A corrosion-resistant fusion-bonded epoxy coating for a tank and a method of making the same

By preparing a fusion-bonded epoxy coating specifically for tank passages, the shortcomings of tank passage coating materials in terms of corrosion resistance, waterproofing, and aging resistance are solved. A dense network structure is formed, which improves the overall performance of the coating and makes it suitable for tank passage applications in humid or corrosive gas environments.

CN120590837BActive Publication Date: 2026-11-20SHANDONG HENGXIN COMPOSITE MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510962856.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-14
Publication Date
2026-11-20
Estimated Expiration
2045-07-14

AI Technical Summary

Technical Problem

Existing tank coating materials cannot effectively adjust their overall performance to suit their application environment, especially in terms of corrosion resistance, water resistance, aging resistance, and wear resistance.

Method used

A fusion-bonded epoxy coating specifically for tank passages is used, comprising epoxy resin, composite coated particles, dispersant, curing agent, leveling agent, defoamer, and antioxidant. It is prepared through a specific ratio and process to form a dense three-dimensional network structure, thereby improving the coating's corrosion resistance, water resistance, and aging resistance.

Benefits of technology

It achieves excellent performance of tank channel coating in humid or corrosive gas environments, improves coating stability and service life, and meets the high-performance requirements of tank channels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application relates to the field of paint, in particular to a tankway corrosion-resistant fusion-bonded epoxy coating and a preparation method thereof. The tankway corrosion-resistant fusion-bonded epoxy coating is prepared from raw materials including an epoxy resin, an accelerator, composite coated particles, a dispersing agent, a curing agent and a leveling agent. The prepared fusion-bonded epoxy coating not only has excellent corrosion resistance, but also can effectively maintain the waterproof, aging resistance and wear resistance of the coating, thereby meeting the application requirements of the tankway in a humid environment or containing corrosive gas, having very excellent market prospects, and providing a new solution for the coating material of the tankway.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of coatings, and more particularly to a corrosion-resistant fusion-bonded epoxy coating for tank passages and its preparation method. Background Technology

[0002] With the continuous development of the economy and industry, people's demand for coatings is also constantly increasing, especially for coatings with specific properties or high performance, which are in high demand in different fields and environments. Among them, as a key component of the mine hoisting system, the coating protection of the tank guide can effectively improve its wear resistance and corrosion resistance, and greatly improve the efficiency, safety and economy of the tank guide.

[0003] The hoisting guide is installed along the shaft axis, fixed to the guide beam or directly suspended from the headframe. It ensures the hoisting container can move precisely along a predetermined path and helps limit the risk of accidental falls, making it an indispensable safety feature in the hoisting system. The design and selection of the hoisting guide must comprehensively consider factors such as the specific conditions of the mine, the type of hoisting container, the hoisting speed, and economic efficiency, as the coating used also needs to meet various performance requirements.

[0004] Given the current application environment of tank passages, the coatings used in them have high requirements for corrosion resistance, waterproofing, aging resistance, wear resistance and noise reduction. However, existing coating materials cannot effectively adjust their overall performance to suit the application environment of tank passages, and the selection of coating materials for tank passages is generally limited.

[0005] Therefore, in order to effectively solve the above problems, this application provides a fusion-bonded epoxy coating for tank passages. The fusion-bonded epoxy coating obtained by this application not only has excellent corrosion resistance, but also effectively maintains the coating's waterproof, aging-resistant and wear-resistant properties, thereby meeting the application requirements of tank passages that are humid or contain corrosive gases. It has excellent market prospects and provides a new solution for coating materials of tank passages. Summary of the Invention

[0006] To address the aforementioned problems, the first aspect of this application provides a corrosion-resistant fusion-bonded epoxy coating for tank passages, comprising, by weight, 60-80 parts epoxy resin, 1-6 parts accelerator, 15-25 parts composite coated particles, 1-8 parts dispersant, 5-10 parts curing agent, 1-3 parts leveling agent, 1-3 parts defoamer, and 0.5-3 parts antioxidant.

[0007] As a preferred embodiment, the mass ratio of the epoxy resin, composite coated particles, and dispersant is (7~8):(1.8~2.2):(0.5~0.7).

