A high-density erasable information storage glass based on a negatively charged network polyhedron for improving solubility of silver ions and a preparation method thereof
By introducing a charged network polyhedron into the glass and combining femtosecond and continuous laser technologies, the problem of low-cost and precise erasure of silver quantum cluster signals in existing technologies has been solved, achieving the effect of high-density erasable information storage.
Patent Information
- Application Number
- CN202510500732.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-04-21
AI Technical Summary
Existing technologies struggle to achieve low-cost, precise micro-area erasure and rewriting of silver quantum cluster signals in femtosecond laser information storage, and traditional methods suffer from high costs or glass loss due to overall thermal erasure.
By introducing a charged network polyhedron into the glass, the glass is prepared by high-temperature melting, and combined with femtosecond laser and continuous laser processing technology, a high-density erasable information storage glass is formed. Femtosecond laser is used to write silver quantum clusters, and continuous laser is used to achieve micro-area erasure.
It achieves low-cost and precise micro-area signal erasure and rewriting, reduces losses during the erasure process, and improves the erasability and stability of information storage.
Smart Images

Figure CN120483519B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of information storage glass, and particularly relates to a high-density erasable information storage glass based on a negatively charged polyhedron to improve the solubility of silver ions and its preparation method. Background Technology
[0002] The rapid development of femtosecond laser technology recently promises to cleverly resolve the contradiction between the photosensitivity required for high-speed read / write operations and the stability required for long lifespan in high-capacity optical storage materials. Femtosecond lasers have very narrow pulse widths, and after focusing, their energy density can reach as high as 10^6 kiloseconds. 14 -10 15 W / cm 2 This exceeds the Coulomb field strength of a hydrogen atom. Therefore, near the focal point, even if the material itself does not have intrinsic absorption at the laser wavelength, it will undergo highly selective microstructural modification due to nonlinear reactions such as laser-induced multiphoton absorption and multiphoton ionization, thus endowing the material with unique optical functions. This advantage is unmatched by other laser sources (traditional continuous and long-pulse lasers).
[0003] Fluorescent silver quantum clusters, [Ag m ] x+ It is a molecular cluster composed of several to dozens of silver atoms or ions, and is also a novel, efficient, multi-level femtosecond laser-induced fluorescence information carrier. [Ag] m ] x+ With sub-nanometer dimensions comparable to the electron Fermi wavelength, a molecular-like energy level structure determined by quantum confinement effects, and highly efficient molecular-like fluorescence, it exhibits low optical sensitivity suitable for low-power femtosecond laser writing. Its valence state is relatively easy to control, and the raw material cost is also low. Therefore, as a low-threshold fluorescent active center, it is considered a superior choice for quantum clusters with overall performance compared to other noble metals such as copper, gold, and platinum. Meanwhile, inorganic glass is considered one of the best media materials for femtosecond laser information storage, possessing excellent physicochemical stability, particularly low optical sensitivity and a high laser damage threshold. Due to the fluorescence [Ag... m ] x+ Quantum clusters exhibit high chemical reactivity, thus dispersing them within a glass network is beneficial for stabilizing their size distribution and fluorescence properties. Therefore, femtosecond lasers can be used to... (The sentence is incomplete and requires further context to translate accurately.) + Spatially resolved microstructure rewriting in glass, Ag + Electrons readily accepting laser-induced ionization are reduced and aggregate to grow into fluorescent [Ag] m ] x+ Quantum clusters.
[0004] Network External Body Y 3+The function of connecting glass network structures differs from that of alkaline earth metals (e.g., Na, K, Ca, and Ba), where the Y-ion electric field strength is K(Y). 3+ The electric field strength of Y₂O₃ (3.75) is greater than that of any other alkaline earth metal ion. When a large amount of Y₂O₃ is introduced into the glass system, unlike other alkaline earth metal ions that exhibit crystallization, the [YO₆] octahedra are connected by shared edge oxygen to form a glass network, similar to a differential phase in the middle of the glass. This glass network does not cause crystallization in the glass, and it can connect multiple phosphate segments to form a three-dimensional network structure. The formation of this hybrid network not only increases the proportion of non-bridging oxygen in the middle of the glass network, but also forms silver ion channels when the glass is irradiated by a femtosecond laser, thereby improving the sensitivity of silver ions to the femtosecond laser.
