Low-silver lead-free tin-based solder paste and preparation method thereof

By using phenolic antioxidants and Bi and Ni elements in low-silver lead-free solder paste, the problem of insufficient residues and wettability after welding is solved, and a low-cost and high-reliability welding material is achieved.

CN120533356APending Publication Date: 2025-08-26YUNNAN PRECIOUS METALS LAB CO LTD

Patent Information

Application Number
CN202510814239.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-18
Publication Date
2025-08-26

AI Technical Summary

Technical Problem

The existing low-silver lead-free solder paste has problems such as many residues after welding, insufficient wetting and high cost, especially corrosive problems caused by the residue of antioxidants and the pressure of rising prices of precious metal silver.

Method used

Phenolic antioxidants such as butylhydroxytoluene or hydroquinol are used to combine Bi and Ni elements to optimize the flux formulation, reduce the silver content to 0.35-0.6%, and oxidation reaction is suppressed at high temperature through phenol antioxidants, decompose and volatilize after welding, and Bi and Ni jointly improve wetting and reliability.

Benefits of technology

Significantly reduce post-weld residues, maintain good wetting and reliability, reduce production costs, and achieve high-performance and low-cost green welding materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120533356A_ABST
    Figure CN120533356A_ABST
Patent Text Reader

Abstract

The invention discloses low-silver lead-free tin-based solder paste and a preparation method thereof, and belongs to the field of welding materials. The soldering paste is composed of 85 wt%-87.5 wt% of tin-based powder brazing filler metal and 12.5 wt%-15 wt% of scaling powder, wherein the tin-based powder brazing filler metal comprises 0.35 wt%-0.6 wt% of Ag, 0.5 wt%-0.8 wt% of Cu, 1.0 wt%-4.0 wt% of Bi, 0.05 wt%-0.08 wt% of Ni and the balance Sn; the soldering flux is composed of rosin, a solvent, an active agent, a thixotropic agent, a film-forming agent, a PH regulator, a surfactant, a phenolic antioxidant and a corrosion inhibitor. The soldering paste has excellent low residue, good wettability and welding reliability, and is especially suitable for surface mount technology (SMT) in the electronic and electric appliance industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a low-silver, lead-free tin-based solder paste and a preparation method thereof, and in particular to a low-silver, lead-free tin-based solder paste that uses a specific phenolic antioxidant in a flux formula to achieve low residue and high wettability and a preparation process thereof. The invention belongs to the field of welding materials and is suitable for surface mount technology (SMT) in the electronic and electrical appliance industry. Background Art

[0002] With the rapid development of electronic technology, electronic products play a vital role in aerospace, automotive, radio and television, and even our daily lives. As society progresses, people's expectations for electronic products are increasing, and electronic products are also moving towards becoming lighter, more portable, more advanced, and more environmentally friendly. The welding of electrode plates in electronic products plays a guiding role in the development of the electronics industry. Among various electrode plate welding processes, SMT (Surface Mounted Technology) significantly reduces raw material loss, saves processing costs, and has simple process technology. Therefore, SMT technology is often used for the welding and mounting of electrode plates in electronic products. The key material in SMT technology is solder paste, which allows surface assembly components to be directly mounted on electrode plates. Solder paste is a paste made of solder powder (generally 85% to 90% by weight) and flux in a specific ratio.

[0003] In traditional SMT technology, Sn-Pb alloy solder pastes are widely produced and used due to their excellent soldering performance and low price. However, they contain high lead content, which poses significant risks to human health and the environment. With increasing awareness of health and global environmental protection, researchers have begun developing new lead-free solder pastes. To effectively replace Sn-Pb solder pastes, researchers have developed various alloys, including Sn-Ag-Cu, Sn-Ag, Sn-Bi, and Sn-Zn. Among them, Sn-Ag-Cu alloy solders offer comparable comprehensive performance to Sn-Pb solders and are expected to become a viable alternative. Common examples of these solders include Sn-3.9Ag-0.6Cu, Sn-3.8Ag-0.7Cu, Sn-3.0Ag-0.5Cu, and Sn-1.0Ag-0.5Cu. Although these solders exhibit excellent weldability, electrical conductivity, oxidation resistance, and thermal stability when made into solder paste, they are prone to forming Ag3Sn brittle phases during use, leading to brittle fracture. Therefore, their wettability needs to be improved. The electronics and electrical industry currently consumes large amounts of solder paste annually, and the price of precious metal silver continues to rise. To enhance market competitiveness, developing new, low-silver Sn-Ag-Cu solder pastes with excellent wettability and low post-solder residue is crucial.

