A low-expansion invar foil and a method for manufacturing and using the same

By using periodic commutation square wave pulse electrodeposition and heat treatment processes, the problems of uneven composition and high thermal expansion coefficient of Invar alloy foil in traditional processes have been solved, and low-expansion Invar alloy foil suitable for OLED displays has been prepared, achieving high-resolution and low-cost production.

CN120485878BActive Publication Date: 2026-11-24UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510772662.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-11
Publication Date
2026-11-24
Estimated Expiration
2045-06-11

AI Technical Summary

Technical Problem

Existing technologies struggle to produce ultra-thin, uniformly composed Invar alloy foils with low thermal expansion coefficients required for high-resolution OLED displays. Traditional rolling processes are complex and costly, while electrodeposition methods suffer from limitations on iron content due to the thickness of the diffusion layer.

Method used

A low-expansion Invar alloy foil was prepared by using a periodic commutation square wave pulse electrodeposition combined with heat treatment. By adjusting parameters such as forward and reverse conduction time, duty cycle and frequency, the nickel-iron ratio and compositional uniformity were controlled. Subsequently, the crystal orientation and grain size were controlled by heat treatment.

Benefits of technology

A low-expansion Invar alloy foil with a smooth surface, uniform composition, and easily controllable thickness was obtained, with a thermal expansion coefficient of less than 1×10⁻⁶/℃, which meets the performance requirements of OLED displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120485878B_ABST
    Figure CN120485878B_ABST
Patent Text Reader

Abstract

This invention discloses a low-expansion Invar alloy foil, its preparation method, and its application, belonging to the field of electronic information material preparation technology. The preparation method includes the following steps: performing periodically commutated square wave pulse electrodeposition on an Invar alloy plating solution, followed by heat treatment of the electrodeposited Invar alloy foil to obtain the low-expansion Invar alloy foil; wherein the conditions during the periodically commutated square wave pulse electrodeposition process are: forward conduction working time: 50-500 ms, forward duty cycle: 30%-70%, forward pulse frequency: 10-500 Hz, and forward current density: 30-80 mA / cm². 2 Reverse conduction time: 50-500ms, reverse duty cycle: 30%-70%, reverse pulse frequency: 10-500Hz, reverse current density: 5-20mA / cm² 2 This invention reduces the thickness of the cathode diffusion layer through periodically commutated square wave pulse electrodeposition, thereby promoting Fe deposition. 2+ Mass transfer is improved to increase and stabilize the iron content of the alloy foil, resulting in an ultrathin Invar alloy foil with uniform composition. The obtained alloy foil is then subjected to heat treatment to control its crystal orientation and grain size, thereby reducing the linear thermal expansion coefficient and achieving the preparation of low-expansion Invar alloy foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic information material preparation technology, and particularly relates to a low-expansion Invar alloy foil, its preparation method and application. Background Technology

[0002] Organic light-emitting diodes (OLEDs) have garnered significant attention due to their high brightness, high contrast, vibrant colors, and lightweight portability, and are widely used as a key semiconductor device to replace traditional liquid crystal displays (LCDs). For OLED displays, the fine metal mask (FMM) is a core component that greatly influences the display's performance. Invar alloy foil has an extremely low coefficient of thermal expansion over a wide temperature range, making it considered the best substrate for fabricating FMMs, with huge market demand and economic benefits. However, it requires meeting stringent requirements such as near-zero inclusions, extremely low coefficient of thermal expansion, and ultra-thinness.

[0003] Generally, the thinner the Invar alloy foil, the higher the resolution of the OLED display. Industrial Invar alloy foil with a thickness of 20μm or more is typically produced using a rolling process. Rolling Invar alloy foil involves multiple processes, including smelting and forging, hot or cold rolling, annealing, and pickling. This process is complex, requires large equipment, involves many inclusions, and the high rolling pressure makes controlling the thickness, width, and surface quality of the product extremely difficult and complex. The thinner the alloy foil, the higher the rolling cost, and it is accompanied by problems such as reduced rigidity, processing difficulties, and increased defects. Obtaining ultra-thin Invar alloy foil through rolling is very difficult. Therefore, it is difficult to achieve a resolution higher than one-quarter high definition (QHD) for rolled Invar alloy foil.

