A process information laser marking method for assisting assembly of large-size wallboard parts
By spraying a fast-curing coating onto the surface of large panel-like parts and combining it with laser marking, the problems of surface contamination and unclear boundaries during assembly were solved, achieving efficient and accurate assembly marking and cleaning, and improving the standardization of parts manufacturing.
Patent Information
- Application Number
- CN202510652336.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-05-21
AI Technical Summary
Large-sized panel parts suffer from surface contamination, poor boundary standardization, and low processing efficiency during assembly. In particular, the cleaning of stains on titanium alloy and composite material parts is complex, and traditional marking processes are difficult to meet the requirements for precision.
A thin layer is formed by spraying a fast-curing and easy-to-peel coating. Combined with an automated laser marking process, the hole positions and edge boundaries are precisely marked on the thin layer. The coating is then peeled off with a high-pressure water gun to ensure that the surface of the parts is clean.
It enables the assembly of large-size panel parts with precision and standardization, improves production efficiency, reduces manual experience-based operations, and ensures assembly accuracy and appearance quality.
Smart Images

Figure CN120533296B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of assembly marking technology for large-size wall panel parts, and relates to a laser marking method for assisting in the assembly of large-size wall panel parts. Background Technology
[0002] With the continuous development of the aviation industry and the ongoing design and launch of new aircraft models, the requirements for product quality and production efficiency are constantly increasing. Modern aircraft design places higher demands on the surface quality of parts, especially large panel components. As an important part of the aircraft, their surface condition directly affects the overall performance and appearance. To meet the new requirements of future aircraft manufacturing, refined machining markings, assembly precision control, and surface quality protection technologies have become increasingly important. During the assembly and machining of large panel components, operators often leave various ink stains, oil stains, and even shoe prints on the panel surface when marking assembly information such as hole positions. This not only directly affects the appearance of the parts but, in severe cases, can even affect assembly precision, causing many inconveniences for subsequent processing. Especially for panels mainly composed of titanium alloys and composite materials, subsequent stain cleaning is more complex, and improper handling can seriously affect processes such as the final aircraft painting after assembly.
[0003] Furthermore, large panel-type parts often have complex edges such as serrated edges during the assembly process. Because a precise boundary definition standard has not yet been established, the allowances retained during design and manufacturing fluctuate greatly, often ranging from 5 to 10 mm. The removal and alignment of these allowances rely heavily on the experience and judgment of the operators, resulting in low standardization and efficiency in assembly. Traditional manual assembly and marking processes are no longer sufficient to meet the increasingly sophisticated manufacturing requirements.
[0004] CN 115304802 A discloses a rapidly curing protective film for production lines and its application. This film, prepared from polyester diol, dicarboxylic acid ester, and acrylic monomers, has a curing time of less than 5 seconds and can be peeled off without residue. However, it requires a high temperature of 200℃ to achieve residue-free peeling, making it unsuitable for large panel-like parts. CN118755330A discloses an environmentally friendly peelable coating, its preparation method, and its application. Using water-based acrylic emulsion as the main component, combined with various film-forming aids and other additives, a low-VOC environmentally friendly peelable coating is prepared. However, the curing time of this coating exceeds 8 hours, and the film thickness reaches 70-80 μm. An excessively thick protective coating will adversely affect the subsequent assembly accuracy. CN118875508A discloses a laser engraving method and system for automotive interior parts textures. It utilizes a vision lens assembly and a precision UVW vision alignment platform to position the processed parts, achieving precise engraving of the interior texture. However, to avoid adverse effects of laser marking on parts requiring high-performance surfaces, the depth and width of the laser lines must be more precisely controlled. Summary of the Invention
[0005] To address the aforementioned problems, this invention provides a laser marking method for assisting in the assembly of large-size panel-like parts. By using a thin-layer spraying process with a rapidly curing and easily peelable coating, effective anti-fouling can be achieved without affecting assembly accuracy. Simultaneously, combined with automated laser marking technology, various hole positions and edge boundaries can be precisely marked on the thin coating, enabling more refined assembly operations without damaging the appearance and performance of the parts. This improves production efficiency and quality, providing a new feasible solution for high-performance parts facing similar challenges in related fields. This invention solves the problems of high surface contamination, poor standardization of mating boundaries, and low processing efficiency in traditional part assembly marking processes.