[0004] CN115488546A discloses a silver nanowire-modified tin-silver-copper composite solder paste, which is made of silver nanowires, flux and Sn3.0Ag0.5Cu lead-free solder, wherein the mass percentage of the Sn3.0Ag0.5Cu lead-free solder is 79.6% to 89.9%. The flux is composed of an activator, a film-forming agent, a thixotropic agent, a regulator, a corrosion inhibitor and a solvent. By utilizing silver nanowires to slow down the diffusion rate of Cu in the interface to inhibit the growth of IMC at the solid phase interface, the microstructure at the solder joint is refined, and the soldering performance of the solder paste is improved. CN114367760A discloses a high-reliability halogen-free and lead-free solder paste, which is composed of a flux and a solder alloy powder. The flux includes rosin, an activator, a thixotropic agent, a thermosetting resin, an antioxidant, and an organic solvent. The solder alloy powder is composed of tin, silver, copper, zirconium, cerium, scandium, and iridium, wherein the mass percentage of silver in the solder alloy powder is 6.1% to 9.1%. The addition of scandium and iridium to the solder paste can synergistically improve thermal conductivity, electrical conductivity, and ductility. At the same time, a small amount of multiple rare earth elements can reduce signal interference generated during use, improve the hardness, strength, and heat resistance of the alloy, reduce dielectric loss, and improve the stability of the solder paste. CN118268757A discloses a tin-silver-copper high-temperature solid-crystal solder paste with ultrafine particle size. The solder paste is composed of tin-based solder alloy powder and flux. The mass percentage of silver in the tin-based solder alloy powder is 2% to 3%. The flux is composed of rosin, surfactant, thixotropic agent, activator, solvent, corrosion inhibitor, antioxidant, di(2-ethylhexyl) adipate and dimethyl succinate. By adding appropriate amounts of Ni and Fe elements, the mechanical properties and solder joint reliability of the solder paste are improved. At the same time, ultrafine tin-based solder alloy powder is selected to improve the collapse resistance and printing ability during use.

[0005] Although the SnAgCu solder pastes in the above-mentioned prior art have been improved in terms of solderability, thermal conductivity, heat resistance, stability, etc., there are still some common problems that need to be solved:

[0006] 1. Post-solder residue is a prominent issue: Many solder pastes leave noticeable residue on substrates or around solder joints after soldering. This residue not only affects aesthetics but, more importantly, may contain corrosive ions. Long-term use can lead to reliability issues such as circuit board corrosion, reduced insulation resistance, electromigration, and even short circuits. Antioxidants used in existing technologies (such as phosphites) often incompletely decompose or leave significant residue, a major contributor to post-solder residue.

[0007] 2. Balancing Wettability with the Low Silver Target: Reducing silver content to control costs often results in decreased solder paste wettability. While adding elements like Bi and Ni can improve wettability to a certain extent, the effect is limited and not a core technological breakthrough. Furthermore, simply adjusting alloying elements has little effect on resolving post-solder residue issues.

[0008] 3. Cost pressure: The price of precious metal silver continues to rise, and further reducing the silver content in solder paste is an urgent need of the industry, but it must be achieved without sacrificing welding performance and reliability.

[0009] Therefore, developing a lead-free solder paste that can significantly reduce the silver content while effectively solving the problem of post-soldering residues and maintaining good wettability and reliability has important practical significance and market value. Summary of the Invention

[0010] The present invention addresses the key issues of existing low-silver, lead-free solder pastes, such as excessive post-weld residues and insufficient wettability, and provides an innovative low-silver, lead-free, tin-based solder paste and its preparation method. The developed low-silver, lead-free, tin-based solder paste has a low silver content by mass, low production cost, and is conducive to mass production. At the same time, appropriate amounts of Bi and Ni are added to the tin-based solder. The Bi element can reduce the surface tension between the tin-based solder and the substrate, allowing the solder paste to more evenly cover the solder joints during the welding process. The Ni element can reduce the wetting time and increase the wetting force. The two elements have a synergistic effect on the wettability of the solder. In addition, the antioxidant in the flux is a phenolic antioxidant, which can maintain the activity of the solder at high temperatures, prevent it from reacting with oxygen in the air to cause oxidation, and help maintain the fluidity and wettability of the solder. It is also not easy to carbonize during the welding process, and there is less residue after welding.

