An insulating film, a method for manufacturing the same, and an application thereof to a battery case
By using a layered insulating film structure, with the inner and outer layers cured by photoinitiator inks in different proportions, the problems of insufficient shear strength, insulation and thermal conductivity of existing lithium-ion battery casing insulating films are solved, realizing efficient and low-cost insulating film preparation and improving the safety and aging resistance of battery casings.
Patent Information
- Application Number
- CN202510526249.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-04-25
AI Technical Summary
The existing blue film on lithium-ion battery casings has poor shear strength and insulation and fireproofing properties, and low thermal conductivity, which leads to significant safety hazards during fast charging of the battery cells. In addition, the coating process is complicated and costly, and it is impossible to increase the thickness of the insulating film to enhance insulation performance while ensuring aging resistance.
An insulating film structure with multiple layers is adopted. The inner layer is photocured with a first ink containing a high amount of long-wave photoinitiator, and the outer layer is photocured with a second ink containing a small amount of long-wave photoinitiator. By controlling the content ratio of photoinitiator, the photocuring efficiency and cross-linking degree are ensured, forming an insulating film with high shear strength and anti-aging ability.
The thickness and insulation performance of the insulating film were increased, which enhanced the safety and production efficiency of the battery casing, reduced costs, and improved the aging resistance and shear strength of the insulating film.
Smart Images

Figure CN120545641B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of insulating film and battery technology, specifically to an insulating film, its preparation method, and its application in battery casing. Background Technology
[0002] Lithium-ion batteries have advantages such as high specific capacity, high operating voltage, long cycle life, portability, safety, environmental friendliness, and low environmental pollution, and are widely used in various products. Conventional lithium-ion battery casings are covered with a blue insulating protective film, which serves to insulate and protect the battery cells, reduce scratches from impacts, and improve the shock absorption of the cells within the module. However, this type of blue film has poor shear strength and insulation / fireproofing properties, and its low thermal conductivity is not conducive to heat conduction on the cell surface. This hinders cell cooling during fast charging, posing a significant safety hazard. Furthermore, the blue film coating process is prone to defects such as bulging, leading to a decrease in yield. Different cell sizes require redesigning the blue film size and coating fixtures, a cumbersome and costly process.
[0003] Addressing the shortcomings of existing blue film coating technology, a method for in-situ forming of insulating films on the surface of battery casings using UV printing inks has been proposed. This method is unrestricted by the type and size of the battery casing, effectively improving production efficiency and reducing costs. The insulating film used for battery casings requires a certain thickness to ensure its buffering and insulation properties; it cannot be too thin. However, with conventional UV printing inks, the wavelength of ultraviolet light entering the coating decreases with increasing coating thickness during the curing process. This prevents the effective promotion of free radical generation by photoinitiators with specific absorption wavelength ranges, leading to incomplete cross-linking reactions between internal photocurable monomers and affecting the aging resistance of the printed insulating film. Furthermore, it is impossible to improve the insulating film's insulation performance by further increasing its thickness while maintaining its aging resistance. Summary of the Invention
[0004] To address the aforementioned problems, this invention provides an insulating film, its preparation method, and its application in battery casings. The inner layer (first film layer) of the insulating film is prepared using a first ink with a high content of long-wavelength photoinitiator, while the outer layer (second film layer) is prepared using a second ink with a relatively low content of long-wavelength photoinitiator. This ensures that the attenuation of light wavelength during photocuring does not affect the curing effect of the inner layer and facilitates faster photocuring efficiency. The resulting insulating film not only possesses high shear strength and superior anti-aging capabilities but also allows for further increases in the thickness of the insulating protective film, meeting the application requirements for high insulation.
[0005] Specifically, the following technical solutions are provided:
[0006] The first aspect of the present invention provides an insulating film comprising a first film layer and a second film layer stacked thereon; the first film layer is obtained by photocuring a first ink, and the second film layer is obtained by photocuring a second ink.
[0007] Both the first ink and the second ink contain photoinitiators, which include long-wavelength photoinitiators and short-wavelength photoinitiators. The mass percentage of long-wavelength photoinitiators in the first ink is greater than that in the second ink.
[0008] Further, the thickness of the insulating film is preferably 50-500 μm, and the thickness of the first film layer is preferably 30%-55% of the total thickness of the insulating film; more preferably, the thickness of the insulating film is 60-500 μm, and the thickness of the first film layer is 30%-50% of the total thickness of the insulating film.
[0009] Furthermore, the maximum absorption wavelength of the long-wavelength photoinitiator is greater than that of the short-wavelength photoinitiator, wherein the absorption wavelength range of the long-wavelength photoinitiator is within the range of 260-480nm, and the absorption wavelength range of the short-wavelength photoinitiator is within the range of 230-340nm.