[0005] The mechanism of femtosecond laser-induced silver quantum cluster formation is as follows: When the initial series of femtosecond laser pulses interact with the glass mechanism, Ag+ and the phosphate matrix generate a large number of free electrons through multiphoton absorption. These free electrons lead to the formation of Ag+ ions. 0 Formation (Ag) + +e - →Ag 0 The reaction rate depends on the doping concentration and the degree of electron diffusion. However, the formation of silver quantum clusters is an irreversible reaction, meaning that information stored in micro-areas is very difficult to erase. Currently, in the field of laser information storage, there are two common methods for erasing: 1. In the field of laser storage perovskite quantum dot glass, the common method is to use femtosecond lasers to achieve micro-area erasure. The limitation of this method is that femtosecond laser erasure is expensive, and there are currently no literature reports on this method for erasing silver clusters; 2. By heat-treating the glass with signals written in the micro-area at a temperature slightly above the glass transition point, the silver quantum clusters within the glass flow, thereby achieving signal erasure. The disadvantages are: this method achieves thermal erasure of the entire glass through heat treatment, and cannot achieve micro-area signal erasure; secondly, the erasure process generates silver quantum clusters, causing significant loss of information stored in the glass. Summary of the Invention
[0006] To overcome the shortcomings of the prior art, this invention provides a high-density erasable information storage glass based on a charged network polyhedron to improve the solubility of silver ions. The glass prepared by this invention using a high-temperature melting method contains Ag... + This invention develops a glass composition and technology for repeatedly erasing silver quantum cluster micro-regions using femtosecond laser processing, exhibiting high laser sensitivity and chemical stability, and low laser damage threshold. A series of continuous lasers is then employed to achieve continuous erasure of micro-area information storage, with the laser erasure wavelength ranging from 400 to 800 nm. A high-density erasable information storage glass based on a negatively charged network polyhedron to enhance silver ion solubility, wherein, by molar percentage, the network-forming cations, network intermediate cations, network exogenous cations, and activator silver ions have the following stoichiometric ratios:
[0007] The positively charged network is formed by [PO4]. + The intermediate component of the charge-discharge network is [AlO4]. - [MgO4] 2- and [ZnO4] 2- The network exosome cation is Al. 3+ Mg + Y 3+ .
[0008] Furthermore, by molar percentage, the bridging oxygen connected to the network formidable body and the non-bridging oxygen connected to the network exogenous body have the following stoichiometric ratio: bridging oxygen 40-60%, non-bridging oxygen 40-60%.
[0009] A method for preparing high-density erasable information storage glass based on a negatively charged polyhedron network to enhance silver ion solubility includes: (1) Weigh the required mass of the oxide and fluoride powder raw materials corresponding to the cations according to the molar percentage ratio; (2) Mix the corresponding oxide powder raw materials of the cation evenly, melt them and pour them into the mold to form glass blocks, and anneal them to remove internal stress; (3) Using a femtosecond laser to write at a predefined depth downwards on the glass surface, the Ag-based ink is written by the interaction between the femtosecond laser pulse and the glass. + Silver clusters with a molecular-like structure composed of ions and Ag atoms; (4) Erasing the micro-area pattern using a continuous laser; (5) Repeat steps (3) and (4) multiple times to obtain a silver ion information storage glass that can be wiped multiple times.
[0010] Further, in step (1), the corresponding oxide and fluoride powder raw materials include: P2O5, Al2O3, AlF3, Y2O3, MgF2, ZnF2 and Ag2O.
[0011] Furthermore, in step (2), the melting temperature is 1200~1550℃ and the melting time is 0.5~3 hours.
[0012] Furthermore, in step (2), the heat preservation annealing temperature is 300~400℃ and the heat preservation time is 12~24 hours.
[0013] Furthermore, in step (3), the wavelength of the femtosecond laser is 1030 nm; the predefined depth is 100 μm.
[0014] Furthermore, in step (4), the wavelength range of the continuous laser is 400~800 nm.
[0015] The technical solutions provided by the embodiments of this application may include the following beneficial effects: This invention, through the rational introduction of raw materials such as ZnF2, MgF2, and AlF3, can form [AlO4]. - [MgO4] 2- and [ZnO4] 2- Negatively charged tetrahedral units improve the connectivity of the glass three-dimensional network, while Ag... + Ions act as charge compensators for these tetrahedra, promoting uniform distribution, and can also form [ZnO6], [MgO6], and [AlO6], generating a large number of non-bridging oxygen-linked Ag atoms. + Ions; High concentration of non-bridging oxygen, solubility strategy: Introducing fluorides into pure oxide glasses breaks fluorophosphate bonds, generating a large amount of non-bridging oxygen and Ag. + The connection allows for a higher concentration of silver ions.
