Oligonucleotide-modified carriers, methods of making and using the same
Polymer-modified carriers prepared by polymerization of specific monomers have solved the problems of low loading capacity and poor stability of oligonucleotide-modified microspheres in template-free DNA synthesis, achieving efficient and stable oligonucleotide ligation and improving synthesis efficiency and accuracy.
Patent Information
- Application Number
- CN202410230922.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-29
AI Technical Summary
Existing oligonucleotide-modified microspheres suffer from low loading capacity, poor stability, and strong randomness in DNA template-free synthesis, which affects synthesis efficiency and accuracy.
Polymers are prepared by polymerization of specific monomers, and the surface of the support is modified by covalent linkage. Stable linkage of oligonucleotides is achieved by using thiol chemical reactions, which increases the loading capacity and enhances stability, making it suitable for a variety of synthesis scenarios.
This method achieves an upright linkage morphology of oligonucleotides on the carrier surface, improving the success rate and stability of the synthesis reaction, reducing carrier costs, increasing the density and uniformity of oligonucleotide modification, and supporting multiple reuses.
Smart Images

Figure CN120554591B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an oligonucleotide modified carrier, its preparation method and application, specifically to a polymer, a polymer modified carrier, an oligonucleotide modified carrier, its preparation method and application. Background Technology
[0002] Template-free DNA synthesis is a key technology in synthetic biology, used to construct DNA sequences with specific functions. However, traditional synthetic methods have limitations in terms of specificity and efficiency, especially when synthesizing complex sequences. Magnetic beads, as a sample processing and enrichment tool, can improve the efficiency and specificity of template-free synthesis.
[0003] In the field of oligonucleotide modification, surface polymer brush synthesis technology is gradually becoming an area of interest. A surface polymer brush is a high-density polymer chain that can form a uniform and ordered coating layer on the surface of magnetic beads. After oligonucleotide modification, this polymer brush can achieve a high-density directional arrangement of oligonucleotides on the magnetic bead surface, thereby enhancing specific binding and synthesis efficiency. However, in the field of template-free DNA synthesis, the application of this technology remains relatively limited and has not yet been fully developed and explored.
[0004] Currently, the technical solutions for oligonucleotide-modified microspheres generally include methods such as active group modification, click chemistry reaction, biotin-avidin / streptavidin linkage, and single-stranded DNA capture probe linkage.
[0005] Modification of active groups: Active groups, such as amino, hydroxyl or glycidyl groups, are introduced on the surface of microspheres. Then, oligonucleotides are covalently linked to these groups using crosslinking agents or coupling agents. Coupling agents include polyethylene glycol succinimide active ester, glutaraldehyde, terephthalaldehyde, etc.
[0006] Click chemistry: Using click chemistry, such as copper-catalyzed alkyne-azide cyclization (CuAAC), alkyne or azide groups are introduced onto the surface of microspheres, and click reactions occur with the corresponding alkyne or azide compounds, thus immobilizing oligonucleotides on the microspheres.
[0007] Biotin-avidin / streptavidin linkage: Biotin groups are modified on the surface of microspheres, and then avidin / streptavidin is modified onto the microspheres using biotin-avidin interactions. Biotin-avidin-modified oligonucleotide molecules are then captured through biotin-avidin interactions.
[0008] Single-stranded DNA capture probe ligation: Single-stranded DNA capture probes (such as polyT) are attached to the surface of microspheres using chemical bonding methods. The capture probes then hybridize with the reverse complementary sequence in the oligonucleotides to capture the oligonucleotide sequences.
[0009] Currently, most microspheres used for template-free DNA synthesis rely on streptavidin-biotin interactions or polyT modifications on the microsphere surface as capture probes to capture the required oligonucleotides. However, these non-covalent interactions are prone to detachment of the linked oligonucleotides under specific conditions, such as heating or the use of dissociating agents. Furthermore, streptavidin beads tend to stick together under conditions of sonication, vigorous shaking, and heating, hindering microsphere redispersibility. Other linkage methods, such as succinimide-amino coupling, epoxy-amino coupling, and aldehyde-amino coupling, readily react with the amino groups in the ribonucleotide bases of the oligonucleotides, resulting in random oligonucleotide linkage morphology. This is detrimental to the binding of oligonucleotides to enzymes in enzymatic template-free DNA synthesis, reducing reaction success rate and product accuracy. Traditional surface modification methods based on silane coupling agents have limited modification density and relatively low oligonucleotide loading. In the template-free DNA synthesis pathway, microspheres and linked oligonucleotides require multiple rounds of reactions, washing, separation, and redispersibility; therefore, stable linkage is a crucial requirement for oligonucleotide-modified microspheres.
[0010] Therefore, there is an urgent need for oligonucleotide-modified microspheres with high oligonucleotide loading capacity and good stability. Summary of the Invention
[0011] To address the shortcomings of existing oligonucleotide-modified microspheres, such as highly random oligonucleotide linkage morphology, poor stability, and low loading capacity, this invention provides a polymer, a polymer-modified carrier, an oligonucleotide-modified carrier, its preparation method, and its applications. The oligonucleotide-modified carrier based on this polymer ensures the linkage morphology of oligonucleotides on the carrier surface, maintains high loading capacity, is not easily detached, and possesses good stability, making it suitable for successful template-free DNA synthesis reactions.
[0012] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0013] This invention provides a polymer comprising repeating unit A and repeating unit B, wherein repeating unit A is a segment as shown in Formula 1, and repeating unit B is one or more segments as shown in Formulas 2-6:
[0014]
[0015]
[0016] The n represents the degree of aggregation, which is independently 4-112.
[0017] In some embodiments, the molar ratio of repeating unit A to repeating unit B is 1:1 to 1:20, preferably 1:5 to 1:20, for example 1:9 or 1:19.
[0018] In some implementations, in the segments shown in Equations 2-4, n is independently 4-22.
[0019] In some implementations, in the segments shown in Equations 2-4, n is independently 6-15.
[0020] In some specific implementations, n is 6 in the segment shown in Equation 2.
[0021] In some specific implementations, n is 15 in the segment shown in Equation 3.
[0022] In some specific implementations, n is 8 in the segment shown in Equation 4.
[0023] In some embodiments, the average molecular weight of the fragments represented by Formulas 2-4 is independently 300-5000 Da, preferably 300-1000 Da.
[0024] In some specific implementations, the average molecular weight of the fragment shown in Formula 2 is 336 Da.
[0025] In some specific implementations, the average molecular weight of the fragment shown in Formula 3 is 878 Da.
[0026] In some specific implementations, the average molecular weight of the fragment shown in Formula 4 is 438 Da.
[0027] In some specific implementations, the average molecular weight of the fragment shown in Formula 2 is 400 Da.
[0028] In some specific implementations, the average molecular weight of the fragment shown in Formula 4 is 480 Da.
[0029] The present invention also provides a method for preparing a polymer, the method comprising the following steps:
[0030] The polymer is prepared by copolymerization of monomer A and monomer B; wherein...
