Preparation method of lithium metal battery based on two-dimensional inorganic filler polymer electrolyte
By preparing polymer electrolytes based on two-dimensional inorganic fillers, the problems of low ionic conductivity and insufficient mechanical strength of polymer electrolytes are solved, and a high-safety and high-performance lithium metal battery is achieved.
Patent Information
- Application Number
- CN202510937319.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-08
- Publication Date
- 2025-08-19
AI Technical Summary
The existing polymer electrolyte has low ionic conductivity and insufficient mechanical strength, making it difficult to effectively inhibit lithium dendrites penetration and poor interface compatibility, which limits the safety and performance of lithium metal batteries.
The solution casting method is used to prepare polymer electrolytes based on two-dimensional inorganic fillers. By regulating the functional groups on the surface of the two-dimensional fillers and the nano-limited space design, a dense physical barrier network is formed, which improves ion transmission efficiency and mechanical strength, and inhibits the growth of lithium dendrites.
It significantly improves the ion transmission efficiency and mechanical strength of lithium metal batteries, reduces the risk of internal short circuits, and improves the safety and performance of the batteries.
Smart Images

Figure CN120511369A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium metal batteries, and in particular relates to a method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. Background Art
[0002] Lithium metal batteries, due to their extremely high theoretical specific capacity (3860 mAh / g) and low electrochemical potential (-3.04 V vs. SHE), are considered an ideal anode material for next-generation high-energy-density energy storage systems. However, traditional liquid electrolyte systems present serious safety risks: the inherent low flash point, high volatility, and flammability of carbonate organic solvents lead to a serious risk of thermal runaway. More importantly, the uneven deposition of lithium ions on the anode surface during cycling can trigger uncontrolled dendrite growth and internal short circuits. This safety hazard, combined with the thick and uneven solid electrolyte interface formed by continuous electrolyte consumption, restricts the practical application of lithium metal anodes (Adv. Mater. 2023, 35, 2206-228; Energy Environ. Sci., 2024, 17, 4426-4460). Replacing traditional liquid electrolytes with solid electrolytes is expected to fundamentally address safety issues. Among them, polymer solid electrolytes have attracted widespread attention due to their good flexibility and electrode interface contact. However, their inherent defects such as low room temperature ionic conductivity, insufficient mechanical strength, difficulty in effectively inhibiting lithium dendrite penetration, and poor interface compatibility have limited their industrialization process. In order to synergistically improve the ion transfer rate and the mechanical strength of the electrolyte, the present invention proposes a composite polymer electrolyte that introduces two-dimensional inorganic materials into traditional polymer electrolytes, which is expected to solve the inherent shortcomings of traditional polymer solid electrolytes. On the one hand, the addition of inorganic fillers can significantly improve the overall modulus and mechanical strength of the composite electrolyte, providing a solid barrier for physically blocking lithium dendrites; on the other hand, the interaction between the filler and the polymer chain and lithium salt is expected to create new fast lithium ion transmission channels at the interface, or promote the chain segment movement of the polymer matrix, thereby synergistically improving the ionic conductivity of the system. Through this ingenious design of organic-inorganic collaboration, it shows great potential to solve many inherent defects of traditional single polymer solid electrolytes, and opens up a promising path for the practical application of high-safety, high-performance lithium metal batteries. Summary of the Invention
[0003] In view of the problems of low room temperature ionic conductivity, insufficient mechanical strength, difficulty in effectively suppressing lithium dendrite penetration and poor interface compatibility of existing polymer electrolytes, the present invention provides a method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte, which is prepared into a flexible electrolyte film with uniform structure and controllable thickness by a solution casting method. First, by carefully regulating the functional groups on the surface of the two-dimensional filler (such as oxygen-containing groups, nitrogen-containing groups, sulfur-containing groups or specific organic ligands), it is possible to effectively induce and optimize the dissociation of lithium salts, change and stabilize the solvation sheath structure of lithium ions, thereby reducing the energy barrier for ion migration and significantly improving the ion transfer efficiency. Secondly, these two-dimensional nanosheets are stacked in a directionally or semi-directed manner in the polymer matrix, and the nano-confined space formed between the layers provides a unique and efficient transmission channel for lithium ions. This confinement effect can accelerate the diffusion dynamics of ions at the interface, further compensating for the lack of room temperature conductivity of the polymer matrix. More importantly, the two-dimensional sheets build a dense, continuous physical barrier network within the film, and their high modulus properties greatly enhance the overall mechanical strength of the composite electrolyte. When lithium dendrites attempt to grow and penetrate, these laterally extending rigid sheets can effectively block their longitudinal penetration and force the dendrites to expand laterally along the surface of the sheet, greatly extending their path to the counter electrode and consuming more energy, thereby significantly suppressing the risk of internal short circuits caused by dendrites at the physical level. Therefore, this method, through the coordinated design of surface engineering of two-dimensional fillers, nano-confined ion transport, and physical barriers, is expected to simultaneously overcome key challenges such as ion conduction, dendrite suppression, and interface stability, providing an effective path for the development of highly safe and high-performance solid-state lithium metal batteries.