[0016] High-concentration rare-earth Y-doped phosphate glasses form a large number of non-bridging oxygens. The [YO6] octahedra can form inverse glass structures to connect the broken chains of the phosphate phase separation, thus generating a large number of non-bridging oxygen structures that stabilize Ag. + It can also form Ag after femtosecond laser irradiation. + The glass network has a high sensitivity to lasers, and the formation of a large number of non-bridging oxides and fluorides in the glass network results in a low laser damage threshold for the glass. It can achieve ion rearrangement in the network structure with a single pulse of low energy, further reducing the energy loss of femtosecond laser processing.
[0017] This application provides a technique for repeatedly erasing and rewriting micro-area silver clusters using continuous lasers, filling a significant gap in the erasure of silver ions in femtosecond laser information storage. It also provides a technique for erasing silver quantum cluster signals using visible continuous lasers. This involves irradiating the micro-area processed by a femtosecond laser for a certain duration to erase the signal; the erased signal area can then be reprocessed with a new signal using a femtosecond laser. This application achieves micro-area signal erasure using continuous lasers, resulting in low cost, precise erasure, and reduced losses during the erasure process.
[0018] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and do not limit this application. Attached Figure Description
[0019] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0020] Figure 1 The X-ray photoelectron spectrum of O1s in the glass sample obtained in Example 1; Figure 2 The image shows the X-ray photoelectron spectrum of Al coordination in the glass sample obtained in Example 2. Figure 3 The image shows the X-ray photoelectron spectrum of Al coordination in the glass sample obtained in Example 3. Figure 4 The X-ray photoelectron spectrum of Al coordination in the glass sample obtained in Example 4; Figure 5 The image shows the micro-area fluorescence mapping of the glass sample obtained in Example 1 after laser erasure at 561 nm, where (a)-(d) are the micro-area fluorescence mapping images after laser erasure at 0s, 6s, 12s, and 18s, respectively. Figure 6 The image shows the micro-area fluorescence mapping of the glass sample obtained in Example 2 after laser erasure at 488 nm, where (a)-(d) are the micro-area fluorescence mapping images after laser erasure at 0s, 6s, 12s, and 18s, respectively. Figure 7 The image shows the micro-area fluorescence mapping of the glass sample obtained in Example 3 after laser erasure at 639 nm, where (a)-(d) are the micro-area fluorescence mapping images after laser erasure at 0s, 6s, 12s, and 18s, respectively. Figure 8 The image shows the micro-area fluorescence mapping of the glass sample obtained in Example 4 after laser erasure at 405 nm, where (a)-(d) are the micro-area fluorescence mapping images after laser erasure at 0s, 6s, 12s, and 18s, respectively. Figure 9 This is a schematic diagram of the repeated wiping of the glass sample obtained in Example 1. Detailed Implementation
[0021] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application.
[0022] The terminology used in this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The singular forms “a,” “the,” and “the” used in this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used herein refers to and includes any or all possible combinations of one or more of the associated listed items.
[0023] It should be noted that, unless otherwise specified, the features in the following embodiments and implementation methods can be combined with each other.
[0024] According to the random network theory of glass, in the fluoroaluminophosphate glass of this invention, the glass mainly contains [PO4]. + [AlO4] - , of which [PO4] + The Q2 and Q1 atoms mainly form a chain-like structure, [AlO4]. - Q4 and Q3 can connect different phosphorus oxygen chains, thus improving the three-dimensional connectivity of the phosphorus oxygen network. This increases Ag... + The concentration in glass can be achieved through two strategies: (1) by introducing negatively charged [AlO4] into the glass system. - [ZnO4] 2- With [MgO4] 2- Tetrahedrons can significantly improve the dispersion uniformity of Ag and enhance Ag... + / (Ag + +Ag 0 (2) In the glass system, [P(O,F)4] forms a broken glass network, and the high electronegativity of [YO6] not only increases the proportion of non-bridging oxygen, but also connects the broken network chains, due to Ag + It can also coordinate with non-bridging oxygen, thus improving the Ag content of the glass system. + Solubility, i.e., the formation of an increase in Ag in the glass system + / (Ag + +Ag 0 This invention realizes a high-concentration non-bridging oxygen-coordinated silver ion information storage glass density information, which can provide a new material basis for the development of low-energy-consumption high-density information storage technology.
