Preparation of ultrathin polymer electrolyte with wide electrochemical window and application of polymer electrolyte in solid-state lithium metal battery

By introducing 4-fluoro-α-methylstyrene into the polymer electrolyte and using free radical polymerization technology to prepare ultra-thin polycarbonate solid electrolyte, it solves the problem that polymer solid electrolyte materials in the prior art are difficult to meet the high room temperature ion conductivity, wide electrochemical window and dendrite resistance at the same time, and achieves the high energy density and stable cycling performance of lithium metal batteries.

CN120511354APending Publication Date: 2025-08-19UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510640294.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-19
Publication Date
2025-08-19

AI Technical Summary

Technical Problem

The existing polymer solid electrolyte materials are difficult to meet high room temperature ionic conductivity, wide electrochemical windows, excellent dendrite resistance and ultra-thin characteristics at the same time, limiting their practical application in lithium metal batteries.

Method used

Using polyvinylidene fluoride-hexafluoropropylene porous membrane as the framework, 4-fluoro-α-methylstyrene is introduced, and free radical in situ polymerization and crosslinking is initiated by high temperature to prepare ultra-thin polycarbonate solid electrolyte, combining unsaturated ester monomers, conductive lithium salts, crosslinking agents and initiators to prepare high-performance polymer electrolytes.

Benefits of technology

It has achieved high room temperature ionic conductivity, wide electrochemical window and excellent anti-dendrite properties. The battery has high energy density, ultra-thin electrolyte material, wide applicable temperature range, and an electrochemical window of 5.3V. The battery is stable cycling for 1,500 cycles under high voltage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120511354A_ABST
    Figure CN120511354A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium metal batteries, and relates to preparation of an ultrathin polymer electrolyte with a wide electrochemical window and application of the ultrathin polymer electrolyte in a solid-state lithium metal battery, a preparation method comprises the following steps: firstly, coating a substrate with polymer slurry, and then soaking, stripping and drying to obtain a porous membrane matrix; the preparation method comprises the following steps: mixing an electrolyte, a conductive lithium salt, a cross-linking agent, 4-fluorine-alpha-methyl styrene and an initiator to obtain an electrolyte precursor solution; and then supporting the electrolyte precursor liquid on the porous membrane substrate, and carrying out in-situ polymerization and curing to obtain the polymer electrolyte. Compared with the prior art, the thickness of the polycarbonate solid electrolyte is 7.8 microns, and the polycarbonate solid electrolyte shows high room-temperature ionic conductivity, a wide electrochemical window and excellent dendritic crystal resistance. And the corresponding 4.5 V high-voltage LiLCO solid-state battery can stably circulate for 1500 circles at room temperature. The electrolyte is ultrathin, the preparation process is simple, the scale is easy to enlarge, and the electrolyte shows a good practical application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries and relates to a polymer electrolyte and a solid-state lithium metal battery, and in particular to the preparation of an ultra-thin polymer electrolyte with a wide electrochemical window and its application in a solid-state lithium metal battery. Background Art

[0002] Lithium metal has an ultra-high theoretical specific capacity (3860 mAh / g), the lowest electrochemical potential (-3.040 V) and a low density (0.53 g cm -3 ), is the most ideal negative electrode material for the next generation of high-energy lithium batteries. However, the severe dendrite growth problem of metallic lithium severely limits its practical application. The development of solid electrolytes is a key strategy to inhibit the growth of lithium dendrites. At the same time, solid electrolytes replacing traditional electrolytes are expected to fundamentally improve battery safety. In particular, polymer solid electrolytes have good electrode interface wettability and are the most promising type of solid electrolyte material. However, the low room temperature ionic conductivity and poor high-voltage stability of polymer solid electrolytes severely limit their practical application.