[0031] The monomer A is glycidyl methacrylate;
[0032] The monomer B is one or more of polyethylene glycol acrylate, polyethylene glycol methacrylate, methoxy polyethylene glycol acrylate, sodium acrylate, and vinyl acetate.
[0033] In some implementations, the polymer is as described above.
[0034] Wherein, the fragment shown in Formula 1 may be derived from glycidyl methacrylate; the fragment shown in Formula 2 may be derived from polyethylene glycol acrylate; the fragment shown in Formula 3 may be derived from polyethylene glycol methacrylate; the fragment shown in Formula 4 may be derived from methoxy polyethylene glycol acrylate; the fragment shown in Formula 5 may be derived from sodium acrylate; and the fragment shown in Formula 6 may be derived from vinyl acetate.
[0035] In some embodiments, the molar ratio of monomer A to monomer B is 1:1 to 1:20, preferably 1:5 to 1:20, for example 1:9 or 1:19.
[0036] In some embodiments, the average molecular weight of the polyethylene glycol acrylate, polyethylene glycol methacrylate, and methoxy polyethylene glycol acrylate is independently 300-5000 Da, preferably 300-1000 Da.
[0037] In some specific embodiments, the average molecular weight of the polyethylene glycol acrylate is 336 Da.
[0038] In some specific embodiments, the average molecular weight of the polyethylene glycol methacrylate is 878 Da.
[0039] In some specific embodiments, the methoxy polyethylene glycol acrylate has an average molecular weight of 438 Da.
[0040] In some specific embodiments, the average molecular weight of the polyethylene glycol acrylate is 400 Da.
[0041] In some specific embodiments, the methoxy polyethylene glycol acrylate has an average molecular weight of 480 Da.
[0042] In some embodiments, the copolymerization reaction is a surface-initiated atom transfer radical polymerization (ATRP) or a reversible addition-fragmentation chain transfer polymerization (RAFT).
[0043] In some embodiments, when the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction, the copolymerization reaction includes the step of reacting in a solvent in the presence of a catalyst and ligands.
[0044] The catalyst may be cuprous bromide and / or copper bromide.
[0045] The ligand may be 2,2'-bipyridine.
[0046] The solvent may be dimethylformamide.
[0047] The copolymerization reaction can be carried out in a nitrogen atmosphere.
[0048] The copolymerization reaction can be carried out at room temperature.
[0049] In some embodiments, the catalyst is cuprous bromide and copper bromide in a molar ratio of 1:0.1.
[0050] In some embodiments, the molar ratio of the catalyst to the ligand is 1:2.
[0051] In some embodiments, the molar ratio of total monomer to catalyst to ligand is (50-200):1.1:2.2, for example 50:1.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
[0052] In some specific embodiments, monomer A is glycidyl methacrylate, monomer B is methoxy polyethylene glycol acrylate with an average molecular weight of 480 Da, the catalyst is cuprous bromide and copper bromide, the ligand is 2,2'-bipyridine, and the molar ratio of each raw material is total monomer:cuprous bromide:copper bromide:2,2'-bipyridine = 50:1:0.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
[0053] The present invention also provides a polymer prepared according to the polymer preparation method described above.
[0054] The present invention also provides a polymer-modified carrier, the polymer-modified carrier comprising the polymer as described above and a carrier having a surface modified with a linking functional group A, wherein the polymer is covalently linked to the linking functional group A.
[0055] In some embodiments, the connecting functional group A is as shown in Formula 7:
[0056]
[0057] In some embodiments, the carrier is a conventional solid substrate in the art, typically selected from microspheres, silicon wafers, silicon dioxide wafers, and anodic aluminum oxide films.
[0058] The microspheres can be magnetic microspheres (magnetic beads) or non-magnetic microspheres, preferably selected from one of the following: silica microspheres, polystyrene microspheres, agarose microspheres, polyacrylamide microspheres, polyglycidyl methacrylate microspheres, silica-coated iron oxide microspheres, polystyrene-coated iron oxide microspheres, and agarose-coated iron oxide microspheres, for example, silica-coated iron oxide microspheres. The particle size of the microspheres can be 200 nm to 20 μm.
[0059] In some embodiments, the polymer is covalently linked to the linking functional group A and then coated onto the surface of the carrier, the thickness of which is preferably 25-150 nm, for example 98 ± 23 nm.
[0060] The present invention also provides a method for preparing a polymer-modified support, the method comprising the following steps:
[0061] The surface-modified carrier with connecting functional group A, monomer A, and monomer B are copolymerized as described above.
[0062] In some embodiments, the polymer-modified carrier is as described above.
[0063] In some embodiments, the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction or a reversible addition-fragmentation chain transfer polymerization reaction.
[0064] In some embodiments, when the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction, the copolymerization reaction includes the step of reacting in a solvent in the presence of a catalyst and ligands.
[0065] The catalyst may be cuprous bromide and / or copper bromide.
[0066] The ligand may be 2,2'-bipyridine.
[0067] The solvent may be dimethylformamide.
[0068] The copolymerization reaction can be carried out in a nitrogen atmosphere.
[0069] The copolymerization reaction can be carried out at room temperature.
[0070] In some embodiments, the catalyst is cuprous bromide and copper bromide in a molar ratio of 1:0.1.
[0071] In some embodiments, the molar ratio of the catalyst to the ligand is 1:2.
[0072] In some embodiments, the molar ratio of total monomer to catalyst to ligand is (50-200):1.1:2.2, for example 50:1.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
[0073] In some specific embodiments, monomer A is glycidyl methacrylate, monomer B is methoxy polyethylene glycol acrylate with an average molecular weight of 480 Da, the catalyst is cuprous bromide and copper bromide, the ligand is 2,2'-bipyridine, and the molar ratio of each raw material is total monomer:cuprous bromide:copper bromide:2,2'-bipyridine = 50:1:0.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
[0074] In some embodiments, when the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction, the support with the surface modified with the linking functional group A is prepared by reacting a support precursor and an initiator, wherein the linking functional group A is, for example, the group represented by Formula 7.
[0075] The term "support precursor" can refer to the product of an unmodified support after activation treatment to modify the hydroxyl groups, before modification of the linked functional group A. The activation treatment step may include, for example, mixing a sodium hydroxide solution with the unmodified support and heating the mixture to obtain the precursor. The heating temperature may be, for example, 80°C.
[0076] The initiator may be 3-(triethoxysilyl)propyl 2-bromo-2-methylpropionic acid.
[0077] The reaction step of the carrier precursor and the initiator may include: mixing the carrier precursor and the initiator in a solvent, and heating the mixture to react. The solvent may be, for example, anhydrous ethanol. The temperature of the heating reaction may be, for example, 80°C.
[0078] The present invention also provides a polymer-modified carrier, which is prepared according to the above-described method for preparing polymer-modified carriers.
[0079] The present invention also provides an oligonucleotide modified vector, the oligonucleotide modified vector comprising an oligonucleotide with terminal modification linking functional group B and a polymer modified vector as described above, wherein the linking functional group B and the polymer modified vector are covalently linked.
[0080] Alternatively, the oligonucleotide modified vector comprises an oligonucleotide with terminal modification of linking functional group B, linking functional group C and the polymer modified vector as described above, wherein the two ends of linking functional group C are covalently linked to linking functional group B and the polymer modified vector, respectively.