[0025] Continuous laser irradiation in a micro-area generates a large amount of heat accumulation, causing the local temperature of the glass to exceed the glass transition point. This accelerates the ion migration rate in the local area, causing silver quantum clusters in the glass to migrate and diffuse outwards from the area previously written by the femtosecond laser, resulting in the disappearance of fluorescence in the glass micro-area. However, after rewriting information using laser irradiation, the femtosecond laser can not only grow new quantum clusters in the glass, but also cause the previously dispersed silver quantum clusters to reassemble in the irradiated area, ensuring that the intensity of the information written a second time remains very high. Example 1
[0026] Step S1: Weigh the required masses of P2O5, Al2O3, AlF3, Y2O3, MgF2, ZnF2ZnF, and Ag2O according to the molar percentage ratio. Mix the powdered raw materials thoroughly and place them in a corundum crucible. In this composition, Ag2O accounts for 10% of the total molar amount of the phase-separated fluorophosphate, AlF3, MgF2, and ZnF2 each account for 5% of the total molar amount of the fluorophosphate, P2O5 and Al2O3 account for 30% and 15% respectively, and Y2O3 accounts for 30%.
[0027] Step S2: Place the glass in a box furnace at 1450ºC for 45 minutes and melt it. Pour the melt into a mold to form a glass block. Place the glass block at 300ºC for 12 hours to remove internal stress. Polish the glass to a surface of 3000 grit and then perform femtosecond laser micro-area processing. Finally, take the powder to test XPS. Figure 1 The XPS image shows that the non-bridging oxygen concentration in the glass obtained in this embodiment is 50.4%, which enables the rapid formation of silver ion channels under femtosecond laser, facilitating the formation of fluorescent silver clusters. The femtosecond laser processing conditions are 200 kHz single pulse, 60 nJ, and the processed area is observed under a confocal microscope. Then, a 2 W 561 nm continuous laser is used to erase the micro-area signal written by the femtosecond laser. The system preset the residual fluorescence intensity to 10%, and after 24 s, the residual fluorescence intensity is 35%, indicating that the erasure effect is generally not ideal and the time needs to be extended. Example 2
[0028] Step S1: Weigh the required masses of P2O5, Al2O3, AlF3, Y2O3, MgF2, ZnF2ZnF, and Ag2O according to the molar percentage ratio. Mix the powdered raw materials thoroughly and place them in a corundum crucible. In this composition, Ag2O accounts for 10% of the total molar amount of fluorophosphate, ZnF2 accounts for 15%, AlF3 and MgF2 each account for 2.5%, P2O5 and Al2O3 account for 30% and 20% respectively, and Y2O3 accounts for 20%.
[0029] Step S2: Subsequently, the glass is placed in a box furnace at 1450ºC for 45 minutes for melting and holding. The melt is then poured into a mold to form a glass block. The glass block is then placed at 300ºC for 16 hours to remove internal stress. Figure 2 The XPS image of the glass obtained in this embodiment shows that [AlO4] accounts for 53.7%, and [AlO4] is negatively charged. - This method effectively improves the stability of glass-type silver. After polishing the glass to a 3000-grit surface, femtosecond laser micro-area processing was performed. The femtosecond laser processing conditions were 200 kHz single pulse, 60 nJ. The processed area was observed under a confocal microscope. Then, a 2 W 488 nm continuous laser was used to erase the micro-area signal written by the femtosecond laser. The system was preset to have a residual fluorescence intensity of 10%. After 24 seconds, the residual fluorescence intensity was 14%, indicating a good erasure effect that met the requirements. Example 3
[0030] Step S1: Weigh the required masses of P2O5, Al2O3, AlF3, Y2O3, MgF2, ZnF2ZnF, and Ag2O according to the molar percentage ratio. Mix the powdered raw materials thoroughly and place them in a corundum crucible. In this composition, Ag2O accounts for 10% of the total molar amount of fluorophosphate, MgF2 accounts for 15%, AlF3 and ZnF2 each account for 2.5%, P2O5 and Al2O3 account for 30% and 20% respectively, and Y2O3 accounts for 20%.