[0004] Electrodeposition offers advantages such as low cost, near-zero inclusions, and precise control over composition and thickness, making it a highly advantageous method for preparing near-zero inclusion ultrathin strips. However, traditional DC electrodeposition results in a relatively thick diffusion layer at the cathode-electrolyte interface, limiting the Fe... 2+ The reduction of this process is not conducive to increasing and stabilizing the iron content of Invar alloy foil. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention proposes a low-expansion Invar alloy foil, its preparation method, and its applications.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] One of the technical solutions of this invention:

[0008] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0009] The low-expansion Invar alloy foil is prepared by periodically commutating square wave pulse electrodeposition on the Invar alloy plating solution and then heat-treating the electrodeposited Invar alloy foil.

[0010] The conditions for the periodic commutation square wave pulse electrodeposition process are as follows:

[0011] Forward conduction time: 50-500ms, forward duty cycle: 30%-70%, forward pulse frequency: 10-500Hz, forward current density: 30-80mA / cm² 2 Reverse conduction time: 50-500ms, reverse duty cycle: 30%-70%, reverse pulse frequency: 10-500Hz, reverse current density: 5-20mA / cm² 2 .

[0012] Beneficial effects: This invention reduces the thickness of the cathode diffusion layer through periodically commutated square wave pulse electrodeposition, promoting Fe... 2+ Mass transfer is improved to increase and stabilize the iron content of the alloy foil, resulting in an ultrathin Invar alloy foil with uniform composition. The obtained alloy foil is then subjected to heat treatment to control its crystal orientation and grain size, thereby reducing the linear thermal expansion coefficient and achieving the preparation of low-expansion Invar alloy foil.

[0013] Optionally, the Invar alloy plating solution comprises the following components:

[0014] Soluble nickel salts, soluble iron salts, pH buffers, ion complexing agents, brighteners, antioxidants, surfactants, and deionized water.

[0015] Furthermore, the mass ratio of nickel salt to iron salt in the Invar alloy plating solution is (235-280):(60-100).

[0016] Furthermore, the soluble nickel salt includes nickel sulfate hexahydrate and nickel chloride hexahydrate; and / or,

[0017] The soluble iron salt is ferrous sulfate heptahydrate; and / or,

[0018] The pH buffer is boric acid; and / or,

[0019] The ionic complexing agent is sodium citrate; and / or...

[0020] The brightening agent is saccharin (o-benzoylsulfonylimide); and / or,

[0021] The antioxidant is ascorbic acid; and / or,

[0022] The surfactant is sodium dodecyl sulfonate.

[0023] The nickel-iron main salt system used in the plating solution of this invention is a sulfuric acid-chlorination system, which has high solubility and good conductivity. Boric acid can improve the stability of the plating solution; sodium citrate can promote the co-deposition of iron and nickel; saccharin can improve the surface brightness of the coating; ascorbic acid can effectively prevent oxidation of the plating solution and the coating; sodium dodecyl sulfonate can reduce surface defects of the alloy foil. Through the synergistic effect between the components, the plating solution of this invention can achieve efficient, stable and quality-controllable Invar alloy deposition.

[0024] Furthermore, based on mass concentration, the Invar alloy plating solution comprises the following components:

[0025] 10-20 g / L boric acid, 200-220 g / L nickel sulfate hexahydrate, 35-60 g / L nickel chloride hexahydrate; 30-50 g / L sodium citrate, 2-4 g / L saccharin, 0.2-0.5 g / L sodium dodecyl sulfate, 5-10 g / L ascorbic acid, and 60-100 g / L ferrous sulfate heptahydrate.

[0026] Furthermore, the temperature of the Invar alloy plating solution is 50-70℃, and the pH is 2-4.

[0027] Beneficial effects: The Invar alloy plating solution provided by this invention, through the scientific proportioning of each component within the mass concentration range and the precise control of the temperature range, is conducive to achieving stability of the electrodeposition process, controlling the nickel-iron ratio of the Invar alloy foil product, and the uniformity of the alloy foil composition.

[0028] Optionally, the conditions during the heat treatment process are:

[0029] In a pure hydrogen atmosphere at a pressure of 1×10 3 ~1×10 6 At Pa, the temperature is increased to 600-900℃ at a heating rate of 5-7℃ / min, held at this temperature for 30-120 minutes, and then cooled to room temperature.

