Loofah sponge nanocellulose hydrogel as well as preparation method and application thereof
Through the eutectic solvent and lithium chloride electrolyte combined with polyacrylamide/nanocellulose dual network structure, a loofah nanocellulose hydrogel suitable for flexible electrons was prepared, which solved the problems of high energy consumption and insufficient hydrogel strength in traditional nanocellulose preparation, and achieved green and environmentally friendly high-performance hydrogel application.
Patent Information
- Application Number
- CN202510731227.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-03
- Publication Date
- 2025-08-29
AI Technical Summary
The existing nanocellulose preparation process has high energy consumption and high pollution. Traditional hydrogels have single functions, insufficient strength in flexible electronic applications, and the preparation process is not green and environmentally friendly.
The loofah nanocellulose hydrogel is prepared by using eutectic solvents. By introducing lithium chloride electrolytes and constructing a polyacrylamide/nanocellulose dual network structure, the conductivity, frost resistance and mechanical strength of the hydrogel are improved, and waste loofah is used as raw material. The preparation process is simple, low-cost, and green and environmentally friendly.
The prepared hydrogel has excellent biocompatibility, mechanical properties and electrical conductivity, and is suitable for flexible electronics, including electronic skin and wearable sensors, and is green and environmentally friendly.
Smart Images

Figure CN120554669A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and in particular to a loofah nanocellulose hydrogel and a preparation method and application thereof. Background Art
[0002] Nanocellulose is a novel natural biomaterial with nanoscale dimensions and numerous excellent properties. The core of nanocellulose's application mechanism lies in its nanoscale structural control and surface chemical functionalization. Through physical barrier properties, mechanical enhancement, biocompatibility optimization, and environmentally responsive design, it has multifunctional applications in barrier materials, composite materials, biomedicine, energy, and environmental protection.
[0003] In terms of raw material selection, loofah is an ideal source of nanocellulose due to its rapid growth, high fiber content (70% to 90%), and strong renewability. However, traditional nanocellulose preparation processes are energy-intensive and polluting, posing challenges to the green production of loofah nanocellulose.
[0004] In recent years, deep eutectic solvent (DES) technology has emerged. Deep eutectic solvents are often made from natural metabolites (such as choline chloride, urea, and carboxylic acids). They have low toxicity to organisms and are completely biodegradable. The degradation products are non-toxic and harmless. Furthermore, the raw materials are inexpensive and the synthesis process is simple, making them a green solvent. Therefore, it is possible to try using deep eutectic solvents (DES) for the preparation of loofah nanocellulose.
[0005] In terms of application, nanocellulose exhibits unique advantages: the hydrogels constructed with it not only have excellent mechanical properties and biocompatibility, but also have excellent water absorption and water retention. These properties can effectively solve the problems faced by traditional hydrogels in flexible electronic applications, such as single functionality and insufficient strength. In addition, studies have found that lithium chloride is a very promising electrolyte that is highly soluble in water. When dissolved in water, it produces lithium ions with small ionic radius and high mobility. It also destroys the hydrogen bond network between water molecules through strong hydration, effectively inhibiting the crystallization of water molecules. Therefore, when introduced into hydrogels, it will give them excellent antifreeze, dryness resistance and electrical conductivity. The double network hydrogel of polyacrylamide and nanocellulose can improve the mechanical strength of the hydrogel.
[0006] Based on this, we can try to develop a loofah nanocellulose hydrogel, and by introducing lithium chloride electrolyte and constructing a polyacrylamide / nanocellulose double network structure, we can further improve the conductivity, frost resistance and mechanical strength of the hydrogel for use in the field of flexible electronics, including electronic skin and wearable sensors. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to provide a loofah nanocellulose hydrogel and its preparation method and application. The hydrogel has excellent biocompatibility, mechanical properties and conductivity, has broad application prospects in the field of flexible electronics, and has a simple preparation process, low cost, and is green and environmentally friendly.