[0004] The technical solution of the present invention is:
[0005] A method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte, comprising the following steps:
[0006] Step (1) adding a high molecular weight polymer and a lithium salt into a solvent, heating and stirring until completely dissolved to obtain a viscous solution;
[0007] Step (2) adding a two-dimensional inorganic filler to the solution obtained in step (1) and continuing to heat and stir to form a viscous suspension;
[0008] Step (3) pouring the viscous suspension obtained in step (2) into a clean mold, placing the mold on a heating table or in an oven, and evaporating the solvent at a certain temperature to prepare a polymer electrolyte based on a two-dimensional inorganic filler;
[0009] Step (4) taking out the polymer electrolyte obtained in step (3) from the polytetrafluoroethylene mold, assembling into a button battery in the order of the positive electrode, the polymer electrolyte obtained in step (3), and the negative electrode Li, and finally packaging; standing at room temperature to obtain a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte.
[0010] Furthermore, the mass fraction of the high molecular weight polymer in the solution in step (1) is 10% to 40%, and the mass fraction of the lithium salt is 10% to 40%;
[0011] Furthermore, the solvent in step (1) is one or a mixture of two or more of N-methylpyrrolidone (NMP), ethylene glycol dimethyl ether (DME), acetonitrile (AN), N,N-dimethylformamide (DMF), and N,N-dimethylacetamide (DMA);
[0012] Furthermore, the high molecular polymer in step (1) is one or a mixture of two or more of polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), poly(vinylidene fluoride-trifluoroethylene) (PVDF-TrFE), poly(vinylidene fluoride-trifluoroethylene-hexafluoropropylene) (PVDF-TrFE-HFP), and polyethylene oxide (PEO);
[0013] Furthermore, the lithium salt described in step (1) is one or a mixture of two or more of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), and lithium difluorophosphate (LiPO2F2);
[0014] Furthermore, the temperature range of the heating and stirring in step (1) is 60 to 80°C;
[0015] Furthermore, the mass of the two-dimensional inorganic filler added in step (2) is 5% to 20% of the mass of the added high molecular polymer;
[0016] Furthermore, the two-dimensional inorganic filler in step (2) is nano-molybdenum disulfide, nano-tungsten disulfide, graphene, Ti3C2T x 、Ti3CNT x One or a mixture of two or more;
[0017] Furthermore, the ball milling time of the two-dimensional inorganic filler in step (2) is 6 to 18 hours;
[0018] Furthermore, the temperature range of the heating and stirring in step (2) is 60 to 80°C;
[0019] Furthermore, the temperature range of the solvent evaporation in step (3) is 60 to 80°C;
[0020] Furthermore, the positive electrode material described in step (4) is one of lithium manganese oxide (LMO), lithium iron phosphate (LFP), lithium nickel cobalt manganese oxide (NCM), and lithium nickel cobalt aluminum oxide (NCA);
[0021] Furthermore, the standing time in step (4) is 1 to 24 hours.
