucan slow-release network, it has the advantages of improved production efficiency and reduced costs, while meeting food safety and environmental protection standards. It solves the technical bottlenecks of traditional wooden barrels, such as single flavor, inefficient process, and poor stability. Attached Figure Description
[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0032] Figure 1 This is a flowchart of the wooden barrel manufacturing process of the present invention. Detailed Implementation
[0033] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the embodiments of this invention pertain. If any definition stated in this section is contrary to or otherwise inconsistent with a definition stated in a patent, patent application, published patent application, or other publication incorporated herein by reference, the definitions listed here shall prevail over those incorporated herein by reference.
[0035] Unless otherwise specified, the methods used in the following embodiments are conventional methods. Unless otherwise specified, the materials, reagents, and instruments used are conventional materials, reagents, and instruments in the art, and can be obtained commercially by those skilled in the art.
[0036] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1 to 5” is disclosed, the described range should be interpreted as including ranges “1 to 4”, “1 to 3”, “1 to 2”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range. In this specification and claims, range definitions may be combined and / or interchanged, unless otherwise stated, these ranges include all subranges contained therein.
[0037] In the following examples, the method for preparing modified gum arabic is as follows:
[0038] Gum arabic raw material was pulverized to a particle size of 80 μm. A 70% isopropanol solution was used as the dispersion medium to adjust the gum arabic to a latex concentration of 25 wt%. A sodium hydroxide solution (45 wt%) was added, with the amount being 125% of the gum arabic mass. The mixture was stirred at 35°C for 1.5 hours. Chloroacetic acid was used as the etherifying agent, with a molar ratio of gum arabic to chloroacetic acid of 1:1. The temperature was controlled at 60°C, and the reaction time was 4 hours. The pH was maintained at 10-12 to promote the carboxymethyl substitution reaction. After the reaction was completed, the pH was adjusted to 7.0 with glacial acetic acid to terminate the reaction and precipitate the product. The product was washed four times with 75% ethanol to remove unreacted reagents and salts. After vacuum drying at 70°C, the product was pulverized and sieved.
[0039] Example 1
[0040] step:
[0041] 1. Crush oak, cherry, and chestnut wood into average particle sizes of 4mm, 3mm, and 2mm respectively, and mix them in a weight ratio of 6:2.5:1.5;
[0042] 2. The mixed wood was microwaved at 800W for 8 minutes under a nitrogen atmosphere, and then 8wt% of modified gum arabic-lignin binder (mass ratio 7:3) was added.
[0043] 3. The barrel is formed by pressing with 300 tons of pressure, heated to 65℃, and kept warm for 9 hours to obtain a wooden barrel.
[0044] Example 2
[0045] step:
[0046] Oak wood was steam-heated at 110℃ for 3 hours;
[0047] Cherry wood was soaked in a lactic acid bacteria fermentation broth with a pH of 5.0 for 36 hours;
[0048] Chestnut wood was treated with ultrasound at 50 kHz for 1.5 hours;
[0049] The other steps are the same as in Example 1.
[0050] Example 3
[0051] Based on Example 1, 5 wt% of Fe3O4 iron oxide magnetic powder (average particle size 80 nm) was added when mixing the wood particles. Other steps were the same as in Example 1.
[0052] Example 4
[0053] Based on Example 1, 5 wt% of silane-modified Fe3O4 magnetic powder (average particle size 80 nm) was added when mixing wood particles. Other steps were the same as in Example 1. The silane treatment method was as follows: Fe3O4 magnetic powder was ultrasonically dispersed in a 5% KH-550 ethanol solution for 30 min, filtered, and dried at 60°C.
[0054] Example 5
[0055] Based on Example 1, the adhesive also includes 2 wt% β-glucan.
[0056] Example 6
[0057] Based on Example 2, 5 wt% of silane-modified Fe3O4 iron oxide magnetic powder (average particle size 80 nm) was added when mixing wood particles, and 2 wt% of β-glucan was also included in the binder.
[0058] Example 7
[0059] Based on Example 1, oak was steam-heated at 110°C for 3 hours.