[0006] The technical solution of the present invention is as follows:
[0007] A method for laser marking process information to assist in the assembly of large-size panel-like parts, comprising the following steps:
[0008] Step 1: Apply and cure the coating using a spraying method to form a fast-curing, peelable thin layer on the surface of large-sized wall panel parts. The coating thickness is controlled within the range of 5-10μm.
[0009] Step 2: Use laser marking technology to make assembly marks and precisely divide the edge boundaries on the thin layer. The laser marking depth is controlled below 5μm and the line width is less than 0.1mm. After marking, process according to the assembly marks, remove excess material and align according to the dividing boundary.
[0010] Step 3: Use a high-pressure water gun to spray and peel off the coating on the surface of the parts, complete the cleaning and drying, and ensure that the surface of the parts is clean before sending them to the next process.
[0011] In step 1, the components of the coating, by weight, include: 15-25 parts of acrylic monomers with hydrolyzable groups, 65-75 parts of modified acrylic prepolymer, 3-5 parts of photoinitiator, 1.5-3.5 parts of film-forming aid, 1-3 parts of inorganic additive, 0.5-1 part of thickener, and 0.1-0.3 parts of defoamer.
[0012] The preparation process of the acrylic monomer with hydrolyzable groups and the modified acrylic prepolymer is as follows: hydrolyzable groups are introduced into the acrylic monomer by transesterification to form an acrylic monomer with hydrophilic groups; then, the acrylic monomer with hydrolyzable groups is subjected to bulk / solution free radical polycondensation to form a modified acrylic prepolymer; the hydrolyzable groups are one or more of carboxylic acid groups, ester groups, amide groups, and glycine groups; the number average molecular weight of the modified acrylic prepolymer is 5000-8000.
[0013] The acrylic monomers mentioned are one or a mixture of two or more of hydroxy acrylates, amino acrylates, and vinyl ether acrylates.
[0014] The photoinitiator is a free radical photoinitiator, which is one or a mixture of two or more of benzophenone, benzophenone, diphenylethylene, 651 photoinitiator, and ethoxybenzophenone.
[0015] The inorganic additives mentioned above are used to improve the coating's resistance to trampling and laser ablation, and are one or more of aluminum silicate, talc, silicon dioxide, and titanium dioxide.
[0016] In step 1, the spraying process is carried out at an ambient temperature of 20-30℃ and a relative humidity of no more than 60%.
[0017] The spraying process uses air spraying with a spraying pressure of 0.2-0.6MPa, a spraying distance of 15-30cm, and a spraying speed controlled at 0.5-2m / s, forming a film in a single spray.
[0018] The coating is rapidly cured by ultraviolet light irradiation, with a wavelength range of 320-400nm, preferably 365nm, and a curing time of 5-20s.
[0019] In step 2, the laser marking is performed using nitrogen or cold air assisted spraying to reduce the heat impact and ensure the clarity of assembly marks and boundary divisions.
[0020] The laser marking uses an ultraviolet laser with a laser power of 3-10W, a preferred wavelength of 355nm, a pulse width of 10-100ns, a pulse frequency of 20-100kHz, and a line speed of 100-500mm / s.
[0021] The ultraviolet laser is held by a robotic arm. A computer-aided design system generates a 3D model of a large-sized panel-like part and automatically generates a marking path. The path planning is optimized using a genetic algorithm or ant colony algorithm to ensure the accuracy and efficiency of the marking path. During the marking process, the marking operation is precisely executed using G-code or ISO6983 format. The workpiece position is located in real time by a machine vision system, and feedback is provided using an industrial camera or CCD camera to ensure that the laser beam is accurately aligned with the target area and to compensate for deviations in real time.
[0022] In step 3, the water pressure is set in the range of 2-5 MPa, and the distance between the cleaning nozzle and the coating surface is kept at 10-30 cm. It is preferable to use warm water at 30-50℃ for cleaning and film removal to improve the peeling efficiency.