[0003] An ideal polymer solid electrolyte should possess the following advantages: 1. High room-temperature ionic conductivity; 2. A wide electrochemical window to match high-voltage cathodes; 3. Excellent dendrite resistance; and 4. Ultrathinness to achieve high battery energy density. However, current polymer solid electrolyte materials struggle to simultaneously meet these advantages. Summary of the Invention

[0004] The present invention aims to provide an ultrathin, wide-electrochemical-window polymer electrolyte for its preparation and application in solid-state lithium metal batteries. The polycarbonate solid electrolyte of the present invention has a thickness of 7.8 microns and exhibits high room-temperature ionic conductivity, a wide electrochemical window, and excellent anti-dendrite properties. The corresponding 4.5V high-voltage Li|LCO solid-state battery can stably cycle 1500 times at room temperature. This electrolyte is ultrathin, has a simple preparation process, and is easily scalable, demonstrating promising prospects for practical application.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A first aspect of the present invention provides a method for preparing a polymer electrolyte, comprising:

[0007] S1: mixing an unsaturated ester monomer, a conductive lithium salt, a cross-linking agent, a modifier, and an initiator to obtain an electrolyte precursor liquid;

[0008] S2: The electrolyte precursor liquid is loaded onto the porous membrane substrate and in situ polymerized and solidified to obtain a polymer electrolyte.

[0009] In some specific embodiments, in step S1, the unsaturated ester monomer is selected from one or more of methyl acrylate, methyl 3,3-dimethacrylate, methyl 2-cyanoacrylate, benzyl acrylate, ethyl acrylate, butyl acrylate, methoxy polyethylene glycol acrylate, vinylene carbonate, and vinyl ethylene carbonate.

[0010] In some specific embodiments, in step S1, the cross-linking agent is selected from one or more of 1,4-butanediol diacrylate, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, N,N'-methylenebisacrylamide, tetraethylene glycol dimethacrylate, ethylene glycol dimethacrylate, pentaerythritol tetraacrylate or 1,4-butanediol diacrylate, and the amount used is 0.1-10 wt% of the unsaturated ester monomer.

[0011] In some specific embodiments, in step S1, the conductive lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate or lithium difluorooxalatoborate, and the amount used is 10-50 wt% of the unsaturated ester monomer.

[0012] In some specific embodiments, in step S1, the modifier is selected from one or more of trifluoroethylene iodide, styrene, 4-chlorostyrene, α-methylstyrene, trifluoroethyl methacrylate or 4-fluoro-α-methylstyrene, and the amount used is 0.1-10 wt% of the unsaturated ester monomer.

[0013] In some specific embodiments, in step S1, in the electrolyte precursor liquid, the mass content of the unsaturated ester monomer is 10-80%; the mass content of the conductive lithium salt is 5-50%; the mass content of the modifier is 0.1-10%; and the mass content of the cross-linking agent is 0.1-10%.

[0014] In some specific embodiments, the mass ratio of vinyl ethylene carbonate, lithium bis(trifluoromethanesulfonyl)imide, trimethylolpropane trimethacrylate, and 4-fluoro-α-methylstyrene is 1140:570:34:(27-81).

[0015] In some specific embodiments, the initiator is azobisisobutyronitrile, and the amount used is 0.1-5% of the mass of vinyl ethylene carbonate.

[0016] In some specific embodiments, in step S2, the method of loading the electrolyte precursor liquid on the porous membrane substrate is selected from one of blade coating, drop coating or dip coating.

[0017] In some specific embodiments, the thickness of the polymer electrolyte is 3 to 30 μm.

[0018] In some specific embodiments, the polymer porous membrane is made of one or more of polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride, polyacrylonitrile, and polymethyl methacrylate.

[0019] In some specific embodiments, in step S2, the method for preparing the porous membrane substrate comprises: coating a polymer slurry on a substrate, then immersing the slurry in water, peeling the slurry, and drying the slurry to obtain a porous membrane substrate. In some specific embodiments, the concentration of the polymer slurry is 80 to 120 g / L, and the coating thickness on the substrate is 80 to 120 μm.

[0020] In some specific embodiments, the solvent in the polymer slurry is one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide or acetone.

[0021] In some specific embodiments, the substrate is selected from one of a glass plate, a silicon wafer or a polytetrafluoroethylene plate.

[0022] In some specific embodiments, the preparation method of the porous membrane substrate includes: using N,N-dimethylformamide as a solvent, dispersing PVDF-HFP therein to prepare a uniform slurry, scraping it onto a glass plate, and then quickly immersing it in deionized water to solidify it into a film, and then fully washing it with anhydrous ethanol and then transferring it to a 100°C vacuum oven to dry overnight to obtain an ultra-thin PVDF-HFP porous membrane material.