[0011] The main technical advantages and innovations of this invention are:

[0012] 1. Significantly Reduces Post-Solder Residue: The selected phenolic antioxidants (butylated hydroxytoluene or hydroquinone) have decomposition temperatures that match typical SMT soldering temperatures (approximately 250°C). During the soldering process, they effectively inhibit the oxidation reaction of solder and flux components at high temperatures, maintaining the solder's excellent activity and fluidity. In the later stages of soldering, they fully decompose and volatilize, leaving virtually no residue on the solder joint or substrate surface. This fundamentally resolves the problem of antioxidant residues in existing technologies.

[0013] 2. Optimizing wettability: The phenolic antioxidant helps maintain the surface tension of the solder at a low level when in liquid state while inhibiting oxidation, and cooperates with the Bi and Ni elements added to the tin-based solder to improve the overall wettability of the solder paste.

[0014] 3. Achieve true low-silver and low-cost: The silver content in tin-based solder is controlled at an ultra-low level of 0.35% to 0.6%, which is significantly lower than the existing common low-silver solder paste (usually >1.0%), greatly reducing the cost of raw materials and facilitating large-scale production and application.

[0015] 4. High reliability: The low residue property avoids the risk of residue corrosion, and the good wettability ensures the integrity and firmness of the solder joint formation. Combined with the potential optimization of the solder joint microstructure by Bi and Ni, the long-term reliability of the solder joint is improved.

[0016] The technical solution of the present invention is:

[0017] The invention discloses a low-silver lead-free tin-based solder paste, which is composed of 85% to 87.5% of tin-based powder solder and 12.5% ​​to 15% of soldering flux (the following percentages are all mass percentages).

[0018] Tin-based powder solder consists of 0.35% to 0.6% silver, 0.5% to 0.8% copper, 1.0% to 4.0% bismuth, 0.05% to 0.08% nickel, and the balance is tin. Bi primarily lowers the solder's melting point and surface tension, improving fluidity; nickel inhibits excessive intermetallic compound (IMC) growth at the interface, enhancing wetting and shortening wetting time. This alloy design maintains basic soldering performance while reducing Ag content, while the phenolic antioxidant in the flux plays a crucial synergistic role in resolving technical challenges.

[0019] Furthermore, the flux composition includes:

[0020] Rosin 30.4% to 35.0%: Provides basic flux activity and film-forming properties. Optional KE-604 rosin, polymerized rosin, hydrogenated rosin, or a combination thereof.

[0021] Solvent 41.2% to 45.2%: dissolves other components and adjusts viscosity. Optional solvents include tripropylene glycol butyl ether, diethylene glycol, triethylene glycol, glycerol, isopropyl ketone, or a combination thereof.

[0022] 5.0% to 7.4% of active agent: removes oxides on the metal surface. Optional agents include succinic acid, oxalic acid, lauric acid, sebacic acid, or a combination thereof.

[0023] Thixotropic agent 5.4% to 7.0%: gives the solder paste good printability and anti-slump properties. Hydrogenated castor oil is preferred;

[0024] Film former 3.2% to 4.6%: forms a protective film to prevent reoxidation. Optional materials include polymethyl methacrylate, acrylic resin, butadiene resin, or a combination thereof.

[0025] PH regulator 2.0%~3.7%: adjusts the acidity of the flux and affects its activity. Triethanolamine is preferred;

[0026] Surfactant 1.8% to 4.2%: Reduces surface tension and improves wetting and spreading. OP-10 or GE-511 are optional.

[0027] Phenolic antioxidant 1.0% to 2.0%: Choose butylated hydroxytoluene (BHT) or hydroquinone (HQ). Its key mechanism of action is that during the soldering heating stage (approximately 150-250°C), it effectively scavenges free radicals, inhibits the oxidation of organic components in the solder and flux, and maintains solder activity and fluidity. Near the peak soldering temperature (~250°C) and during the subsequent cooling process, it undergoes thermal decomposition and volatilization, leaving almost no residue. This characteristic is the key to solving the problem of post-solder residue.