[0008] The present invention adopts the following technical solutions to solve the above technical problems:
[0009] A loofah nanocellulose hydrogel comprises the following steps:
[0010] (1) Extraction and bleaching of loofah cellulose
[0011] The loofah powder and glacial acetic acid-hydrogen peroxide solution are mixed and stirred in a water bath until the solution turns white; the reaction product is filtered, washed to neutrality, and freeze-dried to obtain the loofah purified cellulose;
[0012] (2) Preparation of loofah nanocellulose
[0013] Anhydrous citric acid, choline chloride and deionized water are mixed and stirred in a water bath to react until a clear and transparent ternary deep eutectic solvent is obtained;
[0014] The purified loofah cellulose prepared in step (1) is dispersed in the ternary deep eutectic solvent and reacted under stirring and heating conditions; the reaction product is washed and filtered to neutrality, dispersed in deionized water, and then subjected to ultrasonic treatment to obtain a loofah nanocellulose suspension;
[0015] (3) Preparation of precursor solution
[0016] Dissolve sodium lignin sulfonate and lithium chloride in sodium hydroxide solution to obtain a precursor solution;
[0017] (4) Preparation of loofah nanocellulose hydrogel
[0018] The loofah nanocellulose suspension obtained in step (2) is mixed with deionized water, polyacrylamide, ammonium persulfate, and N,N-methylenebisacrylamide, and the precursor solution prepared in step (3) is poured into the mixture. After stirring evenly, the mixture is poured into a mold and sealed. After the hydrogel is formed, the loofah nanocellulose hydrogel is obtained.
[0019] As one of the preferred embodiments of the present invention, in step (1), the method for obtaining the loofah powder is as follows: removing the skeleton of discarded loofah and cutting it into block loofah; and drying, grinding and sieving the block loofah to obtain the loofah powder.
[0020] As one of the preferred embodiments of the present invention, the block-shaped loofah is dried at 80° C., placed in a grinder for grinding, and then passed through an 80-mesh sieve to obtain the loofah powder.
[0021] As one of the preferred embodiments of the present invention, in step (1), the method for obtaining the glacial acetic acid-hydrogen peroxide solution is as follows: 100 ml of glacial acetic acid and 100 ml of hydrogen peroxide are taken respectively and mixed evenly in a ratio of 1:1.
[0022] As one of the preferred embodiments of the present invention, the specific process of step (1) is as follows:
[0023] Take 10g of loofah powder and mix it evenly with 200ml of glacial acetic acid-hydrogen peroxide solution, and heat it in a water bath at 80℃ in a magnetic stirring heater for 10 hours until the solution turns white; the reaction product is filtered and washed with deionized water until neutral, and then freeze-dried using a freeze dryer to obtain loofah purified cellulose.
[0024] As one of the preferred embodiments of the present invention, the specific process of step (2) is as follows:
[0025] Anhydrous citric acid, choline chloride, and deionized water were mixed in a mass ratio of 2:1:1 and magnetically stirred in a water bath at 80°C for 20 min until a clear and transparent ternary deep eutectic solvent was obtained;
[0026] Take 2g of purified cellulose from loofah and disperse it in 60ml of a ternary low eutectic solvent. Use an overhead stirrer at a stirring rate of 300r / min and react at a heating temperature of 130°C for 2h. Then, wash the reaction product with deionized water, filter it until neutral, disperse it in 150ml of deionized water, and use an ultrasonic cell disruptor at a frequency of 20kHz and a power of 800W for 30min to obtain a uniform suspension of loofah nanocellulose.
[0027] As one of the preferred embodiments of the present invention, the specific process of step (3) is as follows:
[0028] A precursor solution was prepared by dissolving 20 mg of sodium lignin sulfonate and 0.65 g of lithium chloride in 10 ml of 0.3 M sodium hydroxide solution.
[0029] As one of the preferred embodiments of the present invention, in step (4), the mass ratio of the loofah nanocellulose suspension, deionized water, polyacrylamide, and precursor solution is (0.5-1.5):3:2:5.
[0030] As one of the preferred embodiments of the present invention, the specific process of step (4) is as follows:
[0031] Take 0.5-1.5g of loofah nanocellulose suspension, 3g of deionized water, 2g of polyacrylamide, 20mg of ammonium persulfate and 2mg of N,N-methylenebisacrylamide and mix them evenly by ultrasonication, pour in 5ml of precursor solution, stir evenly, pour into a polytetrafluoroethylene mold and seal it; after the hydrogel is formed, rinse with deionized water to clean the unreacted substances on the surface to obtain loofah nanocellulose hydrogel.