[0030] Beneficial effects: The heat treatment process of the present invention is beneficial to controlling grain growth and crystal orientation, reducing the thermal expansion coefficient of Invar alloy foil, thereby obtaining low-expansion Invar alloy foil.

[0031] The second technical solution of the present invention:

[0032] A low-expansion Invar alloy foil is prepared by the above-described preparation method.

[0033] Optionally, the low-expansion Invar alloy foil has an average iron content of 62-66% wt.% and an average coefficient of thermal expansion of less than 1×10⁻⁶ in the temperature range of 25–150°C. -6 / ℃, thickness is 15-20μm.

[0034] Beneficial effects: This invention obtains Invar alloy foil with a smooth surface, uniform composition, and easily controllable thickness by adjusting pulse parameters. Further optimization of the thermal expansion properties of the Invar alloy foil through a controlled atmosphere heat treatment process yields an iron content (mass fraction) of 64±2%, a thickness of approximately 15–20 μm, and an average coefficient of thermal expansion (within the temperature range of 25–150 °C) of less than 1×10⁻⁶. -6 Low expansion Invar alloy foil at / ℃.

[0035] The Invar alloy foil prepared by the highly controllable, simple, and low-cost preparation process of this invention greatly improves the shortcomings of traditional electrodeposited Invar alloy foil, such as uneven composition and high coefficient of thermal expansion.

[0036] The third technical solution of this invention:

[0037] Application of a low-expansion Invar alloy foil in the preparation of electronic information materials and semiconductor devices.

[0038] Compared with the prior art, the present invention has the following advantages and technical effects:

[0039] In the electrodeposition process, this invention adjusts the iron-nickel ratio and compositional uniformity of the deposited alloy foil by adjusting periodic commutation square wave pulse parameters such as forward and reverse conduction time, forward and reverse duty cycle, and forward and reverse frequency. Among these, the reverse current is beneficial for obtaining a smooth Invar alloy foil surface. Furthermore, the thermal expansion performance of the Invar alloy foil is optimized through a heat treatment process, ultimately resulting in an ultrathin Invar alloy foil with near-zero expansion.

[0040] This invention greatly improves upon the shortcomings of traditional electrodeposited Invar alloy foil, such as uneven composition and high coefficient of thermal expansion. The Invar alloy foil obtained by the method of this invention is not only uniform in composition and easy to control in thickness, but also optimizes the overall performance of Invar alloy foil, making it an important method for obtaining Invar alloy foil with near-zero expansion. Attached Figure Description

[0041] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0042] Figure 1 A process flow diagram for preparing low-expansion Invar alloy foil according to the present invention;

[0043] Figure 2 This is a schematic diagram of the periodic commutation square wave pulse current waveform and parameters of the present invention;

[0044] Figure 3 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the low-expansion Invar alloy foil finally obtained in Example 1 of the present invention are shown.

[0045] Figure 4 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the low-expansion Invar alloy foil finally obtained in Example 2 of the present invention are shown.

[0046] Figure 5 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the low-expansion Invar alloy foil finally obtained in Example 3 of the present invention are shown.

[0047] Figure 6 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the low-expansion Invar alloy foil finally obtained in Example 4 of the present invention are shown.

[0048] Figure 7 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the low-expansion Invar alloy foil finally obtained in Example 5 of the present invention are shown.

[0049] Figure 8 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the low-expansion Invar alloy foil finally obtained in Example 6 of the present invention are shown.

[0050] Figure 9 Elemental distribution diagram of the cross section of the iron-nickel alloy foil prepared in Comparative Example 1;

[0051] Figure 10 The graphs show the coefficient of thermal expansion of the low-expansion Invar alloy foils obtained in Examples 1 to 6, and the iron-nickel alloy foils prepared in Comparative Examples 1 and 2, within the temperature range of 25 to 150°C. Detailed Implementation

[0052] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0053] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0054] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0055] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0056] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0057] like Figure 1 As shown, this embodiment of the invention provides a method for preparing a low-expansion Invar alloy foil, comprising the following steps:

[0058] Step 1: Prepare the Invar alloy plating solution: Dissolve the soluble metal salt, pH buffer, ion complexing agent, brightener, antioxidant, and surfactant in deionized water, ensuring thorough dissolution and uniform mixing to obtain the plating solution. Let the plating solution stand for 24 hours, then filter.