[0028] Corrosion inhibitor 1.4% to 1.8%: protects the metal surface after welding. Benzotriazole (BTA) is preferred.

[0029] The core innovation of this flux lies in the specific selection and application of phenolic antioxidants (BHT or HQ). Their decomposition temperatures are highly compatible with the soldering process window (BHT decomposes at approximately 250-300°C, and HQ decomposes at approximately 285°C). This allows them to effectively exert their high-temperature antioxidant properties while also enabling sufficient volatilization and removal during the post-soldering phase. This is the technical foundation for achieving this breakthrough in "low residue." Furthermore, their excellent antioxidant properties, synergistic with the effects of Bi and Ni, ensure excellent solder paste wettability under low-silver conditions.

[0030] Preparation of tin-based powder solder: According to the ratio of different tin-based powder solders, weigh the weight of each metal element component separately, and the total weight percentage of each part is 100%.

[0031] Specifically, sufficient Ag and appropriate Sn are weighed according to the ratio of tin-based powder solder, placed in a boron nitride crucible, and melted in a vacuum induction melting furnace (filled with argon protection). After the alloy liquid is uniform, it is allowed to stand and air-cooled to obtain the SnAg master alloy.

[0032] Specifically, sufficient Cu and an appropriate amount of Sn are weighed according to the ratio of tin-based powder solder, placed in a boron nitride crucible, and melted in a vacuum induction melting furnace (filled with argon protection). After the alloy liquid is uniform, it is allowed to stand and air-cooled to obtain the intermediate alloy SnCu.

[0033] Specifically, sufficient Ni and an appropriate amount of Sn are weighed according to the ratio of tin-based powder solder, placed in a boron nitride crucible, and melted in a vacuum induction melting furnace (filled with argon protection). After the alloy liquid is uniform, it is allowed to stand and air-cooled to obtain the intermediate alloy SnNi.

[0034] Then, according to the ratio of tin-based powder solder, the remaining component raw materials Sn and Bi are weighed and added to a boron nitride crucible, and then the master alloy is added and smelted in a vacuum induction gas atomization powder making equipment. After the alloy liquid is uniform, tin-based alloy powder is prepared by gas atomization (argon is used as atomizing gas), and then the powder is sieved through a 200-mesh sieve using a rotary vibration sieving instrument.

[0035] Preparation of low-silver tin-based solder paste: Weigh an appropriate amount of solvent into a beaker according to the mixing ratio. Adjust the heating mantle temperature to 100°C-120°C. Start a laboratory electric mixer and add the appropriate amount of rosin. Heat and stir until the rosin is completely dissolved. Lower the temperature to 60°C-80°C, add the activator, and continue stirring for 30 minutes. Add a pH adjuster to adjust the pH, then lower the temperature to 50°C-60°C. First, add the thixotropic agent and stir until completely dissolved. Then, add the film-forming agent and surfactant and stir for 30 minutes to fully disperse them. Lower the temperature to 40°C-50°C, add the antioxidant and corrosion inhibitor, stir at low speed for 30 minutes, and then emulsify at high speed for 30 minutes to improve the uniformity and stability of the system. After cooling to room temperature, grind the mixture three times using a three-roll mill to fully refine and mix the components. Allow to stand for degassing to obtain the flux.

[0036] Solder Paste Mixing: Weigh 85% to 87.5% of the prepared tin-based solder powder and 12.5% ​​to 15% of the prepared flux (by mass) into a mixing container. Stir until a uniform, smooth, bubble-free paste forms. Seal the resulting solder paste and store at a low temperature (2-10°C).

[0037] Beneficial effects of the present invention:

[0038] The present invention uses the above-mentioned specific flux formula, especially the innovative application of phenolic antioxidants (butylated hydroxytoluene or hydroquinone), to synergistically optimize the low-silver tin-based alloy components (containing Bi and Ni), successfully solving the technical problems of "high residue" and "insufficient wettability" of low-silver lead-free solder paste, and providing a high-performance, low-cost, and highly reliable green welding material. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the process flow chart for preparing tin-based solder paste.

[0040] Figure 2 This is the ultrasonic nondestructive testing image of the solder paste after soldering in Example 1.