[0032] A loofah nanocellulose hydrogel is prepared by adopting the above preparation method.
[0033] An application of the loofah nanocellulose hydrogel in the field of flexible electronic preparation.
[0034] Preparation principle:
[0035] The present invention uses waste loofah as raw material, processes it into loofah cellulose through hydrogen peroxide and glacial acetic acid, and then uses a low eutectic solvent system (choline chloride / citric acid) to achieve efficient purification and nano-size of cellulose. Subsequently, sodium lignin sulfonate, sodium hydroxide, and lithium chloride are prepared into a precursor solution. Loofah nanocellulose, polyacrylamide, ammonium persulfate, N,N'-methylenebisacrylamide, and water are ultrasonically dispersed and added to the precursor solution to prepare a double network hydrogel. Li+ first acts as an oxidant to oxidize the catechol groups in the lignin molecules into quinone / semiquinone structures. Subsequently, ammonium persulfate is added to initiate a reduction reaction, converting the quinone / semiquinone portion back into catechol. Simultaneously, ammonium persulfate decomposes to produce sulfate radicals, hydroxyl radicals, and singlet oxygen. These radicals trigger the polymerization of acrylamide monomers in the water-organic solvent binary system, and through the synergistic effect of the chemical crosslinker N,N'-methylenebisacrylamide and the physical crosslinker loofah nanocellulose, a hydrogel with both mechanical and sensing properties is finally formed.
[0036] The advantages of the present invention over the prior art are:
[0037] (1) Luffa is agricultural waste (such as the fiber structure of mature luffa), and its use as a raw material can reduce resource waste and conform to the concept of sustainable development. The hydrogel prepared by the present invention using luffa as a raw material has good environmental friendliness, is green, natural and non-toxic, can be in direct contact with the skin, has low cost, and is widely planted (such as the industrial chain has been formed in Quzhou, Zhejiang), which can promote large-scale production and promote local economic development. It is conducive to its use and development in the fields of environmental protection, biomedicine, and flexible electronics (including electronic skin and wearable sensors).
[0038] (2) Carboxylated loofah nanocellulose with high dispersibility and high yield was prepared by using a ternary low eutectic solvent (DES); wherein, a low eutectic solvent is a eutectic mixture composed of two or more components, usually a hydrogen bond acceptor (HBA, such as quaternary ammonium salt) and a hydrogen bond donor (HBD, such as carboxylic acid, amide, polyol, etc.) that interacts through hydrogen bonds to form a melting point significantly lower than that of its individual components; it is biodegradable, low-toxic, recyclable, and easy to prepare, so it is considered to be a new green solvent; at the same time, since the hydrogen bonds between wood cellulose are more easily destroyed by the hydrogen bonds within DES molecules, DES can be used to loosen the cellulose fiber chains, partially reduce the degree of polymerization, increase the available active sites of cellulose macromolecules, and increase the porosity, thus becoming an ideal solution for improving the nanocellulose preparation process.
[0039] (3) Through alkali metal ions (Li + ) has weak oxidizing properties and realizes efficient catalysis through coordination, which is different from the traditional oxidizing metal ion system; catechol generated by lignin hydrolysis forms a complex with alkali metal ions, synergistically promoting the continuous generation of free radicals, realizing rapid polymerization of monomers, and giving hydrogel adhesion; the surface of loofah nanocellulose is rich in carboxyl and hydroxyl functional groups, which make the nanocellulose uniformly dispersed in the precursor solution, and can form a large number of hydrogen bonds, van der Waals forces and electrostatic interactions with functional groups such as carboxyl on the polyacrylamide chain in the hydrogel, and form coordination bonds with alkali metals, effectively enhancing the structural strength of the hydrogel; at the same time, alkali metal ions give the hydrogel a certain mechanical strength and conductivity; this catalytic system provides a new idea for the green and efficient preparation of multifunctional hydrogel electrolytes.
[0040] (4) The maximum elongation of the hydrogel finally obtained by the present invention reaches 1260.67%, the maximum breaking strength reaches 65.33 KPa, and the electrical conductivity is 5.45 S / m.