[0059] Step 2, Pulse Electrodeposition: Using a high-purity titanium plate as the cathode and a high-purity nickel plate or a high-purity iron plate as the anode, the plating solution obtained in Step 1 is used to obtain Invar alloy foil by periodic commutation square wave pulse electrodeposition.

[0060] Step 3, Controlled Atmosphere Heat Treatment: The Invar alloy foil obtained in Step 2 is heat-treated in a specific atmosphere and temperature to obtain a low-expansion Invar alloy foil.

[0061] In some alternative embodiments, the Invar alloy electroplating solution in step (1) is prepared as follows:

[0062] Boric acid (pH buffer) is dissolved in deionized water at 50-70℃, and then nickel sulfate hexahydrate and nickel chloride hexahydrate (soluble metallic nickel salts) are added to obtain an aqueous solution of nickel salts.

[0063] Sodium citrate (ion complexing agent), saccharin (brightening agent), sodium dodecyl sulfonate (surfactant), and ascorbic acid (antioxidant) are dissolved in deionized water at 50-70℃ in sequence to obtain an aqueous solution of the additive.

[0064] Mix the nickel salt aqueous solution and the additive aqueous solution, then dissolve ferrous sulfate heptahydrate (a soluble metallic iron salt) in the mixture, fully dissolve and mix evenly to obtain the plating solution. After the plating solution has stood for 24 hours, filter it for later use.

[0065] In some optional embodiments, in step (1), the Invar alloy plating bath contains boric acid at a concentration of 10-20 g / L, nickel sulfate hexahydrate and nickel chloride hexahydrate at concentrations of 200-220 g / L and 35-60 g / L, respectively; sodium citrate at a concentration of 30-50 g / L, saccharin at a concentration of 2-4 g / L, sodium dodecyl sulfate at a concentration of 0.2-0.5 g / L, ascorbic acid at a concentration of 5-10 g / L, and ferrous sulfate heptahydrate at a concentration of 60-100 g / L. The plating bath temperature is 50-70°C, and the pH is 2-4.

[0066] In some alternative embodiments, the cathode used in step (2) is a high-purity titanium plate, and the anode is a high-purity nickel or high-purity iron plate. A dual-pulse power supply is used to provide a periodically commutated square wave pulse current (current waveform and parameters are as follows). Figure 2 As shown, the forward pulse current and reverse pulse parameters are independently adjustable. During forward square wave pulse electrodeposition, an iron-nickel co-deposition reaction occurs at the cathode. However, when a reverse square wave pulse is applied, the alloy foil deposited on the cathode undergoes anodic dissolution, with iron preferentially dissolving compared to nickel, thus replenishing the iron ions consumed in the solution during forward deposition. The forward pulse current parameters are as follows: forward conduction time: 50-500ms; forward duty cycle: 30%-70%; forward pulse frequency: 10-500Hz; forward current density: 30-80mA / cm². 2 The reverse pulse current parameters are as follows: reverse conduction time: 50-500ms; reverse duty cycle: 30%-70%; reverse pulse frequency: 10-500Hz; reverse current density: 5-20mA / cm² 2 .

[0067] In some alternative embodiments, the specific gas in step (3) is pure hydrogen at a pressure of 1×10⁻⁶. 3 ~1×10 6 Pa, heating rate of 5-7℃ / min, holding temperature of 600-900℃, holding time of 30-120 minutes, and cooling rate of 5-7℃ / min to room temperature after holding.

[0068] Unless otherwise specified, "room temperature" in this invention refers to 20-30℃.

[0069] All raw materials used in this invention were purchased from the market.

[0070] The technical solution of the present invention will be further illustrated by the following embodiments.