[0023] The present invention has the following advantages:
[0024] 1. This invention provides a new process for improving the standardization and precision of assembly marking on large-sized wall panel parts. First, a 5-10μm rapid-curing, peelable thin layer is sprayed onto the part surface to achieve stain resistance and foot wear resistance. Then, automated laser marking of assembly markings is performed on this thin layer. Finally, after the parts are assembled, the protective layer is quickly peeled off using a high-pressure water gun. The entire process enables detailed and precise marking of assembly markings on the surface of large-sized wall panel parts without compromising assembly accuracy.
[0025] 2. This invention provides a method for preparing a UV-curable and water-soluble peelable coating. By introducing hydrolyzable groups to modify acrylic prepolymers, adding acrylic monomers with hydrophilic groups, selecting free radical photoinitiators, and rationally adding inorganic additives, the prepared coating can be rapidly cured within 5-20 seconds and can be completely peeled off under water washing conditions. At the same time, the coating has anti-stepping and anti-fouling functions, and laser marking can be performed on the film, which can effectively assist in the assembly and marking of large-size wall panel parts.
[0026] 3. This invention provides a laser marking process for engraving assembly marks on organic coatings. The marking depth is controlled within 5μm and the line width is less than 0.1mm. This ensures high precision of assembly marks and clarity of part alignment boundaries, significantly reduces manual experience-based operations, improves the standardization of part manufacturing, and meets the needs of precision assembly.
[0027] 4. The method of the present invention is applicable to auxiliary assembly marking of large-size panel parts, including titanium alloys, carbon-based composite materials, stainless steel and aluminum alloys. Attached Figure Description
[0028] Figures 1(a) to 1(c) This is an example drawing of a large-sized wall panel sample, where O is the center and X is the area where holes are to be drilled.
[0029] Figure 2 A flowchart illustrating the assembly and marking process for large-size wall panel parts, aided by rapid curing of peelable coatings and laser marking techniques. Detailed Implementation
[0030] The specific embodiments of the present invention will be further described below with reference to the accompanying drawings and technical solutions.
[0031] A method for laser marking process information to assist in the assembly of large-sized panel-like parts involves spraying a water-soluble, removable coating that cures rapidly under ultraviolet light, followed by ultraviolet laser marking. The coating primarily consists of a modified acrylic prepolymer rich in hydrolyzable groups, acrylic monomers with hydrophilic groups, and a free radical photoinitiator. The addition of appropriate inorganic additives enhances the coating's resistance to impact and laser ablation. The coating is applied in a single spray, achieving rapid curing in 5-20 seconds under ultraviolet irradiation, with a cured coating thickness of 5-10 μm. This method provides surface protection against contamination and damage during the assembly marking process of large-sized panel-like parts without affecting assembly accuracy. A robotic arm holds an ultraviolet laser to automatically mark assembly holes, lines, and patterns on a thin layer, controlling the marking depth to within 5 μm and the line width to less than 0.1 mm. This allows for more detailed and accurate assembly information marking without affecting the surface quality of the parts themselves. After the parts are assembled and aligned, a high-pressure water gun is used to clean the coating on the surface of the parts. The water-soluble coating can be quickly peeled off, ensuring the best surface condition of the parts.
[0032] Optionally, a semi-transparent colored coating can be formed by adding an appropriate amount of dye to the coating to better check the removal of the coating after peeling. After cleaning, infrared radiation lamps or hot air guns can be used to accelerate the drying of the parts.
[0033] Optionally, the hydrolytic peeling properties of the coating can be further improved by adding an appropriate amount of solvent such as lower alcohol or acetone to the coating.
[0034] Optionally, in addition to spraying, the fast-curing peelable coating can also be applied by brushing, rolling, and scraping to form a film for use in local auxiliary assembly markings on parts.
[0035] Optionally, in addition to using an ultraviolet laser, a fiber laser can also be used for laser marking to form assembly marks, with a preferred wavelength of 1064nm.