[0023] In some specific embodiments, in step S2, during the in-situ polymerization curing, the curing temperature is 25 to 90° C., and the curing time is preferably 2 to 18 hours.

[0024] A second aspect of the present invention provides an application of a polymer electrolyte, characterized in that the polymer electrolyte is used to prepare a solid-state lithium metal battery.

[0025] In some specific embodiments, the solid-state lithium metal battery is selected from one of a solid-state lithium symmetric battery, a solid-state Li|LiFePO4 (LFP) battery, or a solid-state Li|LiCoO2 (LCO) battery.

[0026] In some specific embodiments, the preparation method of the solid-state lithium metal battery includes: coating an electrolyte precursor liquid on a porous membrane substrate, assembling electrode sheets from both sides, and in-situ polymerization and curing.

[0027] Compared with the prior art, the present invention has the following characteristics:

[0028] The present invention provides an ultra-thin polycarbonate solid electrolyte. This uses a simple and easy-to-operate phase separation process to prepare a large-scale polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) porous membrane. Using this membrane as a skeleton, 4-fluoro-α-methylstyrene is introduced, and high-temperature-induced free radical in-situ polymerization and crosslinking are used to achieve the preparation of a high-performance ultra-thin polycarbonate solid electrolyte. The polycarbonate solid electrolyte has high room-temperature ionic conductivity, meeting the requirements for wide-temperature use of electrolyte materials and matching high-voltage positive electrode applications. The electrolyte material is ultra-thin (only 7.8 μm), and the corresponding solid-state metal lithium soft pack exhibits excellent electrochemical performance in the range of -10°C to 80°C, with a battery energy density of up to 495Wh kg. -1 , the room temperature ionic conductivity reaches 10 -4 S cm-1 and above, the electrochemical window is 5.3V (vs.Li + / Li). BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 These are the scanning electron microscope (SEM) images and optical photographs of the polyvinylidene fluoride-hexafluoropropylene porous membrane prepared in Example 1.

[0030] Figure 2 The following are scanning electron microscope (SEM) images and optical photographs of the polycarbonate solid electrolyte material of Example 1.

[0031] Figure 3 This is a cross-sectional SEM image of the polyvinylidene fluoride-hexafluoropropylene porous membrane of Example 1.

[0032] Figure 4 : is a cross-sectional SEM image of the polycarbonate solid electrolyte material of Example 1.

[0033] Figure 5 This is the linear voltammetric sweep curve of the solid electrolyte material in Example 1.

[0034] Figure 6 is the ion migration number of the solid electrolyte material in Example 1.

[0035] Figure 7 The solid-state lithium symmetric battery based on the solid electrolyte material of Example 1 is -2 ,0.1mAh cm -2 Long cycle performance under conditions.

[0036] Figure 8 The solid-state lithium symmetric battery based on the solid electrolyte material of Example 1 is -2 ,0.1mAh cm -2 SEM photograph of the deposition morphology of metallic lithium surface after 50 cycles under the same conditions.

[0037] Figure 9 The solid-state lithium symmetric battery based on the solid electrolyte material of Comparative Example 1 is -2 ,0.1mAh cm -2 SEM photograph of the deposition morphology of metallic lithium surface after 50 cycles under the same conditions.

[0038] Figure 10 This is the rate performance of the solid-state Li|LiFePO4 battery based on the solid electrolyte material of Example 1.

[0039] Figure 11 This is the long cycle performance of the solid-state Li|LiFePO4 battery based on the solid electrolyte material of Example 1 at room temperature and 1C conditions.

[0040] Figure 12 Figure 2 shows the long-cycle performance of a 4.5V high-voltage Li|LiCoO2 battery based on the solid electrolyte material of Example 1 at room temperature and 1C. (a) Solid electrolyte of Example 1; (b) Solid electrolyte of Comparative Example 1.

[0041] Figure 13 The surface capacity of the solid electrolyte material assembled based on Example 1 is 4.5 mAh cm -2 Long cycle performance of high-voltage Li|LiCoO2 soft-pack batteries at room temperature and 0.2C. DETAILED DESCRIPTION

[0042] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0043] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained.