[0071] Example 1

[0072] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0073] (1) Dissolve boric acid (pH buffer) in deionized water at 50°C, then add nickel sulfate hexahydrate and nickel chloride hexahydrate (soluble metallic nickel salt) to obtain an aqueous solution of nickel salt;

[0074] Sodium citrate (ion complexing agent), saccharin (brightening agent), sodium dodecyl sulfonate (surfactant), and ascorbic acid (antioxidant) were dissolved in deionized water at 50°C in sequence to obtain an aqueous solution of the additives;

[0075] Mix the above-mentioned nickel salt aqueous solution and additive aqueous solution, then dissolve ferrous sulfate heptahydrate (soluble metallic iron salt) in the mixture, fully dissolve and mix evenly to obtain a plating solution. After the plating solution has stood for 24 hours, filter it for later use.

[0076] In the above Invar alloy plating solution, the concentration of boric acid is 10 g / L, the concentration of nickel sulfate hexahydrate is 220 g / L, the concentration of nickel chloride hexahydrate is 35 g / L, the concentration of sodium citrate is 30 g / L, the concentration of saccharin is 2 g / L, the concentration of sodium dodecyl sulfate is 0.2 g / L, the concentration of ascorbic acid is 5 g / L, the concentration of ferrous sulfate heptahydrate is 60 g / L, and the pH of the plating solution is 2.5.

[0077] (2) Place the high-purity titanium cathode plate and the high-purity nickel anode plate vertically in parallel in the electrolytic cell. Use the plating solution obtained in step (1) and employ a dual-pulse power supply to provide a periodically commutated square wave pulse current for electrodeposition. The forward pulse current parameters are as follows: forward conduction time: 300ms; forward duty cycle: 60%; forward pulse frequency: 100Hz; forward current density: 30mA / cm². 2 The reverse pulse current parameters are as follows: reverse conduction time: 300ms; reverse duty cycle: 50%; reverse pulse frequency: 100Hz; reverse current density: 5mA / cm². 2 An Invar alloy foil was obtained on a cathode titanium substrate by electrodeposition at a temperature of 50°C and a time of 50 min.

[0078] (3) Place the Invar alloy foil obtained in step (2) in high-purity hydrogen gas at a pressure of 1×10⁻⁶. 5 Pa, heating rate of 5℃ / min, holding temperature of 600℃, holding time of 120min, and cooling rate of 5℃ / min to room temperature after holding to obtain low expansion Invar alloy foil.

[0079] Figure 3 The images show the macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross-section (d), and elemental distribution (e) of the Invar alloy foil obtained in this embodiment. Figure 3 As can be seen, the Invar alloy foil has a smooth, crack-free surface, with an iron content of 63.78 wt.% and a nickel content of 36.22 wt.%. The foil is approximately 15 μm thick, with a dense cross-section and uniform composition distribution, and an average iron content of approximately 63.93 wt.%. The Invar alloy foil exhibits good thermal expansion properties, such as... Figure 10 As shown in Table 1, the average coefficient of thermal expansion of the finally prepared Invar alloy foil is 0.49 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃.

[0080] Example 2

[0081] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0082] The difference between Example 2 and Example 1 lies in the pulse parameters: the forward pulse parameters are as follows: forward conduction time: 500ms; forward duty cycle: 50%; forward pulse frequency: 10Hz; forward current density: 40mA / cm². 2 The reverse pulse parameters are as follows: reverse conduction time: 200ms; reverse duty cycle: 50%; reverse pulse frequency: 10Hz; reverse current density: 10mA / cm². 2 The electrodeposition temperature was 50℃ and the electrodeposition time was 40 min.

[0083] Figure 4 The images show the macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross-section (d), and elemental distribution (e) of the Invar alloy foil obtained in this embodiment. Figure 4 As can be seen, the Invar alloy foil has a smooth, crack-free surface, with an iron content of 63.21 wt.% and a nickel content of 36.79 wt.%. The alloy foil is approximately 15 μm thick, with a dense cross-section and uniform composition distribution, and an average iron content of approximately 63.79 wt.%. The thermal expansion properties of the Invar alloy foil are as follows... Figure 10 As shown in Table 1, the average coefficient of thermal expansion of the finally prepared Invar alloy foil is 0.46 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃.