[0081] In some embodiments, the oligonucleotide is an oligonucleotide with a 5' end modified with a linker functional group B, such as an oligonucleotide with a 5' end modified with a thiol group.
[0082] In some embodiments, the 5'-terminal thiol-modified oligonucleotide is linked to repeat unit A of the polymer-modified carrier, for example, the thiol group is linked to repeat unit A in the following manner:
[0083]
[0084] In some embodiments, the connecting functional group C is as shown in Formula 8:
[0085]
[0086] In some embodiments, the 5'-terminal thiol-modified oligonucleotide is linked to the repeating unit A of the polymer-modified carrier via the linking functional group C, for example, the thiol group and repeating unit A are linked via the linking functional group C in the following manner:
[0087]
[0088] In some specific embodiments, the oligonucleotide modification vector includes:
[0089] (1) A carrier with a surface modified with a linker functional group A;
[0090] (2) A polymer covalently linked to the connecting functional group A;
[0091] The polymer comprises repeating unit B and repeating unit C; wherein repeating unit B is one or more segments as shown in Formulas 2-6, and repeating unit C is a segment as shown in Formula 9 or Formula 10.
[0092]
[0093] Wherein, R is an oligonucleotide.
[0094] In some implementations, the oligonucleotide is single-stranded DNA.
[0095] In some embodiments, the oligonucleotide is 12-25 bases in length.
[0096] In some specific embodiments, the oligonucleotide sequence is SH-5'-GCTACTAGGACGACTCGAATG-3'[SEQ ID NO:1].
[0097] In some embodiments, the oligonucleotide sequence further contains an enzyme recognition cleavage site; the enzyme recognition cleavage site is preferably a uracil DNA glycosylase (UDG) cleavage site for deoxyuridine (dU).
[0098] In some specific embodiments, the oligonucleotide sequence is SH-5'-AGT / ideoxyU / GCTACTAGGACGACTCGAATG-3' [SEQ ID NO:2].
[0099] In some embodiments, the oligonucleotide content in the oligonucleotide-modified vector is 0-3500 pmol / mg, and not 0; for example, 850±24 pmol / mg or 604±31 pmol / mg.
[0100] This invention also provides a method for preparing an oligonucleotide-modified vector, the method comprising the following steps:
[0101] The oligonucleotide and polymer-modified carrier are reacted to obtain the product.
[0102] Alternatively, oligonucleotides and cystamine salt solutions can be mixed, a reducing agent added, and then reacted with a polymer-modified support to obtain the final product.
[0103] The oligonucleotide and the polymer-modified carrier are as described above.
[0104] In some implementations, the oligonucleotide modification vector is as described above.
[0105] In some embodiments, the oligonucleotide is covalently linked to the polymer-modified carrier by a CS bond, wherein the CS bond is formed by the reaction of the linking functional group A (epoxy group) in repeating unit A and the linking functional group C (thiol group) at the end of the oligonucleotide; or, the oligonucleotide is covalently linked to the polymer-modified carrier by an SS bond, wherein the SS bond is formed by the reaction of the linking functional group A (epoxy group) in repeating unit A and the cystamine group, the disulfide bond is reduced by a reducing agent, and then the SS bond is formed by the reaction with the linking functional group C (thiol group) at the end of the oligonucleotide.
[0106] In some implementations, the reducing agent is TCEP.
[0107] In some embodiments, the ratio of the oligonucleotide to the polymer-modified carrier is 10 nmol: 10 mg.
[0108] In some embodiments, the reaction steps are conventional in the art, such as stirring in a solvent at room temperature for 24 or 48 hours. When the reaction system contains a cystamine salt solution, the reaction steps may be stirring at room temperature for 48 hours.
[0109] The present invention also provides an oligonucleotide modified vector, which is prepared according to the above-described method for preparing oligonucleotide modified vectors.
[0110] The present invention also provides an application of the oligonucleotide modification vector as described above in template-free DNA synthesis.
[0111] In some embodiments, the application includes mixing the oligonucleotide-modified vector with a template-free DNA synthesis reaction solution, and reacting to obtain the product.
[0112] The DNA template-free synthesis reaction solution can be conventional in the art, generally including a reaction buffer solution, terminal deoxynucleotidyl transferase (TdT enzyme), and deoxyribonucleotides.
[0113] Preferably, the reaction buffer solution comprises one or more of Tris-HCl, sodium chloride, cobalt chloride, and Tween 20.
[0114] Preferably, the deoxyribonucleotide is a natural or 3'-blocked deoxyribonucleotide, such as dideoxyguanosine 5'-triphosphate (ddGTP).
[0115] In some specific embodiments, the DNA template-free synthesis reaction solution includes 50 mM Tris-HCl, 100 mM sodium chloride, 0.25 mM cobalt chloride, 0.1% Tween 20, 1 U / μL terminal deoxynucleotidyl transferase, and 0.25 mM dideoxyguanosine 5'-triphosphate.
[0116] The reaction steps can be conventional in the art, such as incubation at room temperature for 5 minutes.
[0117] The present invention also provides the application of the oligonucleotide modified vector as described above in the preparation of DNA hybridization probe magnetic beads.
[0118] The present invention also provides the application of the oligonucleotide modified vector as described above in the preparation of specific DNA / RNA capturing magnetic beads.
[0119] Without violating common sense in the field, the above-mentioned preferred conditions can be combined arbitrarily to obtain various preferred embodiments of the present invention.
[0120] The reagents and raw materials used in this invention are all commercially available.
[0121] The positive and progressive effects of this invention are as follows:
[0122] The polymer of the present invention is obtained by polymerization of two specific monomers. When an oligonucleotide is further covalently linked to a carrier modified with this polymer to obtain an oligonucleotide-modified carrier, and this carrier is used in template-free DNA synthesis reactions, it has the following advantages:
[0123] 1. The covalent linkage reaction is made specific through chemical reactions based on thiol groups, such as epoxy-thiol addition / disulfide bond exchange, which ensures that the oligonucleotides on the carrier surface are in an upright linkage morphology, which is conducive to improving the success rate of the synthesis reaction. They are also not easy to fall off, have good stability, and are suitable for various synthesis scenarios and conditions.
[0124] 2. By utilizing radial space, polymers can transform oligonucleotides from a two-dimensional distribution on the carrier surface to a three-dimensional distribution, thereby increasing the modification density of oligonucleotides and reducing the carrier cost in synthesis.
[0125] 3. The oligonucleotide modification density in the obtained oligonucleotide modification vector is more uniform, and the distribution of oligonucleotide loading is more concentrated.
[0126] 4. The vector and oligonucleotide are linked in a reversible or irreversible manner. The reversible method allows for easy replacement of the modified oligonucleotide primers, enabling the vector to be reused multiple times in the synthesis process and further reducing the cost of the vector. Attached Figure Description
[0127] Figure 1 This is a schematic diagram of the process for synthesizing polymers on the surface of magnetic beads according to the present invention.