[0008] As a preferred embodiment, the mass ratio of the epoxy resin, composite coated particles, and dispersant is (7.5~8):2:0.6.

[0009] As a preferred embodiment, the epoxy resin is a composition of phenolic modified epoxy resin and bisphenol F epoxy resin.

[0010] As a preferred embodiment, the mass ratio of the phenolic modified epoxy resin to the bisphenol F epoxy resin is (1~2):(4~5).

[0011] As a preferred embodiment, the mass ratio of the phenolic modified epoxy resin to the bisphenol F epoxy resin is (1~1.5):(4~4.5).

[0012] As a preferred embodiment, the epoxy equivalent of the bisphenol F epoxy resin is 150~200 g / eq.

[0013] As a preferred embodiment, the average viscosity of the bisphenol F epoxy resin is 2000~5000 cps / 25℃.

[0014] As a preferred embodiment, the average viscosity of the bisphenol F epoxy resin is 2500~3500 cps / 25℃.

[0015] As a preferred embodiment, the promoter is at least one selected from 2-methylimidazole, 2-ethylimidazole, cobalt octanoate, zinc naphthenate, triethylenetetramine, and diethylenetriamine.

[0016] As a preferred embodiment, the promoter is 2-methylimidazole.

[0017] As a preferred embodiment, the preparation method of the composite coated particles includes the following steps: S1: Mica powder, magnesium fluoride, and alumina are added to a ball mill jar in proportion, anhydrous ethanol is added to immerse the raw materials, polyvinylpyrrolidone is added, and the mixture is ball-milled at a ball-to-material ratio of (4~5):1 at a speed of 300~400 rpm for 3~4 hours; S2: The ball-milled slurry is transferred to a spray dryer with an inlet air temperature of 180~200℃ and an outlet air temperature of 90~100℃. The dried powder is collected, and the dried powder is added to a high-speed mixer with polytetrafluoroethylene and nano-titanium dioxide at a speed of 1300~1500 rpm and a high-speed mixing temperature of 25~35℃ for 20~30 minutes to obtain a mixed powder; S3: The mixed powder is placed in a muffle furnace and heated to 350~380℃ at a rate of 4.5~5℃ / min, and held at that temperature for 2~3 hours. After completion, it is naturally cooled to room temperature and passed through an 800~1000 mesh sieve to obtain the final product.

[0018] As a preferred embodiment, the average particle size of the nano-titanium dioxide is 10~25nm.

[0019] As a preferred embodiment, the average particle size of the mica powder is 10~15μm.

[0020] As a preferred embodiment, the magnesium fluoride has an average particle size of 100-150 nm; and the alumina has an average particle size of 50-80 nm.

[0021] As a preferred embodiment, the average particle size of the polytetrafluoroethylene is 1~2μm.

[0022] As a preferred embodiment, the mass ratio of mica powder, magnesium fluoride, alumina, polytetrafluoroethylene and nano titanium dioxide is (5~6):(1.5~1.8):(1.2~1.6):(2.5~3):(1.5~2).

[0023] As a preferred embodiment, the dispersant is a fatty alcohol polyoxyethylene ether.

[0024] As a preferred embodiment, the fatty alcohol polyoxyethylene ether is a composition of isomeric 13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether.

[0025] As a preferred embodiment, the mass ratio of the isomeric 13 fatty alcohol polyoxyethylene ether to cetearyl alcohol polyoxyethylene ether is (2~4):(0.8~1.4).

[0026] As a preferred embodiment, the hydroxyl value of the isomeric 13 fatty alcohol polyoxyethylene ether is 60~80 mgKOH / g.

[0027] As a preferred embodiment, the hydroxyl value of the cetearyl alcohol polyoxyethylene ether is 140~180 mgKOH / g.