[0022] Beneficial effects of the present invention:
[0023] 1. The present invention can effectively induce and optimize the dissociation of lithium salts by carefully controlling the functional groups (such as oxygen-containing groups, nitrogen-containing groups, sulfur-containing groups or specific organic ligands) on the surface of the two-dimensional filler, thereby reducing the energy barrier of ion migration and significantly improving the ion transfer efficiency.
[0024] 2. The present invention achieves this by stacking two-dimensional nanosheet layers in a polymer matrix in a directional or semi-directional manner. The nano-confined space formed between the layers provides a unique and efficient transport channel for lithium ions. This confinement effect can accelerate the diffusion dynamics of ions at the interface, further compensating for the insufficient room-temperature conductivity of the polymer matrix.
[0025] 3. The present invention constructs a dense, continuous physical barrier network inside the film through two-dimensional layers. Its high modulus characteristics greatly enhance the overall mechanical strength of the composite electrolyte and significantly suppress the risk of internal short circuit caused by dendrites at the physical level. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the charge and discharge curve of the lithium metal battery based on the two-dimensional inorganic filler polymer electrolyte prepared in Example 1 tested at room temperature and a current density of 0.5C.
[0027] Figure 2 This is the charge and discharge curve of the lithium metal battery based on the two-dimensional inorganic filler polymer electrolyte prepared in Example 2 tested at room temperature and 2C current density.
[0028] Figure 3 TEM image of the SEI layer of the battery based on two-dimensional inorganic filler polymer electrolyte prepared in Example 3 after cycling.
[0029] Figure 4 This is the EIS graph of a stainless steel symmetrical battery assembled with a two-dimensional inorganic filler polymer electrolyte prepared in Example 4.
[0030] Figure 5 This is a comparison chart of the specific capacities of lithium metal batteries based on two-dimensional inorganic filler polymer electrolytes prepared in Examples 1, 5, and 6 tested at room temperature and a current density of 0.5C. DETAILED DESCRIPTION
[0031] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0032] Example 1
[0033] Polyvinylidene fluoride and poly(vinylidene fluoride-trifluoroethylene-hexafluoropropylene) (mass ratio of 1:1) were dissolved in N,N-dimethylformamide and N,N-dimethylacetamide (volume ratio of 1:1) and heated and stirred at 60°C to prepare a 10% solution. Then, the same amount of lithium bis(trifluoromethanesulfonylimide) and lithium bis(fluorosulfonylimide) (mass ratio of 1:1) were weighed and dissolved in the solution and heated and stirred at 60°C to prepare a 10% solution. To this solution, nano-tungsten disulfide (20% by mass of the polymer) that had been ball-milled for 6 hours was added and heated and stirred at 60°C to form a viscous suspension. The resulting viscous suspension was poured into a clean polytetrafluoroethylene mold, which was then placed on a heating plate and the solvent was evaporated at 60°C to prepare a nano-tungsten disulfide-based polymer electrolyte. The positive electrode (NCM811), the polymer electrolyte based on nano-tungsten disulfide, and the negative electrode (Li) were assembled into a button cell in this order and left to stand for 1 hour to prepare a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. The battery was tested at room temperature and a current density of 0.5C, and the discharge capacity was 162.97 mAh g -1 ( Figure 1 ).