[0036] Example 1: Preparation of a rapid-curing peelable coating
[0037] The following three methods for monomer modification, prepolymer preparation, and coating composition ratios for fast-curing peelable coatings are provided, with all raw materials calculated in parts by weight:
[0038] (1) Amino acrylate monomers modified with amide groups: 2-(acryloylamino)ethyl hydrosuccinate monomer is formed by transesterification of 2-hydroxyethylacrylamide (HEAA) and succinic anhydride. The reaction is carried out in dichloromethane at a reaction temperature of 65°C and N-methylimidazolium catalysis for 13 hours, so that the hydroxyl group of HEAA and succinic anhydride are esterified to generate a half ester monomer.
[0039] Prepolymer synthesis: Using a bulk / solution free radical polycondensation route, azobisisobutyronitrile (AIBN) was used as an initiator and polymerized in an oil bath at 60°C for 4 hours under inert nitrogen protection to obtain an amide-modified acrylic acid prepolymer with a number average molecular weight of 7000.
[0040] Coating composition ratio: 71.5 parts amide-modified acrylic prepolymer, 21.4 parts 2-(acryloylamino)ethyl hydrosuccinate monomer, 3.5 parts benzophenone, 1.8 parts film-forming aid, 1 part aluminum silicate, 0.5 parts thickener, and 0.3 parts defoamer.
[0041] (2) Hydroxyacrylate monomers modified with carboxylic acid groups: 2-(acryloyloxy)ethyl hydrosuccinate monomer is formed by transesterification of 2-hydroxyethyl acrylate (HEA) and succinic anhydride. In dichloromethane, at a reaction temperature of 65°C and N-methylimidazole catalysis for 13 h, HEA and succinic anhydride undergo ring-opening esterification to generate a half-ester monomer.
[0042] Prepolymer synthesis: Using a bulk / solution free radical polycondensation route, azobisisobutyronitrile (AIBN) was used as an initiator under inert nitrogen protection. Polycondensation was carried out at a reaction temperature of 65℃ for 5 hours to obtain a carboxylic acid-modified acrylic acid prepolymer with a number average molecular weight of 7000.
[0043] The coating composition is as follows: 65.1 parts of carboxylic acid modified acrylic prepolymer, 24.3 parts of 2-(acryloyloxy)ethyl hydrosuccinate monomer, 3 parts of benzophenone, 3.5 parts of film-forming aid, 3 parts of talc, 1 part of thickener, and 0.1 parts of defoamer.
[0044] (3) Modified vinyl ether acrylate monomers with aminoacetic acid groups: 2-vinyloxyethyl acrylate (VEEA) is formed by transesterification with chloroacetic acid to form 2-(acryloyloxy)ethyl aminoacetic acid ester monomer. In dichloromethane, at a reaction temperature of 65°C and N-methylimidazole catalysis for 12 h, the -O- site of VEEA undergoes transesterification with chloroacetic acid to generate a half-ester monomer.
[0045] Prepolymer synthesis: Using a bulk / solution free radical polycondensation route, azobisisobutyronitrile (AIBN) was used as an initiator under inert nitrogen protection. Polycondensation was carried out at a reaction temperature of 60℃ for 6 hours to obtain an aminoacetic acid-modified acrylic acid prepolymer with a number average molecular weight of 8000.
[0046] Coating composition ratio: 74.5 parts of aminoacetic acid modified acrylic prepolymer, 15.5 parts of 2-(acryloyloxy)ethyl aminoacetic acid ester monomer, 4.2 parts of 651 photoinitiator, 3.2 parts of film-forming aid, 1.6 parts of titanium dioxide, 0.8 parts of thickener, and 0.2 parts of defoamer.
[0047] Taking the first formulation ratio as an example, a general preparation method for coatings is provided, including the following steps:
[0048] (1) Add the prepared prepolymer and monomer to a mixing container in proportion and mix thoroughly. The stirring speed is controlled at 300 rpm, the temperature is maintained at 25℃, and the stirring time is 20 minutes.