[0084] Example 3

[0085] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0086] (1) Dissolve boric acid (pH buffer) in deionized water at 60℃, then add nickel sulfate hexahydrate and nickel chloride hexahydrate (soluble metallic nickel salt) to obtain an aqueous solution of nickel salt;

[0087] Sodium citrate (ion complexing agent), saccharin (brightening agent), sodium dodecyl sulfonate (surfactant), and ascorbic acid (antioxidant) were dissolved in deionized water at 60°C in sequence to obtain an aqueous solution of the additives;

[0088] Mix the above-mentioned nickel salt aqueous solution and additive aqueous solution, then dissolve ferrous sulfate heptahydrate (soluble metallic iron salt) in the mixture, fully dissolve and mix evenly to obtain a plating solution. After the plating solution has stood for 24 hours, filter it for later use.

[0089] In the above Invar alloy plating solution, the concentrations are as follows: boric acid 15 g / L, nickel sulfate hexahydrate 200 g / L, nickel chloride hexahydrate 50 g / L, sodium citrate 35 g / L, saccharin 2 g / L, sodium dodecyl sulfate 0.2 g / L, ascorbic acid 5 g / L, ferrous sulfate heptahydrate 80 g / L, and pH 3.5.

[0090] (2) Place the high-purity titanium cathode plate and the high-purity iron anode plate vertically in parallel in the electrolytic cell. Use the plating solution obtained in step (1) and employ a dual-pulse power supply to provide a periodically commutated square wave pulse current for electrodeposition. The forward pulse current parameters are as follows: forward conduction time: 300ms; forward duty cycle: 40%; forward pulse frequency: 300Hz; forward current density: 50mA / cm³. 2 The reverse pulse current parameters are as follows: reverse conduction time: 200ms; reverse duty cycle: 50%; reverse pulse frequency: 100Hz; reverse current density: 10mA / cm². 2 An Invar alloy foil was obtained on a cathode titanium substrate by electrodeposition at a temperature of 60℃ and a time of 30 min.

[0091] (3) Place the Invar alloy foil obtained in step (2) in high-purity hydrogen gas at a pressure of 1×10⁻⁶. 3 Pa, heating rate of 7℃ / min, holding temperature of 750℃, holding time of 60min, and cooling rate of 7℃ / min to room temperature after holding.

[0092] Figure 5 The images show the macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross-section (d), and elemental distribution (e) of the Invar alloy foil obtained in this embodiment. Figure 5 As can be seen, the Invar alloy foil has a smooth, crack-free surface, with an iron content of 65.18 wt.% and a nickel content of 34.82 wt.%. The foil is approximately 15 μm thick, with a dense cross-section and uniform composition distribution, and an average iron content of approximately 65.25 wt.%. The thermal expansion properties of the Invar alloy foil are as follows... Figure 10As shown in Table 1, the average coefficient of thermal expansion of the finally prepared Invar alloy foil is 0.51 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃.

[0093] Example 4

[0094] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0095] The difference between Example 4 and Example 3 lies in the pulse parameters: In step (2), the forward pulse parameters are as follows: forward conduction time: 400ms; forward duty cycle: 30%; forward pulse frequency: 300Hz; forward current density: 50mA / cm² 2 The reverse pulse parameters are as follows: reverse conduction time: 100ms; reverse duty cycle: 70%; reverse pulse frequency: 500Hz; reverse current density: 10mA / cm². 2 The electrodeposition temperature was 60℃ and the electrodeposition time was 30 min.

[0096] Figure 6 The images show the macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross-section (d), and elemental distribution (e) of the Invar alloy foil obtained in this embodiment. Figure 6 As can be seen, the Invar alloy foil has a smooth, crack-free surface, with an iron content of 65.22 wt.% and a nickel content of 34.78 wt.%. The alloy foil is approximately 15 μm thick, with a dense cross-section and uniform composition distribution, and an average iron content of approximately 65.61 wt.%. The thermal expansion properties of the Invar alloy foil are as follows: Figure 10 As shown in Table 1, the average coefficient of thermal expansion of the finally prepared Invar alloy foil is 0.58 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃.