[0010] Furthermore, in the first ink, the long-wave photoinitiator accounts for 30%-85% of the total mass of the photoinitiator, and in the second ink, the long-wave photoinitiator accounts for 10%-40% of the total mass of the photoinitiator.
[0011] Further, both the first ink and the second ink contain the following components by mass parts: 0.5-20 parts of acrylate soft monomers, 1-40 parts of acrylate monomers containing multiple carbon-carbon double bonds, 0.5-20 parts of epoxy acrylates, 0.5-20 parts of flame-retardant monomers, 0.5-10 parts of photoinitiator, 0.5-20 parts of low molecular weight acrylates, 0.5-20 parts of thermally conductive fillers, and 0.5-5 parts of nano-color paste; preferably, the molecular weight of the low molecular weight acrylates is less than 120.
[0012] Furthermore, the acrylate soft monomers include one or more of butyl acrylate, isooctyl acrylate, isoamyl acrylate, and octyl acrylate.
[0013] Furthermore, the acrylate monomer containing multiple carbon-carbon double bonds includes one or more of trimethylolpropionate, triethylolpropionate, tributylolpropionate, dimethylolpropionate, diethylolpropionate, and dibutylolpropionate.
[0014] Furthermore, the epoxy acrylate includes one or more of methyl-modified epoxy acrylate, ethyl-modified epoxy acrylate, and propyl-modified epoxy acrylate.
[0015] Furthermore, the flame-retardant monomer includes at least one of methyl metaphosphate modified acrylate and ethyl metaphosphate modified acrylate; such flame-retardant monomers can be uniformly and stably dispersed.
[0016] Further, the long-wavelength photoinitiator includes one or more of ethyl 2,4,6-trimethylbenzoylphenylphosphonate (absorption peak at 270-370 nm), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (absorption peak at 269-393 nm), and bibenzoyl (absorption peak at 300-480 nm); the short-wavelength photoinitiator includes one or more of 2-methyl-2(4-morpholino)-1(4-(methylthio)phenyl)-1-propanone (absorption peak at 232-307 nm), 1-hydroxycyclohexylphenyl ketone (absorption peak at 244-326 nm), and 2-hydroxy-2-methyl-1-phenylpropanone (absorption peak at 244-331 nm).
[0017] Furthermore, the low molecular weight acrylate includes one or more of methyl acrylate, ethyl acrylate, and methyl methacrylate.
[0018] Furthermore, the thermally conductive filler includes one or more of silicon nitride, zinc oxide, silicon micro powder, boron nitride, aluminum oxide, and magnesium oxide.
[0019] Furthermore, both the first ink and the second ink contain the following components by mass parts: 1-20 parts butyl acrylate, 1-20 parts trimethylolpropene triacrylate, 1-20 parts dimethylolpropene diacrylate, 1-20 parts epoxy acrylate, 1-20 parts metaphosphate-modified acrylate, 1-10 parts photoinitiator, 1-20 parts methyl acrylate, 1-20 parts thermally conductive filler, and 1-5 parts nano-color paste; and the long-wave photoinitiator in the first ink accounts for 35%-85% of the total mass of the photoinitiator, while the long-wave photoinitiator in the second ink accounts for 10%-35% of the total mass of the photoinitiator.
[0020] A second aspect of the present invention provides a method for preparing the insulating film described in the first aspect, comprising the following steps:
[0021] (1) Provide a first ink and a second ink, and use the first ink to form a first UV printing layer by UV printing, and then use the second ink to form a second UV printing layer on the first UV printing layer by UV printing;
[0022] (2) The insulating film is obtained by curing under ultraviolet light.
[0023] Further, in step (1), during the UV printing step: the energy density of the ultraviolet light is 190.4-238 mJ / cm².2 .
[0024] Furthermore, in step (2), the energy density of the ultraviolet light is 26400-34000 mJ / cm². 2 The curing temperature is 30-50℃ and the curing time is 2-10s.
[0025] A third aspect of the present invention provides a battery casing, comprising a casing and an insulating film covering the surface of the casing, wherein the insulating film is the insulating film described in the first aspect or the insulating film prepared by the preparation method described in the second aspect; the insulating film comprises a first film layer and a second film layer stacked thereon, wherein the side of the first film layer away from the second film layer is attached to the surface of the casing.