[0028] By adding the aforementioned composite dispersant, this application not only effectively improves the dispersion of the composite coated particles in the epoxy resin system but also enhances the waterproof and aging-resistant properties of the coating. The addition of this composite dispersant allows for the intercalation of epoxy resin segments with different hydroxyl values ​​and chain lengths. This results in a denser three-dimensional network structure through the combination of long and short segments, increasing the entanglement strength between segments and intermolecular forces, reducing steric hindrance, and thus increasing the penetration resistance and path length of active molecules. Consequently, it maintains good property stability even in harsh environments, avoiding denaturation caused by chemical reactions. Furthermore, the denser network structure promotes the formation of a dense skin layer, significantly increasing the difficulty of forming a surface hydration layer and effectively improving waterproof performance.

[0029] As a preferred embodiment, the curing agent is at least one of dicyandiamide curing agents, phenolic resin modified curing agents, and acid anhydride curing agents.

[0030] As a preferred embodiment, the curing agent is a dicyandiamide-based curing agent.

[0031] As a preferred embodiment, the leveling agent is at least one of acrylate leveling agent, silicone leveling agent, and epoxidized soybean oil.

[0032] As a preferred embodiment, the leveling agent is epoxidized soybean oil.

[0033] As a preferred embodiment, the defoamer is at least one of silicone defoamers.

[0034] As a preferred embodiment, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 1135, antioxidant 1098, and antioxidant 268.

[0035] As a preferred embodiment, the antioxidant is antioxidant 1010 or antioxidant 268.

[0036] The second aspect of this application provides a method for preparing the above-mentioned corrosion-resistant fusion-bonded epoxy coating for tank passages. The preparation method includes the following steps: S1: Weigh all raw materials according to the required weight parts, mix them and add them to a high-speed mixer to mix evenly to obtain a mixture; S2: Add the mixture to a twin-screw extruder for melt extrusion, the extrusion temperature is 120~140℃, the extrusion frequency is 65~85Hz, the extruded material is cooled by the pressure roller, ground and sieved to obtain the fusion-bonded epoxy coating.

[0037] The beneficial effects of this application are:

[0038] 1. The corrosion-resistant fusion-bonded epoxy coating for tank passages provided in this application not only has excellent corrosion resistance, but also effectively maintains the coating's waterproof, aging-resistant, and wear-resistant properties, thereby meeting the application requirements of tank passages that are damp or contain corrosive gases. It has excellent market prospects and provides a new solution for coating materials for tank passages.

[0039] 2. The corrosion-resistant fusion-bonded epoxy coating for tank passages provided in this application has composite coated particles that not only achieve good dispersion in the resin system, but also further form a MgF2 / Al2O3 composite layer to resist acid and alkali corrosion, and promote the formation of a fluorine chain segment layer on the surface. This ensures that the surface is hydrophobic and has low surface energy, while also significantly improving the resistance to water molecule penetration, reducing its diffusion path, and thus improving the overall performance of the fusion-bonded epoxy coating.

[0040] 3. The corrosion-resistant fusion-bonded epoxy coating for tank passages provided in this application incorporates a composite dispersant that not only effectively aids in the dispersion of composite coated particles within the epoxy resin system but also significantly improves the coating's waterproof and aging-resistant properties. The addition of the composite dispersant enables the embedding of epoxy resin segments with different hydroxyl values ​​and chain lengths, thereby forming a denser three-dimensional network structure through the combination of long and short segments. This increases the entanglement strength between segments and intermolecular forces, reduces intermolecular steric hindrance, and thus increases the penetration resistance and path length of active molecules. Consequently, it maintains good property stability even under harsh environments, avoiding denaturation caused by chemical reactions. Furthermore, the denser network structure promotes the formation of a dense skin layer. Detailed Implementation

[0041] The technical solutions described above in this application will be further explained and demonstrated below with specific implementation schemes.

[0042] Example 1

[0043] A corrosion-resistant fusion-bonded epoxy coating for tank passages, comprising, by weight, 78 parts epoxy resin, 3 parts accelerator, 20 parts composite coated particles, 6 parts dispersant, 6 parts curing agent, 2 parts leveling agent, 1 part defoamer, and 2 parts antioxidant.

[0044] The epoxy resin is a composition of phenolic modified epoxy resin and bisphenol F epoxy resin, with a mass ratio of 1.2:4.3.

[0045] The phenolic modified epoxy resin was purchased from Baling Petrochemical's 704 epoxy resin; the bisphenol F epoxy resin was purchased from Mitsubishi Japan's JER807 F170 product, with an epoxy equivalent of 180 g / eq and an average viscosity of 3000 cps / 25℃.