[0049] (2) Add inorganic additive powder, increase the stirring speed to 500 rpm, disperse for 15 minutes, and then slowly add film-forming aid and continue stirring for 10 minutes;
[0050] (3) Gradually add thickener according to the viscosity requirements of the coating, reduce the stirring speed to 300 rpm, and continue stirring for 10 minutes. Add defoamer and continue stirring for 5 minutes to remove air bubbles during the mixing process;
[0051] (4) Transfer the base liquid to a low light or dark room environment, continue to reduce the speed to 100 rpm, slowly add the photoinitiator, and stir for 15 minutes;
[0052] (5) Use a 300-mesh stainless steel filter to filter the prepared coating to remove undispersed and large particles. Transfer the coating to an opaque sealed container for storage at 25°C and avoid exposure to high temperature and strong light.
[0053] Example 2: Laser marking of process information to assist in the assembly of large-size panel-like parts
[0054] Implementation instructions are provided using typical large-size wall panel samples, such as... Figures 1(a) to 1(c) As shown, the radius r of the semi-circular arc-shaped wall panel sample is 3m (i.e., the diameter d is 6m), the wall panel thickness t is 8mm, the wall panel length h is 10m, and the two sides of the wall panel have serrated edges with a tooth height m1 and a tooth pitch m2 of 0.1m.
[0055] It is planned to drill holes on the outer surface of the wall panel, with 10 holes in the entire panel, labeled K1, K2, K3...K10 K1-K4 are threaded holes with a diameter of φ6, each n1 distance from the side edge and semi-circular end face of the wall panel, and a length of 0.5m. K5-K4 are threaded holes arranged vertically at equal intervals in the central area of the wall panel. 10 The hole spacing n2 is 0.1m, where K5 and K 10 K6-K9 are threaded holes with a diameter of φ4, and K is a threaded hole with a diameter of φ3. 10 The distance n3 from the side edge of the wall panel is 3m, and the distance n4 from the semi-circular end face is 0.8m.
[0056] The following provides three examples of laser marking processes, with the general workflow as follows: Figure 2 As shown, the process includes five steps: part surface pretreatment, paint spraying, coating curing and thickness measurement, laser marking on the film, assembly, and coating peeling.
[0057] (1) Surface pretreatment of parts: Cold air is used to blow away dust and fine adsorbents from the surface of the parts. Locally contaminated areas are wiped with ethanol or acetone and then dried. A single spraying of the part surface is carried out using an air spray gun, with a spray thickness of 5μm, a spray pressure of 0.2Mpa, a spray distance of 15cm, a spray speed of 2m / s, an ambient temperature of 25℃, and an ambient humidity of 40%. The parts are irradiated with a 320nm ultraviolet radiation lamp panel with a power setting of 800mW / cm. 2 The irradiation distance was 50cm, and the irradiation time was 8s. After complete curing, the thickness of selected points on each part was measured using an eddy current thickness gauge. A thickness reading between 5 and 10μm was considered acceptable. The part was clamped and fixed with fixtures to ensure it was stable and free from shaking. The position of the robotic arm and the focal length of the ultraviolet laser were adjusted to ensure the spot was focused on the film surface. The marking path and text pattern were set, with a laser power of 3W, a wavelength of 355nm, a pulse width of 30ns, a pulse frequency of 50kHz, and a line speed of 500mm / s. Cold air was used for auxiliary spraying during laser marking to reduce the heat effect until all assembly marks and boundary lines were completed. Drilling and part assembly were performed according to the marks. After assembly, the part was rinsed with a high-pressure water gun at a pressure of 2MPa, with the cleaning nozzle 30cm away from the coating surface. The film was removed using 30℃ warm water and dried with hot air. After drying, the surface was inspected again to ensure there were no watermarks or residues.