[0026] Furthermore, the first film layer is obtained by photocuring the first ink on the surface of the housing.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0028] This invention provides an insulating film that can be prepared in situ by forming first and second inks on the surface of objects to be protected of different sizes and shapes. The inner layer (first film layer) of the insulating film is photocured by the first ink with a high content of long-wavelength photoinitiator, and the outer layer (second film layer) is photocured by the second ink with a relatively low content of long-wavelength photoinitiator. By utilizing the different proportions of long-wavelength and short-wavelength photoinitiators in the different inks, the first ink located in the inner layer can still be cured efficiently even when the light wavelength is attenuated, thereby effectively improving the crosslinking degree and photocuring efficiency of the inner layer of the insulating film (the first film layer that adheres to the battery casing).
[0029] The insulating film preparation method provided by this invention is simple and efficient. The insulating film not only has high shear strength and better anti-aging ability, but also can further increase the thickness of the insulating protective film (the maximum printing thickness can be increased by at least 70%), meeting the application requirements of high insulation. Attached Figure Description
[0030] Figure 1 A schematic diagram of the structure of an insulating film provided by the present invention;
[0031] Figure 2 A schematic diagram of the structure of a battery casing provided by the present invention;
[0032] Icons: 01 represents the first membrane layer, 02 represents the second membrane layer, and 1 represents the shell. Detailed Implementation
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. "Comprising" or "containing" as used herein means that it may include or contain other components in addition to the stated components. "Comprising" or "containing" as used herein may also be replaced with the closed form "is" or "consisting of".
[0034] As described in the background art, when an insulating film is prepared on the surface of a battery casing using a single UV printing ink, the wavelength of ultraviolet light entering during the photocuring process decreases with the increase of coating thickness. This makes it impossible to effectively promote the generation of free radicals by photoinitiators with specific absorption wavelength ranges, resulting in incomplete cross-linking reactions between the photocurable monomers at the bottom layer, which deteriorates the aging resistance of the insulating film. It is also impossible to improve the insulation performance of the insulating film by further increasing the thickness of the insulating film while ensuring its aging resistance.
[0035] To address the aforementioned problems, embodiments of the present invention provide an insulating film comprising a first film layer and a second film layer stacked together, wherein the first film layer is obtained by photocuring a first ink, and the second film layer is obtained by photocuring a second ink.
[0036] Both the first ink and the second ink contain photoinitiators, which include long-wavelength photoinitiators and short-wavelength photoinitiators. The mass percentage of long-wavelength photoinitiators in the first ink is greater than that in the second ink.
[0037] To address the issues of low cross-linking degree of the underlying layer and poor aging performance of the insulating film when using a single UV printing ink, and because the difference in photocuring effect increases with the increase of the insulating film thickness, it is impossible to further increase the thickness of the insulating film to obtain a high-insulation protective film. Based on this, the present invention provides an insulating film prepared by in-situ molding of a first ink and a second ink on the surface of an object to be protected (e.g., the surface of a battery casing). The first ink is used to prepare the inner layer (first film layer), and the second ink is used to prepare the outer layer (second film layer). By controlling the content of long-wavelength photoinitiator in the first ink to be greater than that in the second ink, during the photocuring process, the second ink on the outer side can effectively absorb short-wavelength ultraviolet light, promoting the cross-linking and curing of monomers in the second ink to form the second film layer. Simultaneously, as ultraviolet light diffuses and its wavelength increases in the thickness direction, the large amount of long-wavelength photoinitiator in the first ink on the inner side can effectively absorb the long wavelength, thereby decomposing to generate free radicals that promote the full cross-linking of the bottom monomers. This allows both the inner and outer sides of the insulating film to be fully cured and cross-linked, improving the aging resistance of the insulating film. Furthermore, it eliminates the need for layered curing, improving photocuring efficiency while enhancing the bonding force between different film layers, further improving the aging resistance and insulation performance of the insulating film.
[0038] In this invention, the first film layer of the insulating film is the inner film layer of the insulating film, and the second film layer is the outer film layer of the insulating film. The side of the first film layer away from the second film layer is in contact with the surface of the object to be protected.
[0039] In this invention, the thickness of the insulating film is preferably 50-500 μm, and the thickness of the first film layer is preferably 30%-55% of the total thickness of the insulating film; more preferably, the thickness of the insulating film is 60-500 μm, such as 60 μm, 80 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, etc., including but not limited to the thickness values listed above, and the thickness of the first film layer is 30%-50% of the total thickness of the insulating film, such as 30%, 35%, 40%, 45%, 50%, etc.
[0040] In this invention, the maximum absorption wavelength of the long-wavelength photoinitiator is greater than that of the short-wavelength photoinitiator. The absorption wavelength range of the long-wavelength photoinitiator is within the range of 260-480 nm, and the absorption wavelength range of the short-wavelength photoinitiator is within the range of 230-340 nm.