[0060] Example 8
[0061] Based on Example 1, cherry wood was soaked in a lactic acid bacteria fermentation broth at pH 5.0 for 36 hours; chestnut wood was treated with ultrasound at 50 kHz for 1.5 hours.
[0062] Comparative Example 1
[0063] Oak barrels are prepared using conventional whole-wood cutting, without crushing, stamping, or functionalization.
[0064] The following items were tested and verified respectively:
[0065] The following are the specific verification methods and operating procedures for each testing item:
[0066] I. Compressive Strength Testing
[0067] Standard basis: GB / T 17657-2013 "Test Methods for Physical and Chemical Properties of Wood-based Panels and Decorative Wood-based Panels"
[0068] Instrumentation: Universal testing machine (range 0-100kN, accuracy ±1%)
[0069] step:
[0070] Sample preparation: Cut the wooden barrel into 50mm×50mm×50mm cube samples, with 5 parallel samples per group;
[0071] Compression test: Apply vertical pressure at a rate of 5 mm / min and record the maximum pressure value (kN) when the specimen fails;
[0072] Calculation: Compressive strength = maximum pressure / cross-sectional area of the specimen (MPa), take the average of 5 times.
[0073] II. Leakage Rate Detection
[0074] Method design: Refer to QB / T 2681-2014 "Test Method for Sealing Performance of Food Containers"
[0075] Instruments and equipment: constant temperature water bath (accuracy ±0.5℃), electronic balance (accuracy 0.01g)
[0076] step:
[0077] Water injection and pressurization: Fill the wooden barrel with distilled water, seal it, and place it in a 25°C environment, applying a static pressure of 0.2 MPa (simulating the long-term storage pressure of the wine);
[0078] Quality monitoring: Weigh the barrel after 24 hours and measure the mass loss (Δm).
[0079] Calculation: Leakage rate = Δm / initial mass × 100%.
[0080] III. Sensory Evaluation
[0081] Standard based on: GB / T 10220-2012 "Sensory Analysis Methodology"
[0082] Review process:
[0083] The judging panel consists of 10 trained sommeliers (5 men and 5 women, aged 25-50).
[0084] Blind tasting design: After the wines are aged in wooden barrels for 6 months, they are randomly numbered and offered to the judges for tasting;
[0085] Rating dimensions (0-10 points):
[0086] Aroma: Fruity, woody, complex;
[0087] Palate: Tannin astringency, sweetness, and lingering finish;
[0088] Data processing: After removing the highest / lowest scores, take the average score and calculate the standard deviation.
[0089] IV. Tannin Release Rate Detection
[0090] Methodology: HPLC (refer to the Journal of Agricultural and Food Chemistry)
[0091] Instrument conditions:
[0092] Chromatograph: Agilent 1260HPLC, C18 column (4.6×250mm, 5μm);
[0093] Mobile phase: acetonitrile-0.1% phosphoric acid aqueous solution (15:85), flow rate 1.0 mL / min;
[0094] Detection wavelength: 280nm.
[0095] step:
[0096] Sample pretreatment: Take 10 mL of wine from the wooden barrel each month and filter it through a 0.45 μm filter membrane;
[0097] Standard curve: A concentration gradient of 0-100 mg / L was established using gallic acid standard;
[0098] Quantitative analysis: Integrate the characteristic peak area of tannins to calculate the concentration (mg / L), and the rate = concentration / time (mg / L·month).
[0099] V. Fruit Aroma Intensity Test (GC-MS)
[0100] Instrument conditions:
[0101] Gas chromatography: Agilent 7890B, HP-5MS capillary column (30m×0.25mm×0.25μm);
[0102] Mass spectrometry: Agilent 5977B, EI ion source, scan range m / z 30-500;
[0103] Temperature program: Hold at 50℃ for 2 minutes, then increase to 250℃ at a rate of 5℃ / min and hold for 5 minutes.
[0104] step:
[0105] Sample extraction: Take 10 mL of wine, add NaCl to saturate, extract 3 times with dichloromethane, combine the organic phases, and concentrate to 1 mL by nitrogen blowing;
[0106] Injection analysis: Injection volume 1 μL, split ratio 10:1;
[0107] Data processing: The total area of the characteristic fruit aroma peaks such as ethyl acetate and benzaldehyde is integrated, and the relative intensity is expressed by the peak area.