[0044] In the following examples, unless otherwise specified, raw materials, reagents or processing techniques are all conventional commercially available products or conventional processing techniques in the art.

[0045] 1. Preparation of polycarbonate solid electrolyte

[0046] Example 1-1

[0047] (1) Preparation of polyvinylidene fluoride-hexafluoropropylene porous membrane

[0048] 500 mg of polyvinylidene fluoride-hexafluoropropylene (Aladdin reagent, Mw ~ 455,000) was weighed and added to 5 mL of N,N-dimethylformamide. After thorough stirring, a uniform transparent slurry was obtained. Then, a 100 μm scraper was used to evenly apply the slurry to a glass plate. The glass plate containing the slurry was then quickly immersed in deionized water. The slurry quickly solidified into a film upon contact with water and detached from the glass substrate. The polyvinylidene fluoride-hexafluoropropylene film was removed using a polytetrafluoroethylene substrate, repeatedly washed with anhydrous ethanol, and dried in a vacuum oven at 80°C overnight to obtain an ultra-thin porous membrane with uniform thickness.

[0049] Figure 1 The scanning electron microscope (SEM) image and optical photograph of the ultrathin porous membrane prepared in Example 1 of the present invention clearly show that the polyvinylidene fluoride-hexafluoropropylene membrane prepared in the present invention has a rich pore structure.

[0050] (2) Preparation of solid electrolyte precursor

[0051] In an argon-filled glove box (H₂O ≤ 1 ppm, O₂ ≤ 1 ppm), 1140 mg of vinyl ethylene carbonate was added to 570 mg of lithium bis(trifluoromethanesulfonylimide) and stirred uniformly for 1 hour. Then, 34 mg of trimethylolpropane trimethacrylate and 54 mg of 4-fluoro-α-methylstyrene were added and stirred uniformly at room temperature for 2 hours. Then, 10 mg of azobisisobutyronitrile was added as an initiator to the homogeneous slurry, and after stirring at room temperature for 5 hours, a uniform electrolyte precursor solution was obtained.

[0052] (3) Preparation of ultrathin polycarbonate solid electrolytes by in situ polymerization

[0053] In an argon-filled glove box (H2O≤1ppm, O2≤1ppm), the electrolyte precursor liquid was added dropwise to the ultra-thin polyvinylidene fluoride-hexafluoropropylene porous membrane matrix until adsorption saturation, and then heated at 80°C for 8h for in-situ polymerization and curing to prepare an ultra-thin high-performance solid electrolyte with a thickness of 7.8μm.

[0054] Figure 1 This is an SEM photo of the polyvinylidene fluoride-hexafluoropropylene porous membrane, from which we can see that it has a rich pore structure. Figure 2 The following are scanning electron microscope (SEM) and optical photographs of the solid electrolyte of Example 1 of the present invention. Comparison shows that the pore structure of the polyvinylidene fluoride-hexafluoropropylene porous membrane is completely filled with the polycarbonate electrolyte.

[0055] Figure 3 This is a cross-sectional SEM image of a polyvinylidene fluoride-hexafluoropropylene porous membrane. Figure 4 This is a cross-sectional SEM photograph of the solid electrolyte of Example 1 of the present invention. Figure 3 and Figure 4This fully demonstrates that the pores of the polyvinylidene fluoride-hexafluoropropylene porous membrane are fully filled with the polycarbonate electrolyte. The thickness of the prepared polycarbonate solid electrolyte membrane is 7.8 μm.

[0056] Comparative Example 1

[0057] The only difference compared with Example 1-1 is:

[0058] In an argon-filled glove box (H₂O ≤ 1 ppm, O₂ ≤ 1 ppm), 1140 mg of vinyl ethylene carbonate was added to 570 mg of lithium bis(trifluoromethanesulfonylimide) and stirred uniformly for 1 hour. Then, 34 mg of trimethylolpropane trimethacrylate was added and stirred uniformly at room temperature for 2 hours. Then, 10 mg of azobisisobutyronitrile was added as an initiator to the homogeneous slurry. After stirring at room temperature for 5 hours, a uniform electrolyte precursor solution was obtained.