[0031] Step S2: Subsequently, the glass is placed in a box furnace at 1450ºC for 45 minutes for melting and holding. The melt is then poured into a mold to form a glass block. The glass block is then placed at 300ºC for 24 hours to remove internal stress. Figure 3 The XPS image of the glass obtained in this embodiment shows that [AlO4] accounts for 57%, and [AlO4] is negatively charged. -The improvement can further enhance the stability of silver in the glass. After polishing the glass to a surface of 3000 grit, femtosecond laser micro-area processing was performed. The femtosecond laser processing conditions were 200 kHz single pulse and 60 nJ. The processed area was observed under a confocal microscope. Then, a 10 W 639 nm continuous laser was used to erase the micro-area signal written by the femtosecond laser. The system preset the residual fluorescence intensity to 10%. After 24 s, the residual fluorescence intensity was 41%, which was a poor erasure effect. The laser erasure time still needs to be extended. Example 4
[0032] Step S1: Weigh the required masses of P2O5, Al2O3, AlF3, Y2O3, MgF2, ZnF2, ZnF, and Ag2O according to the molar percentage ratio. Mix the powdered raw materials thoroughly and place them in a corundum crucible. In this composition, Ag2O accounts for 10% of the total molar amount of fluorophosphate, AlF3 accounts for 15%, MgF2 and ZnF2 each account for 2.5%, P2O5 and Al2O3 account for 30% and 20% respectively, and Y2O3 accounts for 20%.
[0033] Step S2: Place the glass in a box furnace at 1450ºC for 45 minutes and heat for melting. Pour the melt into a mold to form a glass block. Place the glass block at 300ºC for 20 hours to remove internal stress. Figure 4 The XPS image of the glass obtained in this embodiment shows that [AlO4] accounts for 64.1%. Compared to Embodiments 2 and 3, the glass obtained in this embodiment contains negatively charged [AlO4]. - With a higher proportion, the stability of silver in the glass was further improved. After polishing the glass to a surface of 3000 grit, femtosecond laser micro-area processing was performed. The femtosecond laser processing conditions were 200 kHz single pulse, 60 nJ, and the processed area was observed under a confocal microscope. Then, a 10 W 405 nm continuous laser was used to erase the micro-area signal written by the femtosecond laser. The system was preset to have a residual fluorescence intensity of 10%, and after 24 seconds, the residual fluorescence intensity was 10%, indicating excellent erasure performance that meets application requirements.
[0034] Table 1. Fluorescence intensity of the glass sample obtained in Example 4 after multiple erasures and re-input signals.
[0035] Depend on Figure 5-8After continuous laser erasure at different wavelengths under the same time and conditions, the residual fluorescence intensity in the glass was 639nm > 561nm > 488nm > 405nm, and the residual fluorescence intensity was 41% > 35% > 14% > 10%, respectively. The shorter the continuous laser erasure wavelength, the better the erasure effect. This system allows erasable glass to still be inscribed after multiple erasures. Figure 9 The diagram shows the fluorescence intensity after two erasures and inscriptions. Table 1 shows that after 10 inscriptions, the fluorescence intensity was still 54%.
[0036] Other embodiments of this application will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed herein.
Claims
1. A method for preparing high-density erasable information storage glass based on a negatively charged polyhedron to improve the solubility of silver ions, characterized in that, (1) Weigh the required mass of the oxide and fluoride powder raw materials corresponding to the cations according to the molar percentage ratio. The powder raw materials include P2O5, Al2O3, AlF3, Y2O3, MgF2, ZnF2 and Ag2O. Based on the total molar number of fluorophosphates, Ag2O accounts for 10%, AlF3 accounts for 15%, MgF2 and ZnF2 each account for 2.5%, P2O5 and Al2O3 account for 30% and 20% respectively, and Y2O3 accounts for 20%. (2) Mix the powder raw materials evenly, melt them and pour them into a mold to form glass blocks, and anneal them to remove internal stress; (3) Using a femtosecond laser to write at a predefined depth downwards on the glass surface, the Ag-based ink is written by the interaction between the femtosecond laser pulse and the glass. + Silver clusters with a molecular-like structure composed of ions and Ag atoms; (4) Erasing the micro-area pattern using a continuous laser; (5) Repeat steps (3) and (4) multiple times to obtain a silver ion information storage glass that can be wiped multiple times.
2. The preparation method according to claim 1, characterized in that, In molar percentage, the stoichiometric ratio of bridging oxygen connected to the network foramen to non-bridging oxygen connected to the network exosome is as follows: bridging oxygen 40-60%, non-bridging oxygen 40-60%.
3. The preparation method according to claim 1, characterized in that, In step (2), the melting temperature is 1200~1550℃ and the melting time is 0.5~3 hours.
4. The preparation method according to claim 1, characterized in that, In step (2), the heat preservation annealing temperature is 300~400℃ and the heat preservation time is 12~24 hours.
5. The preparation method according to claim 1, characterized in that, In step (3), the wavelength of the femtosecond laser is 1030 nm; the predefined depth is 100 μm.