[0041] In this invention, the long-wave photoinitiator in the first ink accounts for 30%-85% of the total mass of the photoinitiator, such as 30%, 40%, 50%, 60%, 70%, 80%, 85%, etc., including but not limited to the mass percentages listed above. The long-wave photoinitiator in the second ink accounts for 10%-40% of the total mass of the photoinitiator, such as 10%, 20%, 30%, 40%, etc., including but not limited to the mass percentages listed above.
[0042] In this invention, both the first ink and the second ink contain the following components in parts by weight: 0.5-20 parts of acrylate soft monomers (e.g., 0.5 parts, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, etc., including but not limited to the listed parts), and 1-40 parts of acrylate monomers containing multiple carbon-carbon double bonds (e.g., 1 part, 4 parts, 8 parts, 12 parts, 16 parts, 20 parts, 24 parts). 28 parts, 32 parts, 36 parts, 40 parts, etc., including but not limited to the listed parts); 0.5-20 parts of epoxy acrylate (e.g., 0.5 parts, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, etc., including but not limited to the listed parts); 0.5-20 parts of flame retardant monomer (e.g., 0.5 parts, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, etc., including but not limited to the listed parts); 28 parts, 32 parts, 36 parts, 40 parts, etc. ... 18 parts, 20 parts, etc., including but not limited to the listed parts); 0.5-10 parts of photoinitiator (e.g., 0.5 parts, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc., including but not limited to the listed parts); 0.5-20 parts of low molecular weight acrylate (e.g., 0.5 parts, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, etc., including but not limited to the listed parts); (Not limited to the listed parts), thermally conductive filler 0.5-20 parts (e.g., 0.5 parts, 2 parts, 4 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, etc., including but not limited to the listed parts), nano pigment 0.5-5 parts (e.g., 0.5 parts, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc., including but not limited to the listed parts); preferably, the molecular weight of the low molecular weight acrylate is less than 120.
[0043] In this invention, the first ink and the second ink are mainly formulated from acrylate monomers. The acrylate monomers containing multiple carbon-carbon double bonds form a first cross-linked network with a three-dimensional network structure through free radical polymerization of the carbon-carbon double bonds. Furthermore, the introduced epoxy acrylates can further form a second cross-linked network through epoxy ring-opening reactions. Under the synergistic effect of the first and second cross-linked networks, the insulating film with high cross-linking density exhibits superior aging resistance and insulation properties. Simultaneously, the first and second inks incorporate appropriate amounts of soft acrylate monomers to improve the flexibility of the insulating film, enabling it to better resist external stress and improve the stability of its electrical properties under deformation. In addition, given the poor fire resistance and thermal conductivity of current insulating films used on battery casing surfaces, posing significant safety hazards, this invention introduces flame-retardant monomers and conductive fillers into the first and second inks to enhance the fire resistance and thermal conductivity of the insulating film. Furthermore, to improve the dispersibility of the conductive fillers in the ink and the ink's processability, an appropriate amount of low molecular weight acrylates is introduced to reduce the ink viscosity. The synergistic effect of the above components results in an insulating film formed by photocuring the first and second inks, which not only has excellent anti-aging properties and insulation, but also better fire resistance and thermal conductivity, making it particularly suitable for protective films for battery casings.
[0044] In this invention, acrylate soft monomers include, but are not limited to, one or more of butyl acrylate, isooctyl acrylate, isoamyl acrylate, and octyl acrylate.
[0045] In this invention, acrylate monomers containing multiple carbon-carbon double bonds include, but are not limited to, one or more of trimethylolpropionate, triethylolpropionate, tributylolpropionate, dimethylolpropionate, diethylolpropionate, and dibutylolpropionate.
[0046] In this invention, epoxy acrylates include, but are not limited to, one or more of methyl-modified epoxy acrylates, ethyl-modified epoxy acrylates, and propyl-modified epoxy acrylates, such as methyl-modified epoxy acrylate, ethyl-modified epoxy acrylate, etc.
[0047] In this invention, the flame-retardant monomer includes at least one of methyl metaphosphate modified acrylate and ethyl metaphosphate modified acrylate, such as methyl metaphosphate modified methyl acrylate and methyl metaphosphate modified ethyl acrylate. These flame-retardant monomers exist stably in the insulating film through the polymerization reaction of carbon-carbon double bonds, and can decompose at high temperature to produce a covering material that isolates air and achieves a flame-retardant effect.
[0048] In this invention, long-wavelength photoinitiators include, but are not limited to, one or more of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester (absorption peak at 270-370 nm), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (absorption peak at 269-393 nm), and bibenzoyl (absorption peak at 300-480 nm); short-wavelength photoinitiators include, but are not limited to, one or more of 2-methyl-2(4-morpholino)-1(4-(methylthio)phenyl)-1-propanone (absorption peak at 232-307 nm), 1-hydroxycyclohexylphenyl ketone (absorption peak at 244-326 nm), and 2-hydroxy-2-methyl-1-phenylpropanone (absorption peak at 244-331 nm).