[0128] Figure 2 This is a schematic diagram of the process for irreversibly linking oligonucleotides to the surface of polymer-modified magnetic beads according to the present invention.
[0129] Figure 3 This is a schematic diagram of the process for reversibly linking oligonucleotides to the surface of polymer-modified magnetic beads according to the present invention.
[0130] Figure 4 The particle size distribution of the polymer-modified magnetic beads in Example 1 of Example 1 is shown at different reaction times.
[0131] Figure 5 The standard curve for measuring oligonucleotide loading in Example 2 is shown.
[0132] Figure 6 The electrophoresis results are for template-free DNA synthesis products of oligonucleotide-modified magnetic beads obtained in Examples 5-8 of Application Example 1. Detailed Implementation
[0133] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.
[0134] Unless otherwise specified, in the following examples and effect examples, the storage buffer A is pH 7.2 and contains an aqueous solution of 50 mM Tris-HCl, 100 mM sodium chloride, and 0.1% Tween 20. The percentages here are by mass.
[0135] Example 1: Preparation of Polymer-Modified Magnetic Beads
[0136] like Figure 1 The diagram shown illustrates the process of synthesizing polymers on the surface of magnetic beads according to the present invention, specifically including the following steps:
[0137] 1. Surface activation of magnetic beads
[0138] 10 mg of silica-coated iron oxide magnetic beads (500 nm in size) were dispersed in 10 mL of deionized water. The beads were separated using a magnetic field, and the supernatant was removed. The washing process was repeated three times. The magnetic beads were then dispersed in 10 mL of 0.1 M sodium hydroxide solution and added to a three-necked flask. The mixture was heated to 80 °C, refluxed, and stirred for 30 minutes. After the reaction was terminated, the magnetic beads were separated using a magnetic field, and the supernatant was removed. The mixture was washed three times with 10 mL of deionized water and twice with anhydrous ethanol. The beads were then redispersed in 1 mL of anhydrous ethanol to obtain a dispersion of activated magnetic beads.
[0139] 2. Initiator (containing bromine group) modification
[0140] Add 1 mL of the activated magnetic bead dispersion obtained in step 1 to 9 mL of anhydrous ethanol, then add 0.2 mL of 3-(triethoxysilyl)propyl 2-bromo-2-methylpropionic acid. Heat under reflux at 80 °C and stir for 24 hours. After the reaction is complete, separate the magnetic beads using a magnetic field, remove the supernatant and unreacted 3-(triethoxysilyl)propyl 2-bromo-2-methylpropionic acid, wash three times with anhydrous ethanol and twice with dimethylformamide, and redisperse the washed magnetic beads in 1 mL of dimethylformamide to obtain the initiator-modified magnetic bead dispersion.
[0141] 3. Surface-initiated atom transfer radical polymerization
[0142] Add 9 mL of dimethylformamide to a three-necked flask, connect it to a Schlenk line, and perform three vacuum-nitrogen circulation cycles to remove dissolved oxygen from the solvent. Weigh 4.5 mg of copper bromide (0.02 mmol), 28.7 mg of cuprous bromide (0.2 mmol), and 68.7 mg of 2,2'-bipyridine (0.44 mmol), add them to the three-necked flask, perform three vacuum-nitrogen circulation cycles to remove oxygen, and stir for 5 minutes to form a brown solution. Add two polymer monomers (total 10 mmol) to the three-necked flask at a molar ratio of glycidyl methacrylate to methoxy polyethylene glycol acrylate (average molecular weight approximately 480 Da, Aladdin P133111-250 mL) of 1:9, and stir for 30 minutes. That is, the molar ratio of monomers and catalyst is total monomers:cuprous bromide:copper bromide:2,2'-bipyridine = 50:1:0.1:2.2.
[0143] Then, 1 mL of the initiator-modified magnetic bead dispersion from step 2 was added, and the mixture was stirred under nitrogen protection and reacted at room temperature for 72 hours. After the reaction was completed, the magnetic beads were separated using a magnetic field, the supernatant was removed, and unreacted monomers and catalysts were removed. The mixture was washed three times with deionized water and redispersed in 1 mL of deionized water to obtain a dispersion of polymer-modified magnetic beads.
[0144] Example 2: Preparation of polymer-modified magnetic beads
[0145] Keeping all other conditions the same as in Example 1, only changing the ratio of polymer monomers in step 3 to a molar ratio of glycidyl methacrylate and methoxy polyethylene glycol acrylate of 1:1, a dispersion of polymer-modified magnetic beads of this example is obtained.
[0146] Example 3: Preparation of polymer-modified magnetic beads
[0147] Keeping all other conditions the same as in Example 1, only changing the ratio of polymer monomers in step 3 to a molar ratio of glycidyl methacrylate and methoxy polyethylene glycol acrylate of 1:4, a dispersion of polymer-modified magnetic beads of this example was obtained.
[0148] Example 4: Preparation of polymer-modified magnetic beads
[0149] Keeping all other conditions the same as in Example 1, only changing the ratio of polymer monomers in step 3 to a molar ratio of glycidyl methacrylate to methoxy polyethylene glycol acrylate of 1:19, a dispersion of polymer-modified magnetic beads of this example was obtained.
[0150] Example 5: Preparation of Oligonucleotide-Modified Magnetic Beads (Irreversible Linkage)
[0151] like Figure 2The diagram shows a process for preparing oligonucleotide-modified magnetic beads by irreversibly linking oligonucleotides to the polymer-modified magnetic beads obtained in Example 1. The process includes the following steps:
[0152] (1) Take 1 mL of the dispersion of polymer-modified magnetic beads obtained in Example 1 (containing 10 mg of magnetic beads), separate the magnetic beads using a magnetic field, remove the supernatant, and disperse it in 900 μL of PBS buffer with pH 6.8 to obtain the magnetic bead dispersion.
[0153] (2) Disperse 10 nmol of 5'-terminal thiol-modified single-stranded DNA oligonucleotides in 90 μL of PBS buffer at pH 6.8 to obtain a single-stranded DNA oligonucleotide solution. Dissolve tris(carboxyethyl)phosphonic acid hydrochloride in PBS buffer at pH 6.8 to obtain a 1 mM tris(carboxyethyl)phosphonic acid hydrochloride solution. Add 10 μL of tris(carboxyethyl)phosphonic acid hydrochloride solution to the 90 μL single-stranded DNA oligonucleotide solution and shake at room temperature for 10 minutes to break any disulfide bonds that may form between the oligonucleotides, thus exposing the thiol groups.
[0154] (3) After the reaction in step (2) is completed, the single-stranded DNA oligonucleotide solution obtained from the reaction is mixed with the magnetic bead dispersion in step (1), with a total solution volume of 1 mL. The pH of the mixture is adjusted to approximately 9 using a 1 M potassium hydroxide solution with the aid of a pH meter. The solution is stirred at room temperature and reacted for 24 hours. After the reaction is completed, the magnetic beads are separated using a magnetic field, the supernatant is removed, unreacted oligonucleotides are removed, and the mixture is washed three times with deionized water. The mixture is then redispersed in magnetic bead storage buffer A to obtain an oligonucleotide-modified magnetic bead dispersion with a concentration of 10 mg / mL.