[0097] Example 5

[0098] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0099] (1) Dissolve boric acid (pH buffer) in deionized water at 70°C, then add nickel sulfate hexahydrate and nickel chloride hexahydrate (soluble metallic nickel salt) to obtain an aqueous solution of nickel salt;

[0100] Sodium citrate (ion complexing agent), saccharin (brightening agent), sodium dodecyl sulfonate (surfactant), and ascorbic acid (antioxidant) were dissolved in deionized water at 70°C in sequence to obtain an aqueous solution of the additives;

[0101] Mix the above-mentioned nickel salt aqueous solution and additive aqueous solution, then dissolve ferrous sulfate heptahydrate (soluble metallic iron salt) in the mixture, fully dissolve and mix evenly to obtain a plating solution. After the plating solution has stood for 24 hours, filter it for later use.

[0102] In the above Invar alloy plating solution, the concentrations are as follows: boric acid 20 g / L, nickel sulfate hexahydrate 200 g / L, nickel chloride hexahydrate 60 g / L, sodium citrate 40 g / L, saccharin 4 g / L, sodium dodecyl sulfate 0.5 g / L, ascorbic acid 10 g / L, ferrous sulfate heptahydrate 100 g / L, and the pH of the plating solution is 2.

[0103] (2) Place the high-purity titanium cathode plate and the high-purity nickel anode plate vertically in parallel in the electrolytic cell. Use the plating solution obtained in step (1) and employ a dual-pulse power supply to provide a periodically commutating square wave pulse current for electrodeposition. The forward pulse current parameters are as follows: forward conduction time: 400ms; forward duty cycle: 40%; forward pulse frequency: 100Hz; forward current density: 80mA / cm². 2 The reverse pulse current parameters are as follows: reverse conduction time: 100ms; reverse duty cycle: 60%; reverse pulse frequency: 100Hz; reverse current density: 20mA / cm². 2 An Invar alloy foil was obtained on a cathode titanium substrate by electrodeposition at a temperature of 70℃ and a time of 20 min.

[0104] (3) Place the Invar alloy foil obtained in step (2) in high-purity hydrogen gas at a pressure of 1×10⁻⁶. 6 Pa, heating rate of 5℃ / min, holding temperature of 900℃, holding time of 30min, and cooling rate of 5℃ / min to room temperature after holding.

[0105] Figure 7 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the Invar alloy foil obtained in this embodiment are shown. Figure 7 The Invar alloy foil has a smooth, crack-free surface. The alloy foil contains 64.20 wt.% iron and 35.80 wt.% nickel. The foil is approximately 15 μm thick, with a dense cross-section and uniform composition distribution, with an average iron content of approximately 64.18 wt.%. The thermal expansion properties of the Invar alloy foil are as follows: Figure 10 As shown in Table 1, the average coefficient of thermal expansion of the finally prepared Invar alloy foil is 0.60 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃.

[0106] Example 6

[0107] A method for preparing a low-expansion Invar alloy foil includes the following steps:

[0108] The difference between Example 6 and Example 5 lies in the pulse parameters: In step (2), the forward pulse parameters are as follows: forward conduction time: 200ms; forward duty cycle: 70%; forward pulse frequency: 500Hz; forward current density: 70mA / cm² 2 The reverse pulse parameters are as follows: reverse conduction time: 50ms; reverse duty cycle: 30%; reverse pulse frequency: 200Hz; reverse current density: 10mA / cm². 2 The electrodeposition temperature was 70℃ and the electrodeposition time was 40 min.

[0109] Figure 8 The macroscopic morphology (a), surface morphology (b), spot scan EDS (c), cross section (d), and elemental distribution map (e) of the Invar alloy foil obtained in this embodiment are shown. Figure 8 The Invar alloy foil has a smooth, crack-free surface. The alloy foil contains 63.60 wt.% iron and 36.40 wt.% nickel. The foil is approximately 16 μm thick, with a dense cross-section and uniform composition distribution, with an average iron content of approximately 63.55 wt.%. The thermal expansion properties of the Invar alloy foil are as follows: Figure 10 As shown in Table 1, the average coefficient of thermal expansion of the finally prepared Invar alloy foil is 0.71 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃.

[0110] Comparative Example 1

[0111] The only difference between Comparative Example 1 and Example 1 is that the electrodeposition process in step (2) uses direct current with a current density of 30 mA / cm². 2 All other conditions are the same.