[0059] The obtained precursor was added dropwise to the ultra-thin porous membrane prepared in Example 1 until adsorption was saturated, and the excess slurry on the surface was removed. The membrane was then heated at 80° C. for 8 h for in-situ polymerization to prepare a solid electrolyte having a thickness of about 7.8 μm. The rest of the process was the same as in Example 1-1.

[0060] Example 1-2

[0061] The only difference compared with Example 1-1 is:

[0062] In an argon-filled glove box (H₂O ≤ 1 ppm, O₂ ≤ 1 ppm), 1140 mg of vinyl ethylene carbonate was added to 570 mg of lithium bis(trifluoromethanesulfonylimide) and stirred uniformly for 1 hour. Then, 34 mg of trimethylolpropane trimethacrylate and 27 mg of 4-fluoro-α-methylstyrene were added and stirred uniformly at room temperature for 2 hours. Then, 10 mg of azobisisobutyronitrile was added as an initiator to the homogeneous slurry, and after stirring at room temperature for 5 hours, a uniform electrolyte precursor solution was obtained.

[0063] The obtained precursor was added dropwise to the ultra-thin porous membrane prepared in Example 1 until adsorption was saturated, and the excess slurry on the surface was removed. The membrane was then heated at 80° C. for 8 h for in-situ polymerization to prepare a solid electrolyte having a thickness of about 7.8 μm. The rest of the process was the same as in Example 1-1.

[0064] Examples 1-3

[0065] The only difference compared with Example 1-1 is:

[0066] In an argon-filled glove box (H₂O ≤ 1 ppm, O₂ ≤ 1 ppm), 1140 mg of vinyl ethylene carbonate was added to 570 mg of lithium bis(trifluoromethanesulfonylimide) and stirred uniformly for 1 hour. Then, 34 mg of trimethylolpropane trimethacrylate and 81 mg of 4-fluoro-α-methylstyrene were added and stirred uniformly at room temperature for 2 hours. Then, 10 mg of azobisisobutyronitrile was added as an initiator to the homogeneous slurry, and after stirring at room temperature for 5 hours, a uniform electrolyte precursor solution was obtained.

[0067] The obtained precursor was added dropwise to the ultra-thin porous membrane prepared in Example 1 until adsorption was saturated, and the excess slurry on the surface was removed. The membrane was then heated at 80° C. for 8 h for in-situ polymerization to prepare a solid electrolyte having a thickness of about 7.8 μm. The rest of the process was the same as in Example 1-1.

[0068] Table 1 shows the room temperature ionic conductivity of different electrolytes. It can be seen from the table that the room temperature ionic conductivity of the polycarbonate solid electrolyte without 4-fluoro-α-methylstyrene is 1.47×10 -5 S cm -1 With the introduction of 4-fluoro-α-methylstyrene, the room temperature ionic conductivity of the obtained polycarbonate electrolyte is improved. When the addition amount of 4-fluoro-α-methylstyrene is 3wt%, the room temperature ionic conductivity of the polycarbonate solid electrolyte reaches a maximum of 4.80×10 -4 S cm -1 Continuing to increase the content of 4-fluoro-α-methylstyrene will lead to a decrease in the conductivity of the electrolyte. Figure 5 : is the linear scanning curve of the polycarbonate solid electrolyte of Example 1. It can be seen from the figure that the electrolyte of Example 1 has a wide electrochemical window, reaching 5.3V. Figure 6 This is the ion transference number measurement of the solid electrolyte of Example 1, where the inner small figure is the electrochemical impedance spectrum before and after polarization. The calculated lithium ion transference number of the solid electrolyte of Example 1 is 0.68.