[0034] Example 2
[0035] Dissolve poly(vinylidene fluoride-co-hexafluoropropylene) in N,N-dimethylformamide and heat and stir at 70°C to prepare a 30% solution by mass. Then weigh the same amount of lithium bis(trifluoromethanesulfonylimide) and dissolve it in the solution, heat and stir at 70°C to prepare a 30% solution by mass. Add nano-molybdenum disulfide (15% of the mass of the polymer) that has been ball-milled for 12 hours to the above solution, and continue heating and stirring at 70°C to form a viscous suspension. Pour the resulting viscous suspension into a clean polytetrafluoroethylene mold, place the mold on a heating table and evaporate the solvent at 80°C to prepare a polymer electrolyte based on nano-molybdenum disulfide. The positive electrode (LFP), the polymer electrolyte based on nano-molybdenum disulfide, and the negative electrode (Li) are assembled into a button cell in this order and left to stand for 6 hours to prepare a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. The battery was tested at room temperature and a current density of 2C, and the discharge capacity was 103.09 mAh g -1 ( Figure 2 ).
[0036] Example 3
[0037] Dissolve poly(vinylidene fluoride-co-hexafluoropropylene) and poly(vinylidene fluoride-trifluoroethylene) (mass ratio of 1:1) in N-methylpyrrolidone and heat and stir at 70°C to prepare a solution with a mass fraction of 40%. Then weigh the same amount of lithium bis(fluorosulfonyl)imide and lithium difluorooxalatoborate (mass ratio of 1:1) and dissolve them in the solution. Heat and stir at 70°C to prepare a solution with a mass fraction of 40%. Add Ti3C2T4 that has been ball-milled for 12 hours to the above solution. x (5% by mass of the polymer), continue heating and stirring at 70°C to form a viscous suspension. The obtained viscous suspension is poured into a clean polytetrafluoroethylene mold, and the mold is placed on a heating table and the solvent is evaporated at 80°C to prepare a Ti3C2T based x The positive electrode (LFP), based on Ti3C2T x The polymer electrolyte and the negative electrode (Li) were assembled into a button battery in this order and left to stand for 24 hours to prepare a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. Figure 3 TEM image of the SEI layer of the battery based on this electrolyte after cycling.
[0038] Example 4
[0039] Dissolve polyethylene oxide in acetonitrile and heat and stir at 80°C to prepare a 10% solution. Then weigh the same amount of lithium hexafluorophosphate and lithium tetrafluoroborate (mass ratio 9:1) and dissolve them in the solution. Heat and stir at 80°C to prepare a 10% solution. Add Ti3CNT that has been ball-milled for 12 hours to the above solution. x (5% by mass of high molecular weight polymer), continue heating and stirring at 80°C to form a viscous suspension. The obtained viscous suspension is poured into a clean polytetrafluoroethylene mold, and the mold is placed in an oven at 60°C to evaporate the solvent to prepare a Ti3CNT-based x The positive electrode (LFP), based on Ti3CNT x The polymer electrolyte and the negative electrode (Li) were assembled into a button battery in this order and left to stand for 12 hours to prepare a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. Figure 4 The ionic conductivity test results of the electrolyte at 60°C.
[0040] Example 5
[0041] Poly(vinylidene fluoride-co-hexafluoropropylene) was dissolved in ethylene glycol dimethyl ether and heated and stirred at 80°C to form a 30% solution by mass. The same amount of lithium bis(fluorosulfonyl)imide and lithium difluorophosphate (mass ratio of 6:1) was weighed and dissolved in the solution and heated and stirred at 80°C to form a 30% solution by mass. Graphene (5% by mass of the polymer) that had been ball-milled for 18 hours was added to the above solution and continued to be heated and stirred at 80°C to form a viscous suspension. The resulting viscous suspension was poured into a clean polytetrafluoroethylene mold, and the mold was placed in an oven at 60°C to evaporate the solvent to prepare a graphene-based polymer electrolyte. The positive electrode (NCM811), graphene-based polymer electrolyte, and negative electrode (Li) were assembled into a button cell in this order and allowed to stand for 24 hours to prepare a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. The battery was tested at room temperature and a current density of 0.5C, and the discharge capacity was 144.84 mAh g -1 .