[0041] In summary, the loofah nanocellulose hydrogel prepared in the present invention has excellent biocompatibility, mechanical properties and conductivity, and has broad application prospects in the field of flexible electronics, including electronic skin and wearable sensors. The preparation process is simple, low-cost, and green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 1 and 2 are scanning electron microscopy results of the hydrogels of Example 2, Example 3, and Comparative Example 1 of the present invention (Figure a is a microscopic structure diagram of the hydrogel of Example 2; Figure b is a microscopic structure diagram of the hydrogel of Example 3; Figure c is a microscopic structure diagram of the hydrogel of Comparative Example 1);
[0043] Figure 2 FT-IR spectra of the hydrogels of Example 2 of the present invention and Comparative Example 1;
[0044] Figure 3 This is the zeta potential measurement result of the loofah nanocellulose in Example 2 of the present invention;
[0045] Figure 4 1 is the stress-strain curve of the hydrogels of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3;
[0046] Figure 5 is the conductivity result of the hydrogel of Example 2 of the present invention;
[0047] Figure 6 This is the tensile sensing performance result of the hydrogel in Example 2 of the present invention. DETAILED DESCRIPTION
[0048] The following examples of the present invention are described in detail. These examples are implemented based on the technical solutions of the present invention, and detailed implementation methods and specific operating procedures are given. However, the scope of protection of the present invention is not limited to the following examples. The raw materials, reagents, or devices used in the following examples, unless otherwise specified, can be obtained from conventional commercial channels or can be obtained by existing known methods; unless otherwise specified, the methods used in the examples of the present invention are methods known to those skilled in the art.
[0049] Example 1
[0050] The loofah nanocellulose hydrogel of this embodiment comprises the following steps:
[0051] (1) Loofah pretreatment
[0052] The skeleton of discarded loofah is removed and the loofah is cut into block loofahs; the block loofahs are dried at 80° C., placed in a grinder for grinding, and then passed through an 80-mesh sieve to obtain loofah powder.
[0053] (2) Extraction and bleaching of loofah cellulose
[0054] Prepare a glacial acetic acid-hydrogen peroxide solution by mixing 100 ml of glacial acetic acid and 100 ml of hydrogen peroxide in a 1:1 ratio. Mix 10 g of loofah powder with 200 ml of the glacial acetic acid-hydrogen peroxide solution and heat in a magnetic stirring heater at 80°C for 10 hours until the solution turns white. Filter the reaction product, wash it with deionized water until neutral, and then freeze-dry it in a freeze dryer to obtain purified loofah cellulose.
[0055] (3) Preparation of loofah nanocellulose
[0056] Anhydrous citric acid, choline chloride and deionized water were mixed in a mass ratio of 2:1:1 and magnetically stirred in an 80°C water bath for 20 minutes until a clear and transparent ternary low eutectic solvent was obtained; 2 g of purified loofah cellulose was dispersed in 60 ml of the ternary low eutectic solvent and reacted at a heating temperature of 130°C for 2 hours using an overhead stirrer at a stirring rate of 300 r / min; then, the reaction product was washed with deionized water and filtered until neutral, dispersed in 150 ml of deionized water, and ultrasonicated using an ultrasonic cell disruptor at a frequency of 20 kHz and a power of 800 W for 30 minutes to obtain a uniform loofah nanocellulose suspension, recorded as LF.
[0057] (4) Preparation of precursor solution
[0058] 1.2 g of sodium hydroxide was dissolved in 100 g of deionized water to obtain a 0.3 M sodium hydroxide aqueous solution; 20 mg of sodium lignin sulfonate and 0.65 g of lithium chloride were dissolved in 10 ml of the 0.3 M sodium hydroxide solution to prepare a precursor solution.
[0059] (5) Preparation of loofah nanocellulose hydrogel
[0060] 0.5 g of loofah nanocellulose suspension, 3 g of deionized water, 2 g of polyacrylamide, 20 mg of ammonium persulfate, and 2 mg of N,N-methylenebisacrylamide were mixed evenly by ultrasound, and 5 ml of the precursor solution was poured into the mixture. After stirring evenly, the mixture was poured into a polytetrafluoroethylene mold and sealed. After the hydrogel was formed, it was rinsed with deionized water to clean the unreacted substances on the surface to obtain the loofah nanocellulose hydrogel, which was recorded as PAM-LLi-LF. 0.5 Hydrogel.