[0069] Table 1 Room temperature ionic conductivity of different electrolytes

[0070] Sample name <![CDATA[Ionic conductivity (S cm -1 )]]> Example 1-1 <![CDATA[4.80×10 -4 ]]> Comparative Example 1 <![CDATA[1.47×10 -5 ]]> Example 1-2 <![CDATA[2.65×10 -4 ]]> Examples 1-3 <![CDATA[3.98×10 -4 ]]>

[0071] 2. Preparation and performance testing of solid-state lithium symmetric batteries

[0072] Example 2

[0073] In an argon-filled glove box (H2O≤1ppm, O2≤1ppm), the PVDF-HFP ultra-thin porous membrane prepared in step (1) of Example 1-1 was immersed in the electrolyte precursor liquid prepared in step (2) of Example 1-1 for adsorption saturation, and then the excess slurry on the surface was scraped off. The lithium symmetrical battery was assembled in the order of lithium sheet, PVDF-HFP porous membrane adsorbing the precursor liquid, and lithium sheet. The assembled battery was left to stand at room temperature for 2 hours, and then heated at 80°C for 8 hours to allow the electrolyte to solidify. After the battery was cooled to room temperature, the battery performance test was carried out, and the charge and discharge performance test was carried out under different current densities and different capacities.

[0074] Comparative Example 2

[0075] In an argon-filled glove box (H2O≤1ppm, O2≤1ppm), the PVDF-HFP ultra-thin porous membrane prepared in step (1) of Example 1 was immersed in the uniform electrolyte precursor liquid prepared in Comparative Example 1 for adsorption saturation, and then the excess slurry on the surface was scraped off. The lithium sheet, the PVDF-HFP porous membrane adsorbing the precursor liquid, and the lithium sheet were assembled in this order. The assembled battery was left to stand at room temperature for 2 hours, and then heated at 80°C for 8 hours to allow the electrolyte to solidify. After the battery was cooled to room temperature, the battery performance test was performed, and the charge and discharge performance test was performed under different current densities and different capacities.

[0076] Figure 7 The lithium symmetric battery assembled based on the solid electrolyte of Example 1 was tested at 0.5 mA cm -2 , 0.1mAh cm -2 Long-cycle performance under these conditions. The lithium symmetric battery based on the solid electrolyte of Example 1 exhibited an ultra-long cycle life of up to 6000 hours at room temperature, with a polarization overpotential of only ~62 mV. In comparison, the lithium symmetric battery based on the solid electrolyte of Comparative Example 1 showed a rapid increase in polarization after only 200 hours of cycling under the same conditions, with a polarization overpotential as high as ~168 mV. Figure 8 The lithium symmetric battery assembled based on the solid electrolyte of Example 1 was -2 , 0.1mAh cm -2 Scanning electron microscope (SEM) photograph of the surface morphology of lithium metal after 50 cycles under the same conditions. It can be seen that the surface deposition of lithium metal after cycling is uniform and no dendrite growth is observed, which indicates that the polycarbonate electrolyte synthesized in the present invention has excellent anti-dendrite performance. In comparison, the lithium symmetric battery assembled based on the solid electrolyte of Comparative Example 1 has severe dendrite growth on the surface of lithium metal after cycling under the same conditions ( Figure 9 ).

[0077] 3. Preparation and performance testing of solid-state lithium metal full batteries

[0078] Example 3

[0079] (1) Preparation of LiFePO4 (LFP) electrode

[0080] LFP, conductive carbon black and polyvinylidene fluoride were weighed according to the mass ratio of 8:1:1, and N-methylpyrrolidone solvent was added. The slurry was evenly mixed using a mixer, and then the slurry was evenly coated on the surface of the aluminum foil using a doctor blade method. The electrode was then transferred to an 80°C vacuum oven for overnight drying.

[0081] (2) Preparation of solid-state LFP / Li half-cell

[0082] In an argon-filled glove box (H2O ≤ 1 ppm, O2 ≤ 1 ppm), the PVDF-HFP ultrathin porous membrane prepared in step (1) of Example 1 was immersed in the electrolyte precursor solution prepared in step (2) of Example 1 until saturated with the electrolyte. Excess slurry on the surface was then scraped off. A battery was assembled in the order of lithium sheet, precursor-adsorbed PVDF-HFP porous membrane, and LFP electrode sheet. The assembled battery was allowed to stand at room temperature for 2 hours, then heated at 80°C for 8 hours to undergo a curing reaction. After cooling the battery to room temperature, the battery cycle performance test was conducted with a test voltage of 2.5-4.0 V.