[0058] (2) Surface pretreatment of parts: Cold air is used to blow away dust and fine adsorbents from the surface of the parts. Locally contaminated areas are wiped with ethanol or acetone and then dried. A single-pass spraying is performed on the surface of the parts using an air spray gun, with a spray thickness of 8μm, a spray pressure of 0.4Mpa, a spray distance of 20cm, a spray speed of 1.5m / s, an ambient temperature of 25℃, and an ambient humidity of 40%. The parts are then irradiated with a 365nm ultraviolet radiation lamp panel with a power setting of 1000mW / cm².2 The irradiation distance was 50cm, and the irradiation time was 12s. After complete curing, the thickness of selected points on each part was measured using an eddy current thickness gauge. A thickness reading between 8±3μm was considered acceptable. The part was clamped and fixed with fixtures to ensure it was stable and free from shaking. The position of the robotic arm and the focal length of the ultraviolet laser were adjusted to ensure the spot was focused on the film surface. The marking path and text pattern were set, with a laser power of 5W, a wavelength of 355nm, a pulse width of 75ns, a pulse frequency of 80kHz, and a line speed of 300mm / s. Cold air was used for auxiliary spraying during laser marking to reduce the heat effect until all assembly marks and boundary lines were completed. Drilling and part assembly were performed according to the marks. After assembly, the part was rinsed with a high-pressure water gun at a pressure of 3.5MPa, with the cleaning nozzle 20cm away from the coating surface. The film was removed using 40℃ warm water and dried with hot air. After drying, the surface was inspected again to ensure there were no watermarks or residues.
[0059] (3) Surface pretreatment of parts: Cold air is used to blow away dust and fine adsorbents from the surface of the parts. Locally contaminated areas are wiped with ethanol or acetone and then dried. A single spraying is performed on the surface of the parts using an air spray gun, with a spray thickness of 10μm, a spray pressure of 0.6Mpa, a spray distance of 30cm, a spray speed of 0.5m / s, an ambient temperature of 25℃, and an ambient humidity of 40%. The parts are irradiated with a 400nm ultraviolet radiation lamp panel with a power setting of 1200mW / cm². 2 The irradiation distance was 50cm, and the irradiation time was 20s. After complete curing, the thickness of selected points on each part was measured using an eddy current thickness gauge. A thickness reading between 10±5μm was considered acceptable. The part was clamped and fixed with fixtures to ensure it was stable and free from shaking. The position of the robotic arm and the focal length of the ultraviolet laser were adjusted to ensure the laser spot was focused on the film surface. The marking path and text pattern were set, with a laser power of 10W, a wavelength of 355nm, a pulse width of 90ns, a pulse frequency of 100kHz, and a line speed of 100mm / s. Cold air was used for auxiliary spraying during laser marking to reduce the heat effect until all assembly marks and boundary lines were completed. Drilling and part assembly were performed according to the marks. After assembly, the part was rinsed with a high-pressure water gun at a pressure of 5MPa, with the cleaning nozzle 15cm away from the coating surface. The film was removed using 50℃ warm water and dried with hot air. After drying, the surface was inspected again to ensure there were no watermarks or residues.
[0060] After the above process, such large-size wall panel parts can reach the preparatory state before process information labeling within 30 minutes. By using automated laser marking technology, the manual input in the process information labeling process can be reduced by more than 5 person-times, the design and processing allowance is as low as 1mm, and the overall assembly efficiency is improved by 20%.
[0061] The core of the process stability of this invention lies in the control of the coating thickness and uniformity, the uniformity of the photocuring radiation field, and the laser marking process parameters. Traditional manual marking is limited by the cleanliness requirements of the panel surface. During assembly marking, only very simple fine-line markings can be made for hole positions and related distance information, resulting in problems such as blurry marks, confusion of processing information, and large marking errors. In actual assembly, further reference to paper process specifications is still required. However, the laser marking method of this invention can mark various hole positions, dimensional data, and special requirements of related parts in detail on the panel surface in the form of data, letters, and even text, without affecting the accuracy of subsequent assembly processing and the appearance of the panel surface, greatly improving assembly efficiency. At the same time, the precise division of part boundaries can also improve the standardization of assembly, reduce the error of manual operation, and facilitate the mating between parts.