[0046] The accelerator is 2-methylimidazole.

[0047] The preparation method of composite coated particles includes the following steps, by mass: S1: 5.4 parts mica powder, 1.6 parts magnesium fluoride and 1.5 parts alumina are added to a ball mill jar in proportion, 40 parts anhydrous ethanol is added to immerse the raw materials, and 0.5 parts polyvinylpyrrolidone K30 is added. The mixture is ball-milled at 400 rpm for 3 hours with a ball-to-material ratio of 5:1; S2: The ball-milled slurry is transferred to a spray dryer with an inlet air temperature of 200℃ and an outlet air temperature of 100℃. The dried powder is collected, and the dried powder is added to a high-speed mixer with 2.8 parts polytetrafluoroethylene and 1.8 parts nano titanium dioxide. The mixture is mixed at 1500 rpm and 30℃ for 30 minutes to obtain a mixed powder; S3: The mixed powder is placed in a muffle furnace and heated to 360℃ at a rate of 5℃ / min. The temperature is maintained for 2 hours. After completion, the mixture is naturally cooled to room temperature and passed through an 850-mesh sieve to obtain the final product.

[0048] The average particle size of nano-titanium dioxide is 20 nm.

[0049] The average particle size of the mica powder is 11.5 μm.

[0050] The average particle size of magnesium fluoride is 125 nm; the average particle size of alumina is 55 nm.

[0051] The average particle size of the polytetrafluoroethylene is 1.5 μm, and the corresponding particle size product was purchased from China Baiyi New Material Technology (Dongguan) Co., Ltd.

[0052] The dispersant is a composition of isomeric 13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether, with a mass ratio of 2.8:1.

[0053] The isomeric 13 fatty alcohol polyoxyethylene ether was purchased from product E-1312 sold by Haian Guoyun Chemical, with an average hydroxyl value of 78 mg KOH / g; the cetearyl alcohol polyoxyethylene ether was purchased from product O-3 sold by Haian Guoyun Chemical, with an average hydroxyl value of 145 mg KOH / g.

[0054] The curing agent was dicyandiamide curing agent K7108, purchased from Liuan Jietongda.

[0055] The leveling agent was epoxidized soybean oil, purchased from Shandong Duoju Chemical Co., Ltd. as an industrial-grade epoxidized acrylic soybean oil product.

[0056] The defoamer is silicone defoamer BYK-088; the antioxidant is antioxidant 1010.

[0057] A method for preparing a corrosion-resistant fusion-bonded epoxy coating for tank passages includes the following steps: S1: Weigh all raw materials according to the required weight parts, mix them and add them to a high-speed mixer to mix evenly to obtain a mixture; S2: Add the mixture to a twin-screw extruder for melt extrusion at an extrusion temperature of 125℃ and an extrusion frequency of 70Hz. After extrusion, the material is cooled by the pressure roller, ground and sieved to obtain the fusion-bonded epoxy coating.

[0058] Example 2

[0059] A corrosion-resistant fusion-bonded epoxy coating for tank passages, comprising, by weight, 70 parts epoxy resin, 3 parts accelerator, 22 parts composite coated particles, 5 parts dispersant, 6 parts curing agent, 2 parts leveling agent, 1 part defoamer, and 2 parts antioxidant.

[0060] The epoxy resin is a composition of phenolic modified epoxy resin and bisphenol F epoxy resin, with a mass ratio of 1:5.

[0061] The phenolic modified epoxy resin was purchased from Baling Petrochemical's 704 epoxy resin; the bisphenol F epoxy resin was purchased from Mitsubishi Japan's JER807 F170 product, with an epoxy equivalent of 180 g / eq and an average viscosity of 3000 cps / 25℃.

[0062] The accelerator is 2-methylimidazole.

[0063] The preparation method of composite coated particles includes the following steps, in parts by mass: S1: 5.4 parts mica powder, 1.6 parts magnesium fluoride and 1.5 parts alumina are added to a ball mill jar in proportion, 40 parts anhydrous ethanol is added to immerse the raw materials, and 0.5 parts polyvinylpyrrolidone K30 is added. The mixture is ball-milled at 400 rpm for 3 hours with a ball-to-particle ratio of 5:1; S2: The ball-milled slurry is transferred to a spray dryer with an inlet air temperature of 200℃ and an outlet air temperature of 100℃. The dried powder is collected, and the dried powder is added to a high-speed mixer with 2.8 parts polytetrafluoroethylene and 1.8 parts nano titanium dioxide. The mixture is mixed at 1500 rpm and 30℃ for 30 minutes to obtain a mixed powder; S3: The mixed powder is placed in a muffle furnace and heated to 360℃ at a rate of 5℃ / min. The temperature is maintained for 2 hours. After completion, the mixture is naturally cooled to room temperature and passed through an 850-mesh sieve to obtain the final product.

[0064] The average particle size of nano-titanium dioxide is 20 nm.

[0065] The average particle size of the mica powder is 11.5 μm.

[0066] The average particle size of magnesium fluoride is 125 nm; the average particle size of alumina is 55 nm.

[0067] The average particle size of the polytetrafluoroethylene is 1.5 μm, and the corresponding particle size product was purchased from China Baiyi New Material Technology (Dongguan) Co., Ltd.

[0068] The dispersant is a composition of isomeric 13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether, with a mass ratio of 2.8:1.

[0069] The isomeric 13 fatty alcohol polyoxyethylene ether was purchased from product E-1312 sold by Haian Guoyun Chemical, with an average hydroxyl value of 78 mg KOH / g; the cetearyl alcohol polyoxyethylene ether was purchased from product O-3 sold by Haian Guoyun Chemical, with an average hydroxyl value of 145 mg KOH / g.

[0070] The curing agent was dicyandiamide curing agent K7108, purchased from Liuan Jietongda.

[0071] The leveling agent was epoxidized soybean oil, purchased from Shandong Duoju Chemical Co., Ltd. as an industrial-grade epoxidized acrylic soybean oil product.

[0072] The defoamer is silicone defoamer BYK-088; the antioxidant is antioxidant 1010.

[0073] A method for preparing a corrosion-resistant fusion-bonded epoxy coating for tank passages includes the following steps: S1: Weigh all raw materials according to the required weight parts, mix them and add them to a high-speed mixer to mix evenly to obtain a mixture; S2: Add the mixture to a twin-screw extruder for melt extrusion at an extrusion temperature of 125℃ and an extrusion frequency of 70Hz. After extrusion, the material is cooled by the pressure roller, ground and sieved to obtain the fusion-bonded epoxy coating.

[0074] Comparative Example 1

[0075] The only difference between this comparative example and Example 1 is that the corrosion-resistant fusion-bonded epoxy coating for the tank channel, by weight, comprises: 100 parts epoxy resin, 3 parts accelerator, 10 parts composite coated particles, 3 parts dispersant, 6 parts curing agent, 2 parts leveling agent, 1 part defoamer, and 2 parts antioxidant.

[0076] Comparative Example 2

[0077] The only difference between this comparative example and Example 1 is that the preparation method of the composite coated particles includes the following steps, by mass: S1: 8.5 parts mica powder, 1.1 parts magnesium fluoride and 0.5 parts alumina are added to a ball mill jar in proportion, 40 parts anhydrous ethanol is added to immerse the raw materials, and 0.5 parts polyvinylpyrrolidone K30 is added. The mixture is ball-milled at 400 rpm for 3 hours with a ball-to-material ratio of 5:1; S2: The ball-milled slurry is transferred to a spray dryer with an inlet air temperature of 200°C and an outlet air temperature of 100°C. The dried powder is collected, and the dried powder is added to a high-speed mixer with 2.5 parts polytetrafluoroethylene and 2 parts nano titanium dioxide. The mixture is mixed at 1500 rpm and 30°C for 30 minutes to obtain a mixed powder; S3: The mixed powder is placed in a muffle furnace and heated to 360°C at a rate of 5°C / min. The temperature is maintained for 2 hours. After completion, the mixture is naturally cooled to room temperature and passed through an 850-mesh sieve to obtain the final product.

[0078