[0083] Figure 10 The rate performance of the solid-state LFP / Li half-cell assembled based on the solid electrolyte of Example 1. The discharge capacity of the battery at 0.2C, 0.5C, 1C, 2C and 5C conditions is 154.7 mAh g -1 ,153.4mAh g -1 ,150.3mAh g -1 ,144.2mAh g -1 and 131.2mAh g -1 After the battery returns to 0.2C, the discharge capacity can still reach 154.6mAh g -1 . Figure 11 The long cycle performance of the solid-state LFP / Li half-cell assembled based on the solid electrolyte of Example 1 at room temperature and 1C conditions is shown. The battery can stably cycle 1800 cycles, with an average coulombic efficiency of up to 99.93% and a decay rate of as low as 0.01% per cycle.

[0084] Example 4

[0085] (1) Preparation of LiCoO2 (LCO) electrode

[0086] LCO powder, conductive carbon black and polyvinylidene fluoride were added to N-methylpyrrolidone in a mass ratio of 8:1:1. The slurry was evenly mixed using a mixer. The slurry was then evenly coated on the surface of aluminum foil using a doctor blade method. The electrode was transferred to an 80°C vacuum oven and dried overnight.

[0087] (2) Preparation of solid-state LCO / Li button / soft pack batteries

[0088] In an argon-filled glove box (H2O ≤ 1ppm, O2 ≤ 1ppm), the PVDF-HFP ultrathin porous membrane prepared in step (1) of Example 1 was immersed in the electrolyte precursor solution prepared in step (2) of Example 1 until saturated with the electrolyte. Excess slurry on the surface was then scraped off. A button / soft-pack battery was assembled in the order of lithium sheet, precursor-adsorbed PVDF-HFP porous membrane, and LCO electrode sheet. The assembled battery was allowed to stand at room temperature for 2 hours, then heated at 80°C for 8 hours to undergo a curing reaction. The battery was cooled to room temperature, and the battery cycle performance test was performed at room temperature, with a test voltage of 3-4.5V.

[0089] Figure 12 The long cycle performance of the LCO / Li button battery assembled based on the solid electrolyte material of Example 1 shows that the battery exhibits ultra-long life and stable cycling at room temperature and 1C conditions, and the capacity retention rate is as high as 84.8% after 1500 cycles. Figure 13 The cycling performance of the LCO / Li soft pack battery assembled with the solid electrolyte material of Example 1 at room temperature and 0.2C is shown. It is worth noting that the surface capacity of the soft pack battery is as high as 4.5 mAh cm -2 The LCO / Li soft-pack battery utilizes an ultra-thin lithium metal anode. Under the challenging conditions of a negative electrode / positive electrode capacity ratio of only 0.89, it can still stably cycle 40 times. The excellent cycling performance of the soft-pack battery demonstrates the feasibility of this electrolyte material for practical applications.

[0090] In summary, the present invention provides a solid-state lithium metal battery comprising an ultrathin polycarbonate solid electrolyte. The original ultrathin polymer solid electrolyte comprises an ultrathin porous polyvinylidene fluoride-hexafluoropropylene membrane and a polycarbonate solid electrolyte. 4-fluoro-α-methylstyrene is introduced for molecular chain regulation, and a high-performance polycarbonate solid electrolyte is prepared by free radical polymerization. The ultrathin (7.8 μm) polymer solid electrolyte of the present invention has a high room temperature ionic conductivity of 4.8×10 -4 S cm -1 , a wide electrochemical window of 5.3V, wide temperature range applicability (-10℃ to 80℃), and excellent interfacial compatibility with metallic lithium, with a limiting current density of up to 11.5mA cm -2A high-voltage solid-state Li|LiCoO2 (LCO) battery based on this electrolyte can stably cycle 1500 times at room temperature. The electrolyte is simple to prepare and easily scalable, showing promising prospects for large-scale practical applications.

[0091] The above description of the embodiments is intended to facilitate understanding and use of the invention by those skilled in the art. It will be apparent that those skilled in the art can readily make various modifications to these embodiments and apply the general principles described herein to other embodiments without requiring inventive effort. Therefore, the present invention is not limited to the above-described embodiments. Improvements and modifications made by those skilled in the art based on the disclosure of the present invention, without departing from the scope of the present invention, should be within the scope of protection of the present invention.