[0041] Figure 3 This is the ultrasonic nondestructive testing picture of the solder paste after soldering in Example 2.

[0042] Figure 4 This is the ultrasonic nondestructive testing image of the solder paste after soldering in Example 3.

[0043] Figure 5 This is the ultrasonic nondestructive testing image of the solder paste after soldering in Example 4.

[0044] Figure 6 This is the ultrasonic nondestructive testing picture of the solder paste after soldering in Example 5.

[0045] Figure 7 This is the ultrasonic nondestructive testing picture of the solder paste after soldering in Example 6.

[0046] Figure 8 This is the ultrasonic nondestructive testing image of the solder paste after soldering in comparative example 1.

[0047] Figure 9 This is the ultrasonic nondestructive testing image of the solder paste after soldering in comparative example 2. DETAILED DESCRIPTION

[0048] Example 1

[0049] According to the mass ratio of the elemental composition of the tin-based powder solder in Table 1, first weigh a sufficient amount of Ag and an appropriate amount of Sn, add them to a boron nitride crucible, and smelt them in a vacuum induction melting furnace. After the metal liquid is melted evenly, air cool it to obtain a uniform alloy ingot SnAg; similarly, prepare intermediate alloy ingots SnCu and SnNi; then weigh an appropriate amount of the remaining Sn and Bi according to the ratio of the tin-based powder solder in Table 1, put them into a boron nitride crucible, and then put the intermediate alloy ingots SnAg, SnCu and SnNi into it, and smelt them in a vacuum induction gas atomization powder making equipment to obtain a uniform metal liquid, and then use gas atomization to prepare powder. High-purity argon (2.0MPa~5.0MPa) is selected as the high-pressure gas. The prepared powder solder is sieved using a rotary vibration powder sifter to obtain a 200-mesh powder solder.

[0050] According to the mass proportion of the flux composition in Table 2, first weigh appropriate amounts of tripropylene glycol butyl ether, diethylene glycol, and triethylene glycol in a beaker, adjust the temperature of the heating mantle to 110°C, turn on the experimental electric stirrer, add the weighed appropriate amounts of KE-604 rosin and hydrogenated rosin, and heat and stir until the rosin is completely dissolved. After lowering the temperature to 70°C, add succinic acid and continue stirring for 30 minutes, add triethanolamine to adjust the pH value, and then lower the temperature to 55°C. First, add hydrogenated castor oil and stir to completely dissolve it, then add polymethyl methacrylate, butadiene resin and GE-511, stir for 30 minutes to fully disperse it, then lower the temperature to 45°C, add butylated hydroxytoluene and benzotriazole, stir at low speed for 30 minutes, and then use an emulsifier to emulsify at high speed for 30 minutes. After cooling to room temperature, use a three-roll mill to grind 3 times and let it stand to obtain the flux.

[0051] Tin-based solder paste was prepared by weighing 85% by weight of tin-based solder powder and 15% by weight of flux in a beaker and stirring until a uniform paste was formed.

[0052] Example 2

[0053] In this embodiment, the element composition mass ratio of the tin-based powder solder and the flux composition mass ratio are respectively proportioned according to Table 1 and Table 2. The preparation method of the tin-based powder solder and the flux is the same as that of Example 1. Then, 85.5% of the tin-based powder solder and 14.5% of the flux by mass are weighed in a beaker and stirred until a uniform paste is formed to prepare a tin-based solder paste.

[0054] Example 3

[0055] In this embodiment, the element composition mass ratio of the tin-based powder solder and the flux composition mass ratio are respectively proportioned according to Table 1 and Table 2. The preparation method of the tin-based powder solder and the flux is the same as that of Example 1. Then, 86% of the tin-based powder solder and 14% of the flux are weighed in a beaker and stirred until a uniform paste is formed to prepare a tin-based solder paste.

[0056] Example 4

[0057] In this embodiment, the element composition mass ratio of the tin-based powder solder and the flux composition mass ratio are respectively proportioned according to Table 1 and Table 2. The preparation method of the tin-based powder solder and the flux is the same as that of Example 1. Then, 86.5% of the tin-based powder solder and 13.5% of the flux by mass are weighed in a beaker and stirred until a uniform paste is formed to prepare a tin-based solder paste.