[0061] Example 2
[0062] The loofah nanocellulose hydrogel of this embodiment comprises the following steps:
[0063] (1) Loofah pretreatment
[0064] Same as Example 1.
[0065] (2) Extraction and bleaching of loofah cellulose
[0066] Same as Example 1.
[0067] (3) Preparation of loofah nanocellulose
[0068] Same as Example 1.
[0069] (4) Preparation of precursor solution
[0070] Same as Example 1.
[0071] (5) Preparation of loofah nanocellulose hydrogel
[0072] Take 1.0g of loofah nanocellulose suspension, 3g of deionized water, 2g of polyacrylamide, 20mg of ammonium persulfate and 2mg of N,N-methylenebisacrylamide and mix them evenly by ultrasonication. Pour 5ml of precursor solution into it, stir evenly, and then pour it into a polytetrafluoroethylene mold and seal it. After the hydrogel is formed, rinse it with deionized water to clean the unreacted substances on the surface to obtain loofah nanocellulose hydrogel, which is recorded as PAM-LLi-LF1Hydrogel.
[0073] Example 3
[0074] The loofah nanocellulose hydrogel of this embodiment comprises the following steps:
[0075] (1) Loofah pretreatment
[0076] Same as Example 1.
[0077] (2) Extraction and bleaching of loofah cellulose
[0078] Same as Example 1.
[0079] (3) Preparation of loofah nanocellulose
[0080] Same as Example 1.
[0081] (4) Preparation of precursor solution
[0082] Same as Example 1.
[0083] (5) Preparation of loofah nanocellulose hydrogel
[0084] 1.5 g of loofah nanocellulose suspension, 3 g of deionized water, 2 g of polyacrylamide, 20 mg of ammonium persulfate, and 2 mg of N,N-methylenebisacrylamide were mixed evenly by ultrasound, and 5 ml of the precursor solution was poured into the mixture. After stirring evenly, the mixture was poured into a polytetrafluoroethylene mold and sealed. After the hydrogel was formed, it was rinsed with deionized water to clean the unreacted substances on the surface to obtain the loofah nanocellulose hydrogel, which was recorded as PAM-LLi-LF. 1.5 Hydrogel.
[0085] Comparative Example 1
[0086] The loofah nanocellulose hydrogel of this embodiment is basically the same as that of Example 2, with the main difference being that no loofah nanocellulose suspension is added in the hydrogel preparation in step (5). The obtained hydrogel is recorded as PAM-LLgHydrogel.
[0087] Comparative Example 2
[0088] The loofah nanocellulose hydrogel of this embodiment is basically the same as that of Example 2, except that sodium lignin sulfonate is not added in the preparation of the precursor solution in step (4); and no loofah nanocellulose suspension is added in the preparation of the hydrogel in step (5). The resulting hydrogel is designated as PAM-Li Hydrogel.
[0089] Comparative Example 3
[0090] The loofah nanocellulose hydrogel of this embodiment is basically the same as that of Example 2, except that in the hydrogel preparation in step (5), no loofah nanocellulose suspension and precursor solution are added (5 g of deionized water is used instead). The obtained hydrogel is recorded as PAM Hydrogel.
[0091] Experimental Example 1
[0092] This experimental example is used to verify the advantages of the hydrogel of the present invention.
[0093] The results were verified by scanning electron microscopy, FT-IR analysis, Zeta potential measurement, conductivity measurement, mechanical property evaluation, and tensile sensing performance. Figures 1 to 6 shown.
[0094] Figure 1 The scanning electron microscope results of the hydrogels of Example 2, Example 3 and Comparative Example 1 of the present invention are shown (Figure a is a microscopic structure diagram of the hydrogel of Example 2; Figure b is a microscopic structure diagram of the hydrogel of Example 3; Figure c is a microscopic structure diagram of the hydrogel of Comparative Example 1). It can be observed that the pore walls of Comparative Example 1 without the addition of loofah nanocellulose suspension are large and rough, and unevenly distributed, while the pore walls of Example 2 with the addition of loofah nanocellulose are dense and uniform, proving that the nanocellulose fills the pores of the hydrogel and reduces its pore size, which means that the addition of nanocellulose has a positive effect on the polymer network; however, with the further addition of nanocellulose, Example 3 shows a closed hydrogel pore (compared with Example 2), which is due to the excessive addition of nanocellulose, resulting in agglomeration.