[0155] The oligonucleotide sequence used in this embodiment is: SH-5'-AGT / ideoxyU / GCTACTAGGACGACTCGAATG-3'[SEQ ID NO:2].
[0156] To track the reaction conversion rate of oligonucleotides in step (3), 100 μL of the mixture was taken at 0, 1, 2, 4, 8, 12, and 24 hours. Magnetic beads were separated using a magnetic field, and the supernatant was collected. The concentration of unreacted oligonucleotides in the mixture was measured using a UV spectrophotometer. The results are shown in Table 1. After 24 hours of reaction, the remaining amount of oligonucleotides in the mixture was <10%.
[0157] Table 1. Changes in the remaining amount of oligonucleotides in the reaction solution over reaction time.
[0158] Reaction time / hour Remaining oligonucleotide concentration in solution / μM 0 10±0 1 7.23±0.19 2 4.89±0.27 4 3.05±0.34 8 1.75±0.26 12 1.1±0.31 24 0.5±0.25
[0159] Example 6: Preparation of Oligonucleotide-Modified Magnetic Beads (Irreversible Linkage)
[0160] Following the conditions in Example 5, oligonucleotides were modified into the polymer-modified microspheres of Example 2 to prepare the oligonucleotide-modified magnetic bead dispersion of this example.
[0161] Example 7: Preparation of Oligonucleotide-Modified Magnetic Beads (Irreversible Linkage)
[0162] Following the conditions in Example 5, oligonucleotides were modified into the polymer-modified microspheres of Example 3 to prepare the oligonucleotide-modified magnetic bead dispersion of this example.
[0163] Example 8: Preparation of Oligonucleotide-Modified Magnetic Beads (Irreversible Linkage)
[0164] Following the conditions in Example 5, oligonucleotides were modified into the polymer-modified microspheres of Example 4 to prepare a dispersion of oligonucleotide-modified magnetic beads of this example.
[0165] Example 9: Preparation of Oligonucleotide-Modified Magnetic Beads (Reversible Ligation)
[0166] like Figure 3 The diagram shows a process for preparing oligonucleotide-modified magnetic beads by reversibly linking oligonucleotides to the polymer-modified magnetic beads obtained in Example 2. The process includes the following steps:
[0167] (1) 1 mL of the polymer-modified magnetic bead dispersion obtained in Example 2 (containing 10 mg of magnetic beads) was separated using a magnetic field, the supernatant was removed, and the dispersion was placed in 1 mL of PBS buffer at pH 6.8 to obtain a magnetic bead dispersion. Cystamine hydrochloride was dissolved in PBS buffer at pH 6.8 to obtain a 10 mM cystamine solution. The pH of the solution was adjusted to approximately 7 using potassium hydroxide with the aid of a pH meter. 100 μL of cystamine solution was added to the magnetic bead dispersion, and the reaction was carried out at room temperature with shaking for 3 hours. After the reaction was completed, the magnetic beads were separated using a magnetic field, the supernatant and unreacted cystamine were removed, and the mixture was washed 3 times with deionized water and redispersed in 1 mL of PBS buffer at pH 6.8 to obtain a magnetic bead dispersion.
[0168] (2) Dissolve tris(carboxyethyl)phosphine hydrochloride in PBS buffer at pH 6.8 to obtain a 100 mM tris(carboxyethyl)phosphine hydrochloride solution. Add 100 μL of the tris(carboxyethyl)phosphine hydrochloride solution to 1 mL of the magnetic bead dispersion obtained in step (1), and shake at room temperature for 10 minutes to break the disulfide bonds in cystamine and obtain exposed thiol groups. After the reaction, separate the magnetic beads using a magnetic field, remove the supernatant, wash three times with deionized water, and redisperse in 900 μL of 1 M sodium bicarbonate buffer at pH 8 to obtain the magnetic bead dispersion.
[0169] (3) 10 nmol of 5'-terminal thiol-modified single-stranded DNA oligonucleotides were dispersed in 100 μL of 1 M sodium bicarbonate buffer at pH 8, and mixed with the magnetic bead dispersion obtained in step (2) to obtain a mixture. The mixture was stirred at room temperature for 48 hours. After the reaction was completed, the magnetic beads were separated using a magnetic field, the supernatant was removed, unreacted oligonucleotides were removed, and the mixture was washed three times with deionized water and redispersed in magnetic bead storage buffer A to obtain oligonucleotide-modified magnetic beads with a concentration of 10 mg / mL.
[0170] The oligonucleotide sequence used in this embodiment is: SH-5'-AGT / ideoxyU / GCTACTAGGACGACTCGAATG-3'[SEQ ID NO:2].
[0171] To track the reaction conversion rate of oligonucleotides in step (3), 100 μL of the mixture was taken at 0, 1, 2, 4, 8, 12, 24, and 48 hours. Magnetic beads were separated using a magnetic field, and the supernatant was collected. The concentration of unreacted oligonucleotides in the mixture was measured using a UV spectrophotometer. As shown in Table 2, after 48 hours of reaction, the remaining amount of oligonucleotides in the mixture was <30%.
[0172] Table 2. Changes in the remaining amount of oligonucleotides in the reaction solution over reaction time.
[0173] Reaction time / hour Remaining oligonucleotide concentration in solution / μM 0 10±0 1 8.34±0.16 2 7.13±0.21 4 6.05±0.35 8 4.61±0.37 12 3.72±0.25 24 2.81±0.41 48 2.25±0.45
[0174] Example 1: Characterization of relevant structural parameters of polymer-modified microspheres
[0175] To monitor the change in the reaction time of the polymer with surface-initiated atom transfer radical polymerization in Examples 1-4, 0.5 mL of the magnetic bead dispersion in the process of reaction or after the reaction was completed was taken at 0 hours, 6 hours, 12 hours, 24 hours, 48 hours, and 72 hours. The magnetic beads were separated by a magnetic field, the supernatant was removed, and the mixture was washed three times with deionized water. The mixture was then redispersed in 1 mL of deionized water, and the change in the particle size of the magnetic beads was measured using a dynamic light scattering particle size analyzer.
[0176] like Figure 4 As shown, in Example 1 (monomer molar ratio of 1:9), the magnetic bead particle size increased with increasing reaction time, and the particle size distribution slightly widened. After 72 hours of reaction, the thickness of the obtained polymer was approximately 98±23 nm. Furthermore, as shown in Table 3, increasing the proportion of glycidyl methacrylate (monomer molar ratios of 1:1 and 1:4) slowed the polymer growth rate and caused significant fluctuations in thickness. Specifically, the polymer-modified magnetic beads with a monomer ratio of 1:1 exhibited significant agglomeration and adhesion phenomena.
[0177] Table 3. Changes in particle size of polymer-modified magnetic beads obtained in Examples 1-4 as a function of reaction time.