[0058] Example 5

[0059] In this embodiment, the element composition mass ratio of the tin-based powder solder and the flux composition mass ratio are respectively proportioned according to Table 1 and Table 2. The preparation method of the tin-based powder solder and the flux is the same as that of Example 1. Then, 87% of the tin-based powder solder and 13% of the flux by mass are weighed in a beaker and stirred until a uniform paste is formed to prepare a tin-based solder paste.

[0060] Example 6

[0061] In this embodiment, the element composition mass ratio of the tin-based powder solder and the flux composition mass ratio are respectively proportioned according to Table 1 and Table 2. The preparation method of the tin-based powder solder and the flux is the same as that of Example 1. Then, 87.5% of the tin-based powder solder and 12.5% ​​of the flux by mass are weighed in a beaker and stirred until a uniform paste is formed to prepare a tin-based solder paste.

[0062] Comparative Example 1

[0063] In this comparative example, the elemental composition ratios of the tin-based solder powder and flux were proportioned according to Tables 1 and 2, respectively. The preparation methods for the tin-based solder powder and flux were the same as in Example 1. Note that no Bi or Ni elements were added to the tin-based solder in this comparative example, and butylated hydroxytoluene was used as an antioxidant in the flux. A tin-based solder paste was then prepared by weighing 85% tin-based solder powder and 15% flux by weight into a beaker and stirring until a uniform paste formed.

[0064] Comparative Example 2

[0065] In this comparative example, the elemental composition ratios of the tin-based solder powder and flux were proportioned according to Tables 1 and 2, respectively. The preparation methods for the tin-based solder powder and flux were the same as in Example 1. Note that no Bi or Ni elements were added to the tin-based solder in this comparative example, and butylated hydroxytoluene was used as an antioxidant in the flux. A tin-based solder paste was then prepared by weighing 85% tin-based solder powder and 15% flux by weight into a beaker and stirring until a uniform paste formed.

[0066] Table 1: Element composition mass ratio of tin-based powder solders of Examples 1 to 6 and Comparative Examples 1 to 2

[0067]

[0068] Table 2: Mass ratio of flux composition of Examples 1 to 6 and Comparative Examples 1 to 2

[0069]

[0070]

[0071] Test results

[0072] 1. Wetting angle test: Refer to ASTM D7334 standard, use a contact angle tester, and place the solder paste on the copper substrate for testing in a nitrogen atmosphere at 250°C.

[0073] 2. Elongation test: Refer to the standard IPC-TM-650 2.4.44, and place the solder paste on the copper substrate in a nitrogen atmosphere at 250°C for measurement and calculation.

[0074] 3. Post-soldering residue: Place solder paste on a copper substrate at 250°C in a nitrogen atmosphere. After the solder paste melts and cools to room temperature, observe the results.

[0075] 4. Soldering rate test: Use ultrasonic imaging non-destructive testing system to test the copper substrate after welding.

[0076] Table 3: Test results of Examples 1 to 6 and Comparative Examples 1 to 2

[0077]

[0078] From the measured wetting angle data, it can be seen that the embodiments with higher Bi and Ni contents have smaller wetting angles and better wettability than the embodiments with lower Bi and Ni addition amounts. Bi reduces the surface tension of the solder paste, and Ni inhibits interfacial oxidation, thereby synergistically optimizing wettability. Comparative Examples 1 and 2 do not contain Bi and Ni, and their wetting angles are larger and their wettability is poor. In addition, Comparative Example 2 contains a higher Ag content, which results in an increased melting point of the solder, poor fluidity, an increased wetting angle, poor wettability, and a higher cost.

[0079] The Bi and Ni contents in Examples 4 and 6 are higher, and the measured expansion rates are also higher. Adding Bi elements to the solder can reduce the viscosity of the solder and improve the fluidity of the solder. Ni elements can reduce the formation of oxides and improve the spreading uniformity of the solder. Compared with the comparative example, it can be clearly seen that the addition of Bi and Ni in the examples improves the expansion rate.

[0080] Ultrasonic imaging nondestructive testing system was used to test the solder paste soldered copper sheets of each embodiment and comparative example. The obtained soldering rate represents the proportion of effective soldering area. The two-dimensional ultrasonic nondestructive testing image can clearly reflect the welding integrity and reliability of the welded base material. The closer to the dark blue part in the image, the tighter the weld, while the white and red parts may have defects such as unwelded, inclusions or pores. From the test results, the soldering rate measured in Example 4 and Example 6 is the highest, and the welding effect is the best. Figure 5 and Figure 7 It can be seen that there are fewer defects after welding and the welding effect is good; while for the comparative example, large defects after welding can be seen. The main reason is that the solder paste has poor wettability and the solder paste is not evenly spread during welding.