[0095] Figure 2 The FT-IR spectra of the hydrogels of Example 2 and Comparative Example 1 of the present invention are shown in FIG. Figure 2 The results showed that after adding loofah nanocellulose, the peak continued to blue-shift to 3345 cm -1 , which is related to the increase in the number of hydrogen bonds between the nanocellulose and the hydrogel polymer network; 1729cm -1 The characteristic peak at 1729 cm represents the C=O vibration. -1The increase of the characteristic peak indicates that the phenolic hydroxyl and methoxy groups in lignin were successfully oxidized to semiquinone / quinone. The continued increase of the peak indicates the successful addition of carboxylated loofah nanocellulose; 1440 cm -1 The characteristic peak at represents CH stretching, and the increase of this peak in Example 2 also illustrates the successful introduction of nanocellulose.
[0096] Figure 3 The results of the zeta potential measurement of the loofah nanocellulose in Example 2 of the present invention are shown. Zeta potential is an important parameter for evaluating the stability and dispersibility of nanocellulose. The positive or negative value of the potential parameter represents whether the nanocellulose particles carry positive or negative ions on their surface. When the absolute value of the zeta potential is high (>30mV), it indicates that the electrostatic repulsion between the nanocellulose particles is strong, the nanocellulose particles are evenly dispersed in water, and are not prone to coagulation. Figure 3 The average zeta potential was -43.97 mV, which proved that loofah nanocellulose had good dispersibility and stability in water and was not prone to aggregation.
[0097] Figure 4 The stress-strain curves of the hydrogels of Examples 1 to 3 and Comparative Examples 1 to 3 of the present invention are shown in Figure 4. As shown in Figure 4, with the addition of loofah nanocellulose, the tensile properties of the hydrogel show a trend of first increasing and then decreasing. Among them, Example 2 shows the largest tensile strain of 1260.67%, and the tensile strength is increased to 65.33 kPa. On the one hand, this is because the loofah nanocellulose has very good dispersion in the hydrogel system, which can resist stress concentration and transfer energy between interfaces to prevent the hydrogel from cracking and expanding under large strain. On the other hand, due to the addition of Li + The multiple non-covalent interactions mediated by the hydrogels lead to the weakening of polymer chain constraints and segment dynamics, which synergistically improve the mechanical properties of the hydrogel. The downward trend shown in Example 3 is due to the fact that the excessive amount of loofah nanocellulose will cause agglomeration problems, induce stress concentration, and lead to a decrease in mechanical properties.
[0098] Figure 5 This is the conductivity diagram of the hydrogel in Example 2 of the present invention. The conductivity result is 5.45 S / m.
[0099] Figure 6 The figure shows the tensile sensing performance of the hydrogel in Example 2 of the present invention. The figure shows that the resistance change rate of the hydrogel remains stable under tensile strain conditions of 10% to 50%, and the difference in resistance peak change is less than 5%, demonstrating the excellent sensing performance of the hydrogel of the present invention under different strains.
[0100] In summary, the loofah nanocellulose hydrogel prepared in the present invention has excellent biocompatibility, mechanical properties and conductivity, and has broad application prospects in the field of flexible electronics, including electronic skin and wearable sensors. The preparation process is simple, low-cost, and green and environmentally friendly.
[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a loofah nanocellulose hydrogel, characterized in that, The steps include: (1) Extraction and bleaching of loofah cellulose The loofah powder and glacial acetic acid-hydrogen peroxide solution are mixed and stirred in a water bath until the solution turns white; the reaction product is filtered, washed to neutrality, and freeze-dried to obtain the loofah purified cellulose; (2) Preparation of loofah nanocellulose Anhydrous citric acid, choline chloride and deionized water are mixed and stirred in a water bath to react until a clear and transparent ternary deep eutectic solvent is obtained; The purified loofah cellulose prepared in step (1) is dispersed in the ternary deep eutectic solvent and reacted under stirring and heating conditions; the reaction product is washed and filtered to neutrality, dispersed in deionized water, and then subjected to ultrasonic treatment to obtain a loofah nanocellulose suspension; (3) Preparation of precursor solution Dissolve sodium lignin sulfonate and lithium chloride in sodium hydroxide solution to obtain a precursor solution; (4) Preparation of loofah nanocellulose hydrogel The loofah nanocellulose suspension obtained in step (2) is mixed with deionized water, polyacrylamide, ammonium persulfate, and N,N-methylenebisacrylamide, and the precursor solution prepared in step (3) is poured into the mixture. After stirring evenly, the mixture is poured into a mold and sealed. After the hydrogel is formed, the loofah nanocellulose hydrogel is obtained.