[0178] reaction time <![CDATA[Particle size 1:1 > <![CDATA[particle size 1:4 > <![CDATA[Particle size 1:9 > <![CDATA[particle size 1:19 > 0h 507.85±11.9 504.85±12.9 502.85±13.9 501.85±11.9 8h 515.78±17.56 521.78±15.56 527.78±16.56 534.78±15.56 24h 533.63±20.87 542.63±19.87 557.63±18.87 577.63±16.87 48h 557.85±35.15 567.85±20.15 578.85±22.15 605.85±17.15 72h 579.35±49.35 589.35±23.35 600.35±22.35 625.35±19.35
[0179] Example 2: Oligonucleotide loading analysis of oligonucleotide-modified microspheres
[0180] Oligonucleotide-modified magnetic beads from Examples 5-9 were used respectively, and oligonucleotide loading analysis was performed according to the following steps:
[0181] Take 10 μL of the oligonucleotide-modified magnetic bead dispersion (containing 0.1 mg of magnetic beads) with a concentration of 10 mg / mL as described in Examples 5-9, add 100 μL of storage buffer A, separate the magnetic beads using a magnetic field, remove the supernatant, and redisperse the magnetic beads in 100 μL of storage buffer A to obtain the magnetic bead dispersion. Add 2 μL of UDG enzyme (Shanghai Sangon Biotech) with a concentration of 2 U / μL to the magnetic bead dispersion, mix well by pipetting, and incubate at 50°C for 5 minutes. After the reaction is complete, incubate at 95°C for 10 minutes to inactivate the enzyme. Separate the magnetic beads using a magnetic field and collect the supernatant. Use a UV spectrophotometer to establish a standard curve using a 0.1–10 μM reference oligonucleotide (with the same sequence as the modified oligonucleotide after cleavage) solution. Take 5 sets of supernatants for testing, calculate the oligonucleotide concentration in the supernatant using the standard curve, and then deduce the oligonucleotide loading on the magnetic beads.
[0182] The reference oligonucleotide sequence is: 5'-GCTACTAGGACGACTCGAATG-3' [SEQ ID NO:3]. The resulting standard curve is shown below. Figure 5 As shown in the figure, the corresponding specific data is shown in Table 4.
[0183] Table 4. Specific values of the standard curve for oligonucleotide loading assay
[0184]
[0185]
[0186] The results are as follows:
[0187] According to UV spectrophotometer data, the oligonucleotide loading of the oligonucleotide-modified magnetic beads (irreversibly linked) in Example 5 was 850 ± 24 pmol / mg; and the oligonucleotide loading of the oligonucleotide-modified magnetic beads (reversibly linked) in Example 9 was 604 ± 31 pmol / mg.
[0188] Furthermore, the saturated loading of oligonucleotides on the oligonucleotide-modified magnetic beads obtained in Examples 5-8 with different monomer ratios is shown in Table 5. The results show that when the proportion of the spacer monomer polyethylene glycol methacrylate is less than 90%, the saturated oligonucleotide loading of different batches of magnetic beads has a large error because the surface epoxy groups cannot react completely.
[0189] Table 5. Comparison of saturated oligonucleotide loading capacity of the oligonucleotide-modified magnetic beads obtained in Examples 5-8
[0190] Monomer ratio (GMA:PEGMA) Oligonucleotide loading (pmol / mg) 1:1 3378±347 1:4 1543±141 1:9 850±24 1:19 463±15
[0191] Furthermore, as shown in Table 6, compared with commercially available oligonucleotide-modified magnetic beads, the oligonucleotide loading capacity of the polymer-modified magnetic beads of the present invention, whether linked irreversibly (Example 5) or reversibly (Example 9), is superior to that of commercially available oligonucleotide-modified magnetic beads. In particular, compared with carboxyl magnetic beads, the oligonucleotide loading capacity of the oligonucleotide-modified magnetic beads of the present invention is about 4 to 6 times that of carboxyl magnetic beads.
[0192] Among them, the dT magnetic beads were Thermo Fisher, Dynabeads Oligo(dT)25, with the captured DNA sequence 5'-AGT / ideoxyU / GCTACTAGGACGACTCGAATGAAAAAAAAAAAAAAA-3' [SEQ ID NO:4], prepared by incubation at 37°C for 1 hour; the streptavidin magnetic beads were Thermo Fisher, Dynabeads M-270 streptavidin, with the captured DNA sequence biotin-5'-AGT / ideoxyU / GCTACTAGGACGACTCGAATG-3' [SEQ ID NO:5], prepared by incubation at 37°C for 1 hour; and the carboxyl magnetic beads were Thermo Fisher, Dynabeads M-270 carboxylic acid, with the captured DNA sequence NH2-5'-AGT / ideoxyU / GCTACTAGGACGACTCGAATG-3' [SEQ ID NO:6], ligated via EDC / NHS reaction.
[0193] Table 6. Comparison of oligonucleotide loading capacity between the oligonucleotide-modified magnetic beads obtained in this invention and commercially available magnetic beads.
[0194] Oligonucleotide loading (pmol / mg) dT magnetic beads 70 Streptomycin magnetic beads 600 Carboxylic magnetic beads 150 Polymer-modified magnetic beads – reversible 650 Polymer-modified magnetic beads – irreversible 850
[0195] Example 3: Stability analysis of oligonucleotide-modified microspheres
[0196] To verify the stability difference between the oligonucleotide-modified magnetic beads of Examples 5 and 9 of this invention and commercially available oligonucleotide-modified magnetic beads, this invention compared the retention amount of oligonucleotides loaded in different ways on the magnetic beads at different temperatures. The specific steps are as follows:
[0197] Take the same amount of oligonucleotide-modified magnetic beads (100 pmol of oligonucleotides), wash, dilute, and bring the volume to 100 μL. Incubate at different temperatures (60℃, 70℃, 80℃, 90℃) with shaking for 5 min, then separate using a magnetic field. Remove the supernatant, wash once with deionized water, and redisperse in 100 μL of deionized water. Add 2 μL of 2 U / μL UDG enzyme, mix well by pipetting, and incubate at 50℃ for 5 min. After the reaction is complete, incubate at 95℃ for 10 min to inactivate the enzyme. Separate the magnetic beads using a magnetic field and collect the supernatant. Use a UV spectrophotometer to establish a standard curve with 0.1–10 μM reference oligonucleotide (with the same cleaved sequence as the modified oligonucleotide) solutions. Take 5 sets of supernatants for testing, calculate the oligonucleotide concentration in the supernatant using the standard curve, and deduce the oligonucleotide loading on the magnetic beads.
[0198] As shown in Table 7, the oligonucleotide retention of magnetic beads linked by non-covalent methods (dT, streptavidin) decreased significantly after high-temperature treatment, especially at temperatures above 70°C, where the retention was <60%. In contrast, the oligonucleotide retention of magnetic beads linked by covalent methods (carboxyl groups, polymers) was >98% after high-temperature treatment. These results indicate that covalently linked oligonucleotides exhibit higher stability compared to non-covalently linked oligonucleotides (e.g., DNA sequence hybridization, streptavidin-biotin).
[0199] Table 7. Comparison of stability between the oligonucleotide-modified magnetic beads obtained in this invention and commercially available magnetic beads.