[0049] In this invention, low molecular weight acrylates include, but are not limited to, one or more of methyl acrylate, ethyl acrylate, and methyl methacrylate.
[0050] In this invention, the thermally conductive filler includes, but is not limited to, one or more of silicon nitride, zinc oxide, silicon micro powder, boron nitride, aluminum oxide, and magnesium oxide.
[0051] In some preferred embodiments of the present invention, both the first ink and the second ink contain the following components by mass parts: 1-20 parts butyl acrylate, 1-20 parts trimethylolpropene triacrylate, 1-20 parts dimethylolpropene diacrylate, 1-20 parts epoxy acrylate, 1-20 parts metaphosphate-modified acrylate, 1-10 parts photoinitiator, 1-20 parts methyl acrylate, 1-20 parts thermally conductive filler, and 1-5 parts nano-pigment paste; and the long-wave photoinitiator in the first ink accounts for 35%-85% of the total mass of the photoinitiator, while the long-wave photoinitiator in the second ink accounts for 10%-35% of the total mass of the photoinitiator. For example, the long-wave photoinitiator is ethyl 2,4,6-trimethylbenzoylphenylphosphonate, and the short-wave photoinitiator is 1-hydroxycyclohexylphenyl ketone. The long-wave photoinitiator in the first ink accounts for 70% of the total mass of the photoinitiator, and the long-wave photoinitiator in the second ink accounts for 30% of the total mass of the photoinitiator.
[0052] The present invention also provides a method for preparing the above-mentioned insulating film, comprising the following steps:
[0053] (1) Provide a first ink and a second ink, and use the first ink to form a first UV printing layer by UV printing, and then use the second ink to form a second UV printing layer on the first UV printing layer by UV printing;
[0054] (2) The insulating film is obtained by curing under ultraviolet light.
[0055] In this invention, during the UV printing process in step (1), the ink is pre-cured by ultraviolet light while being printed to form the corresponding printing layer. In some preferred embodiments, the energy density of the ultraviolet light in the UV printing step is 190.4-238 mJ / cm². 2 .
[0056] In this invention, in step (2), the energy density of the ultraviolet light is preferably 26400-34000 mJ / cm². 2 The preferred curing temperature is 30-50℃, and the preferred curing time is 2-10s. The curing time can be adjusted appropriately according to the difference in the thickness of the insulating film to improve the curing degree of the insulating film.
[0057] The present invention also provides a battery casing, including a housing and an insulating film covering the surface of the housing. The insulating film is formed in situ on the surface of the battery casing by the above method and includes a first film layer and a second film layer stacked together, wherein the side of the first film layer away from the second film layer is attached to the surface of the housing.
[0058] The present invention will be further described below with reference to specific embodiments, so that those skilled in the art can better understand and implement the present invention, but the embodiments are not intended to limit the present invention.
[0059] Example 1
[0060] This embodiment relates to the preparation of an insulating film, and the specific operation is as follows:
[0061] Preparation of the first ink: 12 parts butyl acrylate, 10 parts methyl tris(hydroxymethyl)triacrylate, 12 parts dimethyl diacrylate, 10 parts methyl-modified epoxy acrylate, 15 parts methyl metaphosphate-modified methyl acrylate, 4.2 parts long-wave photoinitiator (ethyl 2,4,6-trimethylbenzoylphenylphosphonate), 1.8 parts short-wave photoinitiator (1-hydroxycyclohexylphenyl ketone), 16 parts methyl acrylate, 16 parts silicon nitride, and 3 parts nano-pigment paste were added to a mixing tank and stirred for 45 minutes. After mixing evenly, the mixture was ball-milled for 2 hours, dispersed at high speed for 1 hour, and then filtered through a 300-mesh screen to obtain the first ink.
[0062] Preparation of the second ink: 12 parts butyl acrylate, 10 parts methyl tris(hydroxymethyl)triacrylate, 12 parts dimethyl diacrylate, 10 parts methyl-modified epoxy acrylate, 15 parts methyl metaphosphate-modified methyl acrylate, 1.8 parts long-wave photoinitiator (ethyl 2,4,6-trimethylbenzoylphenylphosphonate), 4.2 parts short-wave photoinitiator (1-hydroxycyclohexylphenyl ketone), 16 parts methyl acrylate, 16 parts silicon nitride, and 3 parts nano-pigment paste were added to a mixing tank and stirred for 45 minutes. After mixing evenly, the mixture was ball-milled for 2 hours, dispersed at high speed for 1 hour, and then filtered through a 300-mesh screen to obtain the second ink.