Claims
1. A method for laser marking process information to assist in the assembly of large-size panel-like parts, characterized in that, The steps are as follows: Step 1: Apply and cure the coating using a spraying method to form a fast-curing, peelable thin coating on the surface of large-sized wall panel parts. The coating thickness is controlled within the range of 5-10μm. The coating is rapidly cured by ultraviolet irradiation with a wavelength range of 320-400nm and a curing time of 5-20s. Step 2: Use laser marking technology to make assembly marks and precisely divide the edge boundaries on the thin layer. The laser marking depth is controlled below 5μm and the line width is less than 0.1mm. After marking, process according to the assembly marks, remove excess material and align according to the dividing boundary. Step 3: Use a high-pressure water gun to spray and peel off the coating on the surface of the parts, complete the cleaning and drying, and ensure that the surface of the parts is clean before sending them to the next process. In step 1, the components of the coating, by weight, include: 15-25 parts of acrylic monomers with hydrolyzable groups, 65-75 parts of modified acrylic prepolymer, 3-5 parts of photoinitiator, 1.5-3.5 parts of film-forming aid, 1-3 parts of inorganic additive, 0.5-1 part of thickener, and 0.1-0.3 parts of defoamer; The preparation process of the acrylic monomer with hydrolyzable groups and the modified acrylic prepolymer is as follows: hydrolyzable groups are introduced into the acrylic monomer via transesterification to form an acrylic monomer with hydrophilic groups; then, the acrylic monomer with hydrolyzable groups is subjected to bulk / solution free radical polymerization to form a modified acrylic prepolymer; the hydrolyzable groups are one or more of carboxylic acid groups, ester groups, amide groups, and glycine groups; the number average molecular weight of the modified acrylic prepolymer is 5000-8000. The acrylic monomers are one or more of hydroxy acrylates, amino acrylates, and vinyl ether acrylates; the photoinitiator is a free radical photoinitiator, one or more of benzophenone, diphenylethylene, 651 photoinitiator, and ethoxybenzophenone; the inorganic additives, used to improve the coating's resistance to trampling and laser ablation, are one or more of aluminum silicate, talc, silica, and titanium dioxide.
2. According to claim 1, the laser marking method for assisting in the assembly of large-size wall panel parts, in step 1, the spraying is carried out with the ambient temperature controlled at 20-30℃ and the relative humidity not exceeding 60%; air spraying is used, the spraying pressure is 0.2-0.6MPa, the spraying distance is 15-30cm, the spraying speed is controlled at 0.5-2m / s, and a film is formed by a single spraying.
3. The laser marking method for assisting the assembly of large-size panel-like parts according to claim 2, wherein the ultraviolet light irradiation wavelength is 365nm.
4. In the laser marking method for assisting the assembly of large-size panel-like parts according to claim 1, in step 2, the laser marking is performed using nitrogen or cold air assisted spraying.
5. The laser marking method for assisting the assembly of large-size panel-like parts according to claim 1, wherein in step 2, the laser marking uses an ultraviolet laser with a laser power of 3-10W, a wavelength of 355nm, a pulse width of 10-100ns, a pulse frequency of 20-100kHz, and a line speed of 100-500mm / s.
6. The laser marking method for assisting the assembly of large-size panel-like parts according to claim 5, wherein the ultraviolet laser is held by a robotic arm, and a three-dimensional model of the large-size panel-like part is generated by a computer-aided design system, and a marking path is automatically generated. The path planning is optimized using a genetic algorithm or an ant colony algorithm to ensure the accuracy and efficiency of the marking path. The workpiece position is located in real time by a machine vision system, and feedback is provided by an industrial camera to ensure that the laser beam is accurately aligned with the target area and to compensate for deviations in real time.
7. In the laser marking method for process information of large-size wall panel parts according to claim 1, in step 3, the water pressure is set in the range of 2-5MPa, the distance between the cleaning nozzle and the coating surface is maintained at 10-30cm, and warm water at 30-50℃ is used for cleaning and removing the coating.
Citation Information
Patent Citations
Protective film capable of being rapidly cured on production line and application of protective film
CN115304802A
Environment-friendly peelable coating as well as preparation method and application thereof
CN118755330A
Laser engraving method and system for textures of automotive upholstery
CN118875508A
Hot water peelable protective ink and method for improving glass processing protection performance
CN115627096A
PET protective film