[0081] The antioxidants used in the flux of the examples are phenolic antioxidants such as butylated hydroxytoluene or hydroquinone, while the antioxidant used in the comparative examples is triethyl phosphite. Comparison of post-weld residue results shows that the phenolic antioxidant effectively reduces post-weld residue. Phenolic antioxidants decompose at temperatures similar to the solder paste temperature, effectively inhibiting oxidation reactions and reducing oxide production. They are also volatile during the soldering process, leaving virtually no residue.

[0082] Through further analysis and summary of the above embodiments and comparative examples, the present invention has the following characteristics:

[0083] (1) Application of phenolic antioxidants. In the field of welding materials, although there are solder pastes containing phenolic substances in the prior art, most of them are used as active agents or film-forming agents rather than utilizing their thermal decomposition properties. The present invention combines the antioxidant properties and low residual properties of phenolic substances and uses phenolic substances as antioxidants;

[0084] (2) Matching of phenolic antioxidants with decomposition temperature. Antioxidants in the prior art (such as phosphites, benzotriazole, etc.) generally have the problem of incomplete decomposition or high residual rate. Although some patent documents mention the problem of "low residue" in solder paste, none of them achieve this goal through the thermal decomposition characteristics of antioxidants. Instead, they rely on solvent preparation or cleaning processes, which has limited effect and increases costs. The present invention finds that the decomposition temperature of butylated hydroxytoluene and hydroquinone is (250-285℃) and highly matches the welding temperature (~250℃). This characteristic enables them to effectively inhibit oxidation during the welding stage and completely decompose and volatilize during the cooling process, fundamentally solving the problem of post-weld residue.

[0085] (3) Synergistic optimization of Bi-Ni elements and Bi+Ni+phenolic antioxidants to improve solder paste performance in multiple aspects;

[0086] (4) The preparation of solder paste with low silver content is achieved. Existing low-silver solder pastes (such as Sn-0.3Ag-0.7Cu) suffer from decreased wettability and poor mechanical properties after reducing the silver content. Through collaborative design, the present invention achieves excellent wettability and high reliability even when the Ag content is reduced to 0.35-0.6%.

[0087] In summary, the present invention effectively solves the problem of high post-soldering residue in low-silver lead-free solder paste by innovatively selecting a specific phenolic antioxidant (butylated hydroxytoluene or hydroquinone) in the flux formula, and synergistically optimizes the alloy components to achieve good wettability and high reliability at a low silver content, which has significant practical value.

Claims

1. A low-silver lead-free tin-based solder paste, characterized in that: The solder paste is made of 85wt% to 87.5wt% of tin-based powder solder and 12.5wt% to 15wt% of flux; the flux includes 30.4wt% to 35.0wt% of rosin, 41.2wt% to 45.2wt% of solvent, 5.0wt% to 7.4wt% of activator, 5.4wt% to 7.0wt% of thixotropic agent, 3.2wt% to 4.6wt% of film-forming agent, 2.0wt% to 3.7wt% of pH regulator, 1.8wt% to 4.2wt% of surfactant, 1.0wt% to 2.0wt% of phenolic antioxidant and 1.4wt% to 1.8wt% of corrosion inhibitor; The phenolic antioxidant is butylated hydroxytoluene or hydroquinone; The tin-based powder solder contains 0.35 wt% to 0.6 wt% of silver, 0.5 wt% to 0.8 wt% of copper, 1.0 wt% to 4.0 wt% of bismuth, 0.05 wt% to 0.08 wt% of nickel, and the balance is tin.

2. The low-silver lead-free tin-based solder paste according to claim 1, characterized in that The solvent is composed of one or more of tripropylene glycol butyl ether, diethylene glycol, triethylene glycol, glycerol, and isopropyl ketone.

3. The low-silver lead-free tin-based solder paste according to claim 1, characterized in that The active agent is composed of one or more of succinic acid, oxalic acid, lauric acid and sebacic acid.