Claims

1. A method for preparing a polymer electrolyte, characterized in that: include: S1: mixing an unsaturated ester monomer, a conductive lithium salt, a cross-linking agent, a modifier, and an initiator to obtain an electrolyte precursor liquid; S2: The electrolyte precursor liquid is loaded onto the porous membrane substrate and in situ polymerized and solidified to obtain a polymer electrolyte.

2. The method for preparing a polymer electrolyte according to claim 1, wherein In step S1, the unsaturated ester monomer is selected from one or more of methyl acrylate, methyl 3,3-dimethacrylate, methyl 2-cyanoacrylate, benzyl acrylate, ethyl acrylate, butyl acrylate, methoxy polyethylene glycol acrylate, vinylene carbonate, and vinyl ethylene carbonate; and / or, The cross-linking agent is selected from one or more of 1,4-butanediol diacrylate, polyethylene glycol diacrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, N,N'-methylenebisacrylamide, tetraethylene glycol dimethacrylate, ethylene glycol dimethacrylate, pentaerythritol tetraacrylate or 1,4-butanediol diacrylate, and the amount used is 0.1-10 wt% of the unsaturated ester monomer; and / or, The conductive lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate or lithium difluorooxalatoborate, and the amount used is 10-50 wt% of the unsaturated ester monomer; and / or, The modifier is selected from one or more of trifluoroethylene iodide, styrene, 4-chlorostyrene, α-methylstyrene, trifluoroethyl methacrylate or 4-fluoro-α-methylstyrene, and the amount used is 0.1-10 wt% of the unsaturated ester monomer.

3. The method for preparing a polymer electrolyte according to claim 1, wherein: In step S1, the electrolyte precursor liquid comprises 10-80% by weight of the unsaturated ester monomer, 5-50% by weight of the conductive lithium salt, 0.1-10% by weight of the modifier, and 0.1-10% by weight of the cross-linking agent. The initiator is azobisisobutyronitrile, and the amount used is 0.1-5% of the mass of vinyl ethylene carbonate.

4. The method for preparing a polymer electrolyte according to claim 1, wherein In step S2, the electrolyte precursor liquid is loaded onto the porous membrane substrate by a method selected from blade coating, drop coating or dip coating; and / or, The thickness of the polymer electrolyte is 3 to 30 μm; and / or, The material of the polymer porous membrane is one or more of polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride, polyacrylonitrile and polymethyl methacrylate.

5. The method for preparing a polymer electrolyte according to claim 1, wherein In step S2, the method for preparing the porous membrane substrate comprises: coating a polymer slurry on a substrate, then soaking the substrate in water, peeling the substrate, and drying the substrate to obtain the porous membrane substrate.

6. The method for preparing a polymer electrolyte according to claim 4, wherein: The concentration of the polymer slurry is 80 to 120 g / L, and the coating thickness on the substrate is 80 to 120 μm; and / or, The solvent in the polymer slurry is one or more of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide or acetone; and / or, The substrate is selected from one of a glass plate, a silicon wafer or a polytetrafluoroethylene plate.

7. The method for preparing a polymer electrolyte according to claim 1, wherein: In step S2, during the in-situ polymerization curing, the curing temperature is 25-90°C.

8. Use of the polymer electrolyte according to any one of claims 1 to 7, characterized in that: The polymer electrolyte is used for preparing solid-state lithium metal batteries.

9. Use of the polymer electrolyte according to claim 8, characterized in that: The solid-state lithium metal battery is selected from one of a solid-state lithium symmetrical battery, a solid-state Li|LiFePO4 battery or a solid-state Li|LiCoO2 battery.

10. Use of the polymer electrolyte according to claim 8, characterized in that: The preparation method of the solid-state lithium metal battery comprises: coating an electrolyte precursor liquid on a porous membrane substrate, assembling electrode sheets from both sides, and in-situ polymerization and curing.

Citation Information

Cited By

  • Polyacrylate electrolyte membrane as well as preparation method and application thereof

    CN121484225A

  • Polyacrylate electrolyte membrane, method for preparing the same, and use thereof

    CN121484225B