[0200]
[0201] Application Example 1: Template-free DNA Synthesis Based on Oligonucleotide-Modified Magnetic Beads
[0202] Take the four oligonucleotide-modified magnetic bead dispersions from Examples 5-8, calculate the required dispersion volume based on the oligonucleotide loading to ensure an added oligonucleotide content of 0.1 nmol, and disperse them in 100 μL of storage buffer A. Separate the magnetic beads using a magnetic field and remove the supernatant. Add 100 μL of the following template-free synthesis reaction solution (using water as the solvent) to each.
[0203] Table 8. Component information of template-free synthesis reaction solution
[0204] reagents concentration Tris-HCl 50mM Sodium chloride 100mM cobalt chloride 0.25mM TdT enzyme (NEB) 1U / μL Dideoxyguanosine 5'-triphosphate (ddGTP) 0.25mM Twain 20 0.1%
[0205] After mixing the magnetic beads by pipetting, incubate at room temperature for 5 minutes. Once the reaction is complete, separate the magnetic beads using a magnetic field, remove the supernatant, wash the magnetic beads twice with storage buffer A, and redisperse the beads in 100 μL of storage buffer A. Add 2 μL of 2 U / μL UDG enzyme (Shanghai Sangon Biotech) to the magnetic bead dispersion, mix by pipetting, and incubate at 50°C for 5 minutes. After the reaction is complete, incubate at 95°C for 10 minutes to inactivate the enzyme. Separate the magnetic beads using a magnetic field and collect the supernatant.
[0206] As a control group, 12.5 μL of the oligonucleotide-modified magnetic bead dispersion from Example 5 was dispersed in 100 μL of storage buffer A. The magnetic beads were separated using a magnetic field, the supernatant was removed, and the magnetic beads were washed twice with storage buffer A. The magnetic beads were then redispersed in 100 μL of storage buffer A. 2 μL of UDG enzyme at a concentration of 2 U / μL was added to the magnetic bead dispersion, and the mixture was incubated at 50°C for 5 minutes after mixing. After the reaction was completed, the mixture was incubated at 95°C for 10 minutes to inactivate the enzyme. The magnetic beads were then separated using a magnetic field, and the supernatant was collected.
[0207] Take 10 μL of the supernatant for product analysis, add 10 μL of 2X TBE-Urea Loading Buffer (Beyotime), mix, and load onto TBE-urea gel for comparison.
[0208] like Figure 6 As shown, the results in the TBE-urea gel indicate that the oligonucleotides loaded on the oligonucleotide-modified magnetic beads of Examples 5 and 8 (monomer ratios of 1:9 and 1:19) can serve as primers for template-free enzymatic DNA synthesis, and no unextended oligonucleotides were observed. The oligonucleotides loaded on the oligonucleotide-modified magnetic beads of Examples 6 and 7 (monomer ratios of 1:1 and 1:4) could not be completely reacted, resulting in obvious unreacted bands.
Claims
1. An oligonucleotide modification vector, characterized in that, The oligonucleotide modified vector comprises an oligonucleotide with a thiol group modified at its 5' end and a polymer modified vector, wherein the thiol group and the polymer modified vector are covalently linked. Alternatively, the oligonucleotide modified vector comprises an oligonucleotide with a thiol group modified at its 5' end, a linking functional group C, and a polymer modified vector, wherein the two ends of the linking functional group C are covalently linked to the thiol group and the polymer modified vector, respectively. The connecting functional group C is shown in Equation 8: ; Wherein, the polymer-modified carrier satisfies the following condition (1) or (2): (1) The polymer-modified carrier includes a polymer and a carrier with a surface modified with a linking functional group A, wherein the polymer is covalently linked to the linking functional group A; (2) The polymer-modified carrier is prepared according to the preparation method of the polymer-modified carrier, and the preparation method of the polymer-modified carrier includes the following steps: a carrier with surface modified with a connecting functional group A, monomer A and monomer B are copolymerized; In condition (1) or (2), the connecting functional group A is as shown in Equation 7: ; Wherein, the polymer satisfies the following condition (3) or (4): (3) The polymer comprises repeating unit A and repeating unit B; wherein repeating unit A is a segment as shown in Formula 1, and repeating unit B is one or more segments as shown in Formulas 2-6: 、 , , , and ; The n represents the degree of aggregation, which is independently 4-112; (4) The polymer is prepared according to a polymer preparation method, and the polymer preparation method includes the following steps: The polymer is prepared by copolymerization of monomer A and monomer B; wherein... The monomer A is glycidyl methacrylate; The monomer B is one or more of polyethylene glycol acrylate, polyethylene glycol methacrylate, methoxy polyethylene glycol acrylate, sodium acrylate, and vinyl acetate.
2. The oligonucleotide modification vector as described in claim 1, characterized in that, The oligonucleotide with a thiol group modified at its 5' end is linked to repeat unit A of the polymer-modified carrier; Alternatively, the oligonucleotide modified with a thiol group at its 5' end may be linked to the repeating unit A of the polymer-modified carrier via the linking functional group C.
3. The oligonucleotide modification vector as described in claim 2, characterized in that, When the oligonucleotide modified with a thiol group at its 5' end is linked to repeat unit A of the polymer-modified carrier, the thiol group is linked to repeat unit A in the following manner: ; Alternatively, when the oligonucleotide modified with a thiol group at its 5' end is linked to the repeating unit A of the polymer-modified support via the linking functional group C, the thiol group and the repeating unit A are linked via the linking functional group C in the following manner: 。 4. The oligonucleotide modification vector as described in claim 3, characterized in that, The oligonucleotide modification vector includes: (1) A carrier with a surface modified with a connecting functional group A; (2) A polymer covalently linked to the connecting functional group A; The polymer comprises repeating unit B and repeating unit C; wherein repeating unit B is one or more segments as shown in Formulas 2-6, and repeating unit C is a segment as shown in Formula 9 or Formula 10. 、 。 5. The oligonucleotide-modified vector as described in claim 1, characterized in that, The oligonucleotide is single-stranded DNA; And / or, the oligonucleotide is 12-25 bases in length; And / or, the oligonucleotide content in the oligonucleotide modified vector is 0-3500 pmol / mg, and is not 0.
6. The oligonucleotide modification vector as described in claim 5, characterized in that, The oligonucleotide content in the oligonucleotide modified vector is 850±24 pmol / mg or 604±31 pmol / mg.
7. The oligonucleotide modification vector as described in claim 1, characterized in that, In condition (1) or (2), the carrier is selected from one of microspheres, silicon wafers, silicon dioxide wafers and anodic aluminum oxide films; And / or, in condition (1) or (2), after the polymer is covalently linked to the connecting functional group A, it is wrapped around the surface of the carrier, and the thickness of the wrapping is 25-150 nm.
8. The oligonucleotide-modified vector as described in claim 7, characterized in that, In condition (1) or (2), the microspheres are magnetic microspheres or non-magnetic microspheres; And / or, in condition (1) or (2), the particle size of the microspheres is 200 nm-20 μm; And / or, in condition (1) or (2), after the polymer is covalently linked to the connecting functional group A, it is wrapped around the surface of the carrier, and the thickness of the wrapping is 98±23nm.