4. The low-silver lead-free tin-based solder paste according to claim 1, characterized in that The film-forming agent is composed of one or more of polymethyl methacrylate, acrylic resin, and butadiene resin.

5. The low-silver lead-free tin-based solder paste according to claim 1, characterized in that The surfactant is OP-10 or GE-511.

6. The low-silver lead-free tin-based solder paste according to claim 1, characterized in that: The thixotropic agent is hydrogenated castor oil; The pH regulator is triethanolamine; The corrosion inhibitor is benzotriazole.

7. The low-silver lead-free tin-based solder paste according to claim 1, characterized in that: The rosin is composed of one or more of KE-604 rosin, polymerized rosin and hydrogenated rosin.

8. A method for preparing a low-silver, lead-free, tin-based solder paste according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1 Preparation of tin-based powder solder; Preparation of S2 flux; S3 solder paste mixing; The step S1 comprises: S1.1 Preparation of Sn-Ag, Sn-Cu, and Sn-Ni master alloy ingots: Weigh sufficient amounts of Ag, Cu, Ni, and an appropriate amount of Sn according to the ratio of tin-based solder powder, place them in a boron nitride crucible, and melt them in a vacuum induction melting furnace under argon protection. After the alloy liquid is uniform, let it stand and air-cool to obtain the corresponding master alloy ingot; S1.2 Gas Atomization Powdering: Weigh the remaining raw materials Sn and Bi according to the ratio of tin-based powder solder and add them to a boron nitride crucible. Then add the Sn-Ag, Sn-Cu, and Sn-Ni master alloys prepared in step S1.

1. Melt them in a vacuum induction gas atomization powdering equipment, and then perform gas atomization powdering. S1.3 Powder sieving: Use a rotary vibrating sieving instrument to sieve the tin-based alloy powder obtained in step S1.2; The step S2 comprises: S2.1 Weigh an appropriate amount of solvent according to the ratio into a beaker, heat and stir, add an appropriate amount of rosin, and continue heating and stirring until the rosin is completely dissolved; S2.2 Lower the temperature and add the active agent while continuing to stir; S2.3 Add pH regulator to adjust pH value; S2.4 Lower the temperature, add the thixotropic agent, and stir until it is completely dissolved; S2.5 Add film-forming agent and surfactant and stir to fully disperse them; S2.6 Lower the temperature, add phenolic antioxidant and corrosion inhibitor, stir at low speed, and then use an emulsifier to emulsify at high speed; S2.7 After cooling to room temperature, grind using a three-roll grinder and allow to stand to obtain flux; The step S3 comprises: 85 wt% to 87.5 wt% of the tin-based powder solder prepared in step S1 and 12.5 wt% to 15 wt% of the flux prepared in step S2 are weighed, stirred to form a uniform paste, and stored at low temperature to prepare the low-silver lead-free tin-based solder paste.

9. The preparation method according to claim 8, characterized in that: The gas atomization powder making in step S1.2 includes: using high-purity argon as atomizing gas, and controlling the gas pressure at 2.0 MPa to 5.0 MPa.

10. The preparation method according to claim 8 or 9, characterized in that: The heating and stirring in step S2.1 includes: adjusting the temperature of the electric heating mantle to 100°C to 120°C and turning on the electric stirrer for the experiment; In step S2.2, the temperature is lowered to 60°C to 80°C, the active agent is added, and stirring is continued for 30 minutes; In step S2.4, the temperature is lowered to 50°C to 60°C; In step S2.6, the temperature is lowered to 40°C to 50°C.

Citation Information

Patent Citations

  • High-reliability halogen-free and lead-free soldering paste and preparation method thereof

    CN114367760A

  • Silver nanowire modified tin-silver-copper composite soldering paste and preparation method thereof

    CN115488546A

  • Tin-silver-copper series high-temperature die bonding solder paste with superfine particle size and preparation method thereof

    CN118268757A

Cited By

  • MAX phase enhanced three-dimensional net-shaped tin-based lead-free solder and preparation method thereof

    CN121267458A

  • A max phase reinforced three-dimensional network tin-based lead-free solder and a preparation method thereof

    CN121267458B

  • Cu-Sn-Ti series sintering soldering paste for active metal brazing ceramic copper-clad substrate and preparation method of Cu-Sn-Ti series sintering soldering paste

    CN122125403A