[0063] Preparation of insulating film:
[0064] A first UV-printed layer with a thickness of 80 μm was printed onto the surface of the laser-cleaned aluminum battery casing using a UV printer. Then, a second UV-printed layer with a thickness of 120 μm was printed on top of the first UV-printed layer using the same UV printer. The thickness of the first UV-printed layer accounted for 40% of the total printed layer thickness. (During the UV printing process, ultraviolet light pre-cured both UV-printed layers; the energy density of the ultraviolet light was 236.8 mJ / cm².) 2 Then, it is cured by UV irradiation at 45℃ for 4 seconds (the energy density of the ultraviolet light is 28346 mJ / cm³). 2 )
[0065] Example 2
[0066] This embodiment relates to the preparation of an insulating film. The only difference from Embodiment 1 is that the printing thickness of the first printing layer is 60 μm and the printing thickness of the second printing layer is 140 μm. All other operations are the same.
[0067] Example 3
[0068] This embodiment relates to the preparation of an insulating film. The only difference from Embodiment 1 is that the printing thickness of the first printing layer is 110 μm and the printing thickness of the second printing layer is 90 μm. All other operations are the same.
[0069] Example 4
[0070] This embodiment relates to the preparation of an insulating film. The only difference from Embodiment 1 is that the printing thickness of the first printing layer is 150 μm, the printing thickness of the second printing layer is 350 μm, and the curing time is increased to 6 seconds. All other operations are the same.
[0071] Example 5
[0072] This embodiment relates to the preparation of an insulating film. The only difference from Embodiment 1 is that the long-wave photoinitiator (1.8 parts) in the first ink accounts for 30% of the total photoinitiator, and the long-wave photoinitiator (0.6 parts) in the second ink accounts for 10% of the total photoinitiator. All other operations are the same.
[0073] Example 6
[0074] This embodiment relates to the preparation of an insulating film. The only difference from Embodiment 1 is that the long-wave photoinitiator (5.1 parts) in the first ink accounts for 85% of the total photoinitiator, and the long-wave photoinitiator (2.4 parts) in the second ink accounts for 40% of the total photoinitiator. All other operations are the same.
[0075] Comparative Example 1
[0076] This comparative example relates to the preparation of an insulating film. A commercially available UV printing ink (HP Crememins HSI-KL-04) was used to print a UV-printed layer on the surface of a laser-cleaned battery aluminum casing. The printing thickness was 200 μm. (During the UV printing process, ultraviolet light pre-cured both UV-printed layers; the energy density of the ultraviolet light was 236.8 mJ / cm².) 2 Then, it is cured by UV irradiation at 45℃ for 4 seconds (the energy density of the ultraviolet light is 28346 mJ / cm³). 2 )
[0077] Comparative Example 2
[0078] This comparative example relates to the preparation of an insulating film, which differs from Example 1 only in that the printing thickness of the first printing layer is 20 μm and the printing thickness of the second printing layer is 180 μm, while all other operations are the same.
[0079] Comparative Example 3
[0080] This comparative example relates to the preparation of an insulating film, which differs from Example 1 only in that the printing thickness of the first printing layer is 120 μm and the printing thickness of the second printing layer is 80 μm, while all other operations are the same.
[0081] Comparative Example 4
[0082] This comparative example relates to the preparation of an insulating film, which differs from Example 1 only in that: in the first ink, the long-wave photoinitiator (3 parts) accounts for 50% of the total photoinitiator, and in the second ink, the long-wave photoinitiator (3 parts) accounts for 50% of the total photoinitiator; all other operations are the same.
[0083] Comparative Example 5
[0084] This comparative example relates to the preparation of an insulating film, which differs from Example 1 only in that the first ink contains only a long-wavelength photoinitiator (6 parts) and the second ink contains only a short-wavelength photoinitiator (6 parts), while all other operations are the same.
[0085] Performance testing
[0086] The insulating films prepared in the above embodiments and comparative examples were tested for shear strength, insulation performance, and aging resistance. The specific procedures are as follows:
[0087] UV-printed insulating film shear strength test: Take the printed insulating cell shell and cut it into a 25cm wide sample. Quickly and gently peel off one end of the insulating film, clamp it vertically on the tensile tester, and test the shear strength between the insulating film and the aluminum shell at 180°. Specifically, perform the UV-printed insulating film shear strength test according to GB / T 7124.