[0112] Figure 9 The image shows the elemental distribution of the iron-nickel alloy foil obtained in Comparative Example 1. The iron content of the iron-nickel alloy foil varies greatly across its cross-section, exhibiting an uneven compositional distribution. The average iron content of the iron-nickel alloy foil is only approximately 55.23 wt.%, far below the range of Invar alloy foil (Fe: 62-66% wt.%). The thermal expansion properties of the iron-nickel alloy foil are as follows... Figure 10 As shown in Table 1, the average coefficient of thermal expansion of the iron-nickel alloy foil prepared in this comparative example is 4.11 × 10⁻⁶ °C in the temperature range of 25–150 °C. -6 / ℃, which is much higher than in Examples 1-6.

[0113] Comparative Example 2

[0114] The only difference between Comparative Example 2 and Example 3 is that the heat treatment step (3) was not performed.

[0115] like Figure 10As shown in Table 1, the Invar alloy foil prepared in this comparative example has an average coefficient of thermal expansion of 8.56 × 10⁻⁶ in the temperature range of 25–150 °C. -6 / ℃, which is much higher than in Examples 1-6.

[0116] The analysis results of the various embodiments and comparative examples show that the iron-nickel alloy foil prepared by periodically commutated square wave pulse current and heat treatment can achieve the composition of Invar alloy, and the coefficient of thermal expansion is less than 1×10⁻⁶. -6 / ℃. Using direct current electrodeposition, the iron content in the iron-nickel alloy foil cannot reach the range of Invar alloy foil. Using periodically commutated square wave pulsed current without heat treatment, the coefficient of thermal expansion of the iron-nickel alloy foil cannot meet the requirements of low-expansion Invar alloy foil. It is evident that the synergistic effect of using periodically commutated square wave pulsed current and heat treatment greatly improves the thermal expansion properties of the iron-nickel alloy.

[0117] Table 1 shows the average iron content and average coefficient of thermal expansion of the iron-nickel alloy foils prepared in Examples 1-6 and Comparative Examples 1-2.

[0118] Table 1

[0119]

[0120] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A method for preparing a low-expansion Invar alloy foil, characterized in that, Includes the following steps: The low-expansion Invar alloy foil is prepared by periodically commutating square wave pulse electrodeposition on the Invar alloy plating solution and then heat-treating the electrodeposited Invar alloy foil. The conditions for the periodically commutated square wave pulse electrodeposition process are as follows: Forward conduction time: 200-500 ms, forward duty cycle: 30%-70%, forward pulse frequency: 10-500 Hz, forward current density: 30-80 mA / cm² 2 Reverse conduction time: 50-300 ms; reverse duty cycle: 30%-70%; reverse pulse frequency: 10-500 Hz; reverse current density: 5-20 mA / cm². 2 ; The low-expansion Invar alloy foil has an average iron content of 62-66 wt.% and an average coefficient of thermal expansion of less than 1×10⁻⁶ in the temperature range of 25-150℃. -6 / ℃; The Invar alloy plating solution comprises the following components based on mass concentration: 10-20 g / L boric acid, 200-220 g / L nickel sulfate hexahydrate, 35-60 g / L nickel chloride hexahydrate; 30-50 g / L sodium citrate, 2-4 g / L saccharin, 0.2-0.5 g / L sodium dodecyl sulfate, 5-10 g / L ascorbic acid, and 60-100 g / L ferrous sulfate heptahydrate; The temperature of the Invar alloy plating solution is 60-70℃, and the pH is 2-4.

2. The method for preparing a low-expansion Invar alloy foil according to claim 1, characterized in that, The conditions during the heat treatment process are: In a pure hydrogen atmosphere at a pressure of 1×10 3 ~1×10 6 Under Pa conditions, the temperature is increased to 600-900℃ at a heating rate of 5~7℃ / min, and held at this temperature for 30~120 minutes.

3. A low-expansion Invar alloy foil, characterized in that, It is prepared by the preparation method according to any one of claims 1-2.

4. The low-expansion Invar alloy foil according to claim 3, characterized in that, The low-expansion Invar alloy foil has an average iron content of 62-66 wt.% and an average coefficient of thermal expansion of less than 1×10⁻⁶ in the temperature range of 25-150℃. -6 / ℃, thickness is 15-20 μm.

5. The application of a low-expansion Invar alloy foil as described in claim 3 or 4 in a semiconductor device.