9. The oligonucleotide-modified vector as described in claim 8, characterized in that, In condition (1) or (2), the carrier is selected from one of silica microspheres, polystyrene microspheres, agarose microspheres, polyacrylamide microspheres, polyglycidyl methacrylate microspheres, silica-coated iron oxide microspheres, polystyrene-coated iron oxide microspheres, and agarose-coated iron oxide microspheres.
10. The oligonucleotide-modified vector as described in claim 9, characterized in that, In condition (1) or (2), the carrier is silicon dioxide coated iron oxide microspheres.
11. The oligonucleotide-modified vector according to claim 1, characterized in that, In condition (2), the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction, and the copolymerization reaction includes the steps of reacting in a solvent in the presence of a catalyst and ligands.
12. The oligonucleotide-modified vector according to claim 11, characterized in that, In condition (2), the catalyst is cuprous bromide and / or copper bromide; And / or, in condition (2), the ligand is 2,2'-bipyridine; And / or, in condition (2), the solvent is dimethylformamide; And / or, in condition (2), the copolymerization reaction is carried out in a nitrogen atmosphere; And / or, in condition (2), the temperature of the copolymerization reaction is room temperature.
13. The oligonucleotide-modified vector as described in claim 12, characterized in that, In condition (2), the catalyst is cuprous bromide and copper bromide in a molar ratio of 1:0.1; And / or, in condition (2), the molar ratio of the catalyst to the ligand is 1:
2.
14. The oligonucleotide-modified vector as described in claim 13, characterized in that, In condition (2), the molar ratio of total monomer: catalyst: ligand is (50-200):1.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
15. The oligonucleotide-modified vector as described in claim 14, characterized in that, In condition (2), the molar ratio of total monomer: catalyst: ligand is 50:1.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
16. The oligonucleotide-modified vector according to claim 1, characterized in that, In condition (3) or (4), the molar ratio of repeating unit A to repeating unit B is 1:1-1:20; And / or, in condition (3) or (4), the average molecular weight of the fragments in the repeating unit B, as shown in formulas 2-4, is independently 300-5000 Da.
17. The oligonucleotide-modified vector as described in claim 16, characterized in that, In condition (3) or (4), the molar ratio of repeating unit A to repeating unit B is 1:5-1:20; And / or, in condition (3) or (4), n is independently 4-22; And / or, in condition (3) or (4), the average molecular weight of the fragments in the repeating unit B, as shown in formulas 2-4, is independently 300-1000 Da.
18. The oligonucleotide-modified vector as described in claim 17, characterized in that, In condition (3) or (4), the molar ratio of repeating unit A to repeating unit B is 1:9 or 1:19; And / or, in conditions (3) or (4), n is independently 6-15.
19. The oligonucleotide-modified vector as described in claim 1, characterized in that, In condition (4), the molar ratio of monomer A to monomer B is 1:1 to 1:20; And / or, in condition (4), the average molecular weight of the polyethylene glycol acrylate, polyethylene glycol methacrylate and methoxy polyethylene glycol acrylate is independently 300-5000 Da. And / or, in condition (4), the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction or a reversible addition-fragmentation chain transfer polymerization reaction.
20. The oligonucleotide-modified vector as described in claim 19, characterized in that, In condition (4), the molar ratio of monomer A to monomer B is 1:5-1:20; And / or, in condition (4), the average molecular weight of the polyethylene glycol acrylate, polyethylene glycol methacrylate and methoxy polyethylene glycol acrylate is independently 300-1000 Da.
21. The oligonucleotide-modified vector according to claim 20, characterized in that, In condition (4), the molar ratio of monomer A to monomer B is 1:9 or 1:
19.
22. The oligonucleotide-modified vector as described in claim 19, characterized in that, In condition (4), the copolymerization reaction is a surface-initiated atom transfer radical polymerization reaction, and the copolymerization reaction includes the steps of reacting in a solvent in the presence of a catalyst and ligands.
23. The oligonucleotide-modified vector as described in claim 22, characterized in that, In condition (4), the catalyst is cuprous bromide and / or copper bromide; And / or, in condition (4), the ligand is 2,2'-bipyridine; And / or, in condition (4), the solvent is dimethylformamide; And / or, in condition (4), the copolymerization reaction is carried out in a nitrogen atmosphere; And / or, in condition (4), the temperature of the copolymerization reaction is room temperature.
24. The oligonucleotide-modified vector as described in claim 23, characterized in that, In condition (4), the catalyst is cuprous bromide and copper bromide in a molar ratio of 1:0.1; And / or, in condition (4), the molar ratio of the catalyst to the ligand is 1:
2.
25. The oligonucleotide-modified vector as described in claim 24, characterized in that, In condition (4), the molar ratio of total monomer: catalyst: ligand is (50-200):1.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
26. The oligonucleotide-modified vector as described in claim 25, characterized in that, In condition (4), the molar ratio of total monomer: catalyst: ligand is 50:1.1:2.2, wherein the molar ratio of total monomer is the sum of the molar ratios of monomer A and monomer B.
27. A method for preparing an oligonucleotide-modified vector, characterized in that, The preparation method includes the following steps: The oligonucleotide and polymer-modified carrier are reacted to obtain the product. Alternatively, oligonucleotides and cystamine salt solutions can be mixed, a reducing agent added, and then reacted with a polymer-modified support to obtain the final product. The polymer-modified carrier is as described in any one of claims 1 and 7-15; The oligonucleotide is as described in any one of claims 1-6.
28. The method for preparing the oligonucleotide modified vector as described in claim 27, characterized in that, The oligonucleotide modified vector is as described in any one of claims 1-26; And / or, the reducing agent is TCEP; And / or, the ratio of the oligonucleotide to the polymer-modified carrier is 10 nmol: 10 mg.
29. An oligonucleotide modification vector, characterized in that, It is prepared according to the method for preparing oligonucleotide modified vectors as described in claim 27 or 28.
30. The use of an oligonucleotide-modified vector as described in any one of claims 1-26 and 29 in template-free DNA synthesis, DNA hybridization probe magnetic beads, specific DNA capture magnetic beads, or specific RNA capture magnetic beads.
31. The application as described in claim 30, characterized in that, The application includes: mixing the oligonucleotide modification vector with a template-free DNA synthesis reaction solution, and reacting to obtain the product.
32. The application as described in claim 31, characterized in that, The template-free DNA synthesis reaction solution includes a reaction buffer solution, terminal deoxynucleotidyl transferase, and deoxyribonucleotides.
33. The application as described in claim 32, characterized in that, The reaction buffer solution includes one or more of Tris-HCl, sodium chloride, cobalt chloride, and Tween 20; And / or, the deoxyribonucleotide is a natural or 3'-closed deoxyribonucleotide.
34. The application as described in claim 33, characterized in that, The deoxyribonucleotide is dideoxyguanosine 5'-triphosphate.
Citation Information
Patent Citations
Preparation method of hairbrush-shaped fluorescent polymer modified fluorescent microsphere
CN111995721A
Functional polymer for targeting endotoxin, endotoxin separation material as well as preparation and application of functional polymer and endotoxin separation material
CN116903781A