[0088] UV-printed insulating film insulation performance test: High insulation tester test, DC voltage 1000V test for 5s, insulation resistance ≥1GΩ;
[0089] UV-printed insulating film anti-aging performance test: The battery shell with the insulating film on its surface was left to stand for 1000 hours at a temperature of 85℃ and a humidity of 85%, and the shear strength and insulation resistance of the insulating film after standing were tested.
[0090] The test results are shown in Table 1 below:
[0091] Table 1
[0092]
[0093] As shown in Table 1, compared with Comparative Example 1, the insulating films prepared in Examples 1-6 have higher shear strength, insulation resistance and better anti-aging properties. This is because the insulating film prepared in Examples 1-6 uses a first printing ink formulation on the inner layer near the aluminum shell surface. The first UV printing ink contains a higher proportion of long-wavelength photoinitiators, which ensures better curing of the UV printing ink even when the wavelength of UV light decays (when UV printing the insulating film, the wavelength of UV light becomes longer as the light diffuses in the thickness direction, and the efficiency of cross-linking initiation varies greatly among different initiators within a specific wavelength range. When the printing thickness is large, the initiation efficiency of the short-wavelength initiator at the bottom layer becomes significantly worse). The outer layer of the insulating film away from the aluminum shell surface uses a second UV printing ink formulation. The second UV printing ink contains a higher proportion of photoinitiators with shorter wavelengths, resulting in a higher degree of cross-linking in the entire insulation layer thickness direction. The denser cross-linking network can significantly improve the insulation resistance of the insulation layer, but has little effect on the shear strength. In addition, a higher cross-linking network is beneficial to improving aging resistance and blocking external moisture, oxygen, etc. from entering the interior of the insulating film, thereby reducing the shear strength of the insulating film after aging.
[0094] As shown in Examples 1, 2, and 3 and Comparative Examples 2 and 3, with the increase of the thickness of the first film layer (the inner layer near the aluminum shell) of the insulating film, the corresponding thickness of the inner cross-linked network layer is also higher. This is beneficial to improving its insulation resistance, as well as the residual insulation resistance value and shear strength after aging. Moreover, the insulation performance and anti-aging performance are significantly improved compared to the insulating film prepared in Comparative Example 1 (containing only short-wave initiator). As shown in Comparative Example 2, when the thickness of the first film layer is too small, the overall insulation resistance improvement effect of the insulating film is relatively poor; while when the thickness of the first film layer is too large (e.g., in Comparative Example 3), although it is beneficial to increase the cross-linking density and improve the insulation performance of the insulating film, it will lead to a decrease in the flexibility of the insulating film and a certain degree of decrease in the corresponding shear strength.
[0095] As shown in Examples 1 and 4, with the increase of the total thickness of the insulating film, its total insulation resistance, residual insulation resistance after aging, and shear strength are all significantly improved, and the shear strength is not significantly reduced compared to the thinner insulating film (Example 1). Therefore, the method for preparing the insulating film provided by this invention can produce an insulating film with both high shear strength and high insulation properties to meet the application requirements for high insulation.
[0096] As shown in Examples 1, 5, and 6, with the decrease in the content of long-wave initiator in the first layer (the inner layer near the aluminum shell) and the second layer (the outer layer away from the aluminum shell) of the insulating film, the insulation resistance, residual insulation resistance after aging, and shear strength of the insulating film all decrease to a certain extent. In particular, the insulating film prepared in Example 6 contains a relatively high content of long-wave initiator in the first layer, resulting in a higher degree of cross-linking in the inner layer. While this is beneficial for increasing the resistance of the insulating layer, excessive cross-linking density leads to decreased flexibility and reduced shear strength of the insulating film.
[0097] As can be seen from Example 1 and Comparative Example 4, the proportion of long-wave initiator in the first film layer (inner layer near the aluminum shell) and the second film layer (outer layer away from the aluminum shell) of the insulating film prepared in Comparative Example 4 is the same, the shear strength is not significantly increased, and the insulation performance and anti-aging performance are significantly worse.
[0098] Furthermore, as can be seen from Example 1 and Comparative Example 5, the long-wave initiator content in the first layer (the inner layer near the aluminum shell) of the insulating film prepared in Comparative Example 5 is too high, and the crosslinking density of the corresponding inner layer is too high, resulting in a more obvious deterioration in the overall flexibility of the insulating film and a significant reduction in shear strength.
[0099] The embodiments described above are merely preferred examples to fully illustrate the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the claims.