2. the preparation method of loofah nano cellulose hydrogel according to claim 1, is characterized in that, In the step (1), the method for obtaining the loofah powder is as follows: removing the skeleton of the discarded loofah and cutting it into block loofahs; and drying, grinding and sieving the block loofahs to obtain the loofah powder.
3. the preparation method of loofah nano cellulose hydrogel according to claim 1, is characterized in that, In the step (1), the glacial acetic acid-hydrogen peroxide solution is obtained by taking 100 ml of glacial acetic acid and 100 ml of hydrogen peroxide, respectively, and mixing them in a ratio of 1:
1.
4. the preparation method of loofah nano cellulose hydrogel according to claim 1, is characterized in that, The specific process of step (1) is as follows: Take 10g of loofah powder and mix it evenly with 200ml of glacial acetic acid-hydrogen peroxide solution, and heat it in a water bath at 80℃ in a magnetic stirring heater for 10 hours until the solution turns white; the reaction product is filtered and washed with deionized water until neutral, and then freeze-dried using a freeze dryer to obtain loofah purified cellulose.
5. the preparation method of loofah nano cellulose hydrogel according to claim 1, is characterized in that, The specific process of step (2) is as follows: Anhydrous citric acid, choline chloride, and deionized water were mixed in a mass ratio of 2:1:1 and magnetically stirred in a water bath at 80°C for 20 min until a clear and transparent ternary deep eutectic solvent was obtained; Take 2g of purified cellulose from loofah and disperse it in 60ml of a ternary low eutectic solvent. Use an overhead stirrer at a stirring rate of 300r / min and react at a heating temperature of 130°C for 2h. Then, wash the reaction product with deionized water, filter it until neutral, disperse it in 150ml of deionized water, and use an ultrasonic cell disruptor at a frequency of 20kHz and a power of 800W for 30min to obtain a uniform suspension of loofah nanocellulose.
6. the preparation method of loofah nano cellulose hydrogel according to claim 1, is characterized in that, The specific process of step (3) is as follows: A precursor solution was prepared by dissolving 20 mg of sodium lignin sulfonate and 0.65 g of lithium chloride in 10 ml of 0.3 M sodium hydroxide solution.
7. The preparation method of loofah nano cellulose hydrogel according to claim 1, wherein In the step (4), the mass ratio of the loofah nanocellulose suspension, deionized water, polyacrylamide, and precursor solution is (0.5-1.5):3:2:
5.
8. the preparation method of loofah nano cellulose hydrogel according to claim 1, is characterized in that, The specific process of step (4) is as follows: Take 0.5-1.5g of loofah nanocellulose suspension, 3g of deionized water, 2g of polyacrylamide, 20mg of ammonium persulfate and 2mg of N,N-methylenebisacrylamide and mix them evenly by ultrasonication, pour in 5ml of precursor solution, stir evenly, pour into a polytetrafluoroethylene mold and seal it; after the hydrogel is formed, rinse with deionized water to clean the unreacted substances on the surface to obtain loofah nanocellulose hydrogel.
9. A loofah nanocellulose hydrogel, characterized in that The preparation method is as described in any one of claims 1 to 8.
10. Use of the loofah nanocellulose hydrogel according to claim 9 in the field of flexible electronic preparation.
Citation Information
Cited By
Flexible hydrogel based on cellulose framework as well as preparation method and application of flexible hydrogel
CN120944140A
Gel electrolyte, preparation method thereof and battery
CN121484192A
Nano-cellulose reinforced composite hydrogel as well as preparation method and application thereof
CN121609935A