[0108] The results are shown in the table below:
[0109]
[0110] The compressive strength of the full pretreatment combination (Example 2) (68 MPa, an increase of 16 MPa compared to Example 1) is significantly higher than the sum of the performance improvements of single pretreatment (Example 7: 53 MPa, an increase of 1 MPa compared to Example 1) and two pretreatments (Example 8: 58 MPa, an increase of 6 MPa compared to Example 1).
[0111] The fruit aroma intensity (10500) of the full pretreatment combination was 2.2 times that of the single pretreatment (Example 7: 4800), demonstrating a significant bio-physical synergy between lactic acid bacteria fermentation (cherry wood) and ultrasonic treatment (chestnut wood).
[0112] The compressive strength (75 MPa) of the silane-modified magnetic powder (Example 4) was increased by 15.4% compared with that of the unmodified magnetic powder (Example 3: 65 MPa), the leakage rate was reduced to 0.1% (Example 3: 0.5%), and the iron ion leaching was reduced from 0.35 ppm to 0.05 ppm (safety standard <0.1 ppm).
[0113] By using silane coupling agents to achieve chemical bonding between magnetic powder, wood, and adhesives, the industry problems of traditional magnetic powder agglomeration and metal contamination can be solved.
[0114] After the addition of β-glucan (Example 5), the ester content of the wine during the 6-month aging period was 25% higher than that of the unadded group (Example 1), and the sensory score improved from 7.5 to 8.8.
[0115] For the first time, β-glucan has been introduced into a barrel adhesive, extending the flavor release period through microporous adsorption and overcoming the limitations of traditional barrel flavor overload.
[0116] 82MPa is 2.56 times that of proportion 1 (32MPa) and exceeds the traditional oak barrel industry standard (40-50MPa).
[0117] At 0.05%, it is far below the industry average (3-5%) and meets food-grade sealing requirements.
[0118] 55 vol% rice-aroma baijiu (naturally aged for one year) was placed into wooden barrels of the above-mentioned examples and comparative examples, with the volume accounting for 96% of the solvent. The internal temperature of the container was maintained at 18°C, and the relative humidity was maintained at 75%. The barrels were then aged in the dark for one year. The resulting semi-finished liquor was then evaluated, and the results are shown in the table below:
[0119]
[0120] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a multi-material wooden barrel for brewing, characterized in that, Includes the following steps: Step 1: Soften the oak with steam at 110℃ for 3 hours before crushing, then crush the oak to obtain oak particles with an average particle size of 4mm. Cherry wood was soaked in a lactic acid bacteria fermentation broth with a pH of 5.0 for 36 hours before being crushed, and then the cherry wood was crushed to obtain cherry wood particles with an average particle size of 3 mm. Before crushing, the chestnut wood was ultrasonically treated at 50kHz for 1.5h, and then crushed to obtain chestnut wood particles with an average particle size of 2mm. Step 2: Mix oak, cherry, and chestnut wood particles in a weight ratio of 6:2.5:1.5, and add food-grade Fe3O4 magnetic powder that has been surface-grafted with silane coupling agent. The amount of magnetic powder added is 5% of the weight of the wood, and the average particle size is 80nm. Step 3: Treat the mixed wood obtained in Step 2 with microwave power of 800W for 8 minutes in a nitrogen atmosphere, then add natural plant binder accounting for 8% of the weight of the mixed wood and mix. The natural plant adhesive is composed of modified gum arabic, lignin, and β-glucan, with the mass ratio of modified gum arabic to lignin being 7:3, and the amount of β-glucan added being 2% of the total weight of the adhesive. Step 4: The mixture obtained in Step 3 is stamped into a barrel-shaped structure using a stamping press with a pressure of 300 tons. Step 5: Heat the formed barrel-shaped structure to 65℃ and keep it warm for 9 hours to obtain a multi-material wooden barrel for brewing.
Citation Information
Patent Citations
High strength bamboo and wood composite shaving board production technology
CN108673662A
Manufacturing method and application method of lignin-based adhesive for ENF-grade artificial board
CN118240512A
new material, its manufacturing process and objects made of this material
FR1012945A