Claims
1. An insulating film, characterized in that, The insulating film comprises a first film layer and a second film layer stacked together, wherein the side of the first film layer away from the second film layer is attached to the surface of the battery casing; The first film layer is obtained by photocuring a first ink, and the second film layer is obtained by photocuring a second ink. Both the first ink and the second ink contain photoinitiators, which include long-wavelength photoinitiators and short-wavelength photoinitiators. The mass percentage of long-wavelength photoinitiators in the first ink is greater than that in the second ink. The long-wavelength photoinitiators in the first ink account for 30%-85% of the total mass of the photoinitiators, and the long-wavelength photoinitiators in the second ink account for 10%-40% of the total mass of the photoinitiators. The thickness of the insulating film is 150-500 μm. The thickness of the first film layer is 30%-55% of the total thickness of the insulating film. The maximum absorption wavelength of the long-wavelength photoinitiator is greater than that of the short-wavelength photoinitiator. Both the first ink and the second ink contain the following components by weight: 0.5-20 parts of acrylate soft monomers, 1-40 parts of acrylate monomers containing multiple carbon-carbon double bonds, 0.5-20 parts of epoxy acrylates, 0.5-20 parts of flame-retardant monomers, 0.5-10 parts of photoinitiator, 0.5-20 parts of low molecular weight acrylates, 0.5-20 parts of thermally conductive fillers, and 0.5-5 parts of nano-pigment; wherein the low molecular weight acrylates have a molecular weight of less than 120. The acrylate soft monomers include one or more of butyl acrylate, isooctyl acrylate, isoamyl acrylate, and octyl acrylate; The acrylate monomers containing multiple carbon-carbon double bonds include one or more of the following: methyl trihydroxytriacrylate, trihydroxyethyl triacrylate, trihydroxybutyl triacrylate, dimethyl hydroxydiacrylate, dihydroxyethyl diacrylate, and dihydroxybutyl diacrylate. The epoxy acrylates include one or more of methyl-modified epoxy acrylate, methyl-modified epoxy acrylate, ethyl-modified epoxy acrylate, and propyl-modified epoxy acrylate; The low molecular weight acrylates include one or more of methyl acrylate, ethyl acrylate, and methyl methacrylate.
2. The insulating film according to claim 1, characterized in that, The long-wavelength photoinitiator has an absorption wavelength range of 260-480 nm, and the short-wavelength photoinitiator has an absorption wavelength range of 230-340 nm.
3. The insulating film according to claim 1, characterized in that, The flame-retardant monomer includes at least one of methyl metaphosphate modified methyl acrylate, methyl metaphosphate modified ethyl acrylate, and ethyl metaphosphate modified acrylate. The long-wavelength photoinitiator includes one or more of ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and bibenzoyl. The short-wavelength photoinitiator includes one or more of 2-methyl-2-(4-morpholino)-1-(4-(methylthio)phenyl)-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2-hydroxy-2-methyl-1-phenylpropanone; The thermally conductive filler includes one or more of silicon nitride, zinc oxide, silicon micro powder, boron nitride, aluminum oxide, and magnesium oxide.
4. The insulating film according to claim 3, characterized in that, Both the first ink and the second ink contain the following components in parts by weight: 1-20 parts butyl acrylate, 1-20 parts trimethylolpropene triacrylate, 1-20 parts dimethylolpropene diacrylate, 1-20 parts methyl-modified epoxy acrylate, 1-20 parts methyl metaphosphate-modified methyl acrylate, 1-10 parts photoinitiator, 1-20 parts methyl acrylate, 1-20 parts thermally conductive filler, and 1-5 parts nano-pigment. In the first ink, the long-wave photoinitiator accounts for 35%-85% of the total mass of the photoinitiator, and in the second ink, the long-wave photoinitiator accounts for 10%-35% of the total mass of the photoinitiator.
5. A method for preparing an insulating film according to any one of claims 1-4, characterized in that, Includes the following steps: (1) Provide a first ink and a second ink, form a first UV printing layer by UV printing of the first ink, and then form a second UV printing layer by UV printing of the second ink on the first UV printing layer; (2) The insulating film is obtained by curing under ultraviolet light.
6. The preparation method according to claim 5, characterized in that, In step (1), the UV printing step involves an ultraviolet light energy density of 190.4-238 mJ / cm². 2 ; In step (2), the energy density of the ultraviolet light is 26400-34000 mJ / cm². 2 The curing temperature is 30-50 ℃, and the curing time is 2-10 s.
7. A battery casing, comprising a housing and an insulating film covering the surface of the housing, characterized in that, The insulating film is the insulating film according to any one of claims 1-4 or the insulating film prepared by the preparation method according to claim 5 or 6; The insulating film comprises a first film layer and a second film layer stacked together, wherein the side of the first film layer away from the second film layer is attached to the surface of the housing.
Citation Information
Patent Citations
Quick-drying non-sticky ultraviolet (UV) ink-jet ink and preparation method thereof
CN109971253A
Secondary battery and battery pack
CN118572317A