[0042] Example 6
[0043] Dissolve poly(vinylidene fluoride-co-hexafluoropropylene) in ethylene glycol dimethyl ether and heat and stir at 70°C to prepare a solution with a mass fraction of 30%. Then weigh the same mass of lithium bis(fluorosulfonyl)imide and dissolve it in the solution, heat and stir at 70°C to prepare a solution with a mass fraction of 30%. Add nano-molybdenum disulfide (20% of the mass of the polymer) that has been ball-milled for 12 hours to the above solution, continue heating and stirring at 70°C to form a viscous suspension. Pour the resulting viscous suspension into a clean polytetrafluoroethylene mold, place the mold on a heating table and evaporate the solvent at 70°C to prepare a polymer electrolyte based on nano-molybdenum disulfide. Assemble the positive electrode (NCM811), the polymer electrolyte based on nano-molybdenum disulfide, and the negative electrode (Li) into a button battery in this order and let it stand for 18 hours to prepare a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte. The battery was tested at room temperature and a current density of 0.5C, and the discharge capacity was 182.43 mAh g -1 , Figure 5 The specific capacity results of Examples 1, 5, and 6 are: 162.97 mAh g -1 , 144.84mAh g -1 、182.43mAhg -1 .
Claims
1. A method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte, characterized in that: Here are the steps: Step (1) adding a high molecular weight polymer and a lithium salt into a solvent, heating and stirring until completely dissolved to obtain a viscous solution; Step (2) adding a two-dimensional inorganic filler to the solution obtained in step (1) and continuing to heat and stir to form a viscous suspension; Step (3) pouring the viscous suspension obtained in step (2) into a clean mold, placing the mold on a heating table or in an oven, and evaporating the solvent at a certain temperature to prepare a polymer electrolyte based on a two-dimensional inorganic filler; Step (4) takes the polymer electrolyte obtained in step (3) out of the mold, assembles the positive electrode, the polymer electrolyte obtained in step (3), and the negative electrode Li into a button battery in the order of positive electrode, and finally packages it; and leaves it to stand at room temperature to obtain a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte.
2. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 1, characterized in that: The mass fraction of the high molecular weight polymer in the solution described in step (1) is 10% to 40%, and the mass fraction of the lithium salt is 10% to 40%.
3. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 1, characterized in that: The solution in step (1) is one or a mixture of two or more of N-methylpyrrolidone, ethylene glycol dimethyl ether, acetonitrile, N,N-dimethylformamide, and N,N-dimethylacetamide; The high molecular polymer described in step (1) is one or a mixture of two or more of polyvinylidene fluoride, poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-trifluoroethylene), poly(vinylidene fluoride-trifluoroethylene-hexafluoropropylene), and polyethylene oxide; The lithium salt described in step (1) is one or a mixture of two or more of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium difluorophosphate.
4. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 1, characterized in that: The mass of the two-dimensional inorganic filler added in step (2) is 5% to 20% of the mass of the added high molecular polymer; The two-dimensional inorganic filler described in step (2) is nano-molybdenum disulfide, nano-tungsten disulfide, graphene, Ti3C2T x 、Ti3CNT x One or a mixture of two or more.
5. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 1, characterized in that: The temperature range of the heating and stirring in step (1) is 60-80°C; The temperature range of the heating and stirring in step (2) is 60-80°C; The temperature range of heating and evaporating the solvent in step (3) is 60-80°C.
6. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 1, characterized in that: The positive electrode material described in step (4) is one of lithium manganate, lithium iron phosphate, lithium nickel cobalt manganate, and lithium nickel cobalt aluminum oxide.
7. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 4, characterized in that: The ball milling time of the two-dimensional inorganic filler in step (2) is 6 to 18 hours.
8. The method for preparing a lithium metal battery based on a two-dimensional inorganic filler polymer electrolyte according to claim 1, characterized in that: In step (4), the standing time is 1 to 24 hours.
Citation Information
Cited By
Polymer electrolyte containing oxygen vacancy vanadium-based filler and preparation method and application thereof
CN120955209A
Polymer electrolyte containing oxygen vacancy vanadium-based filler, and preparation method and application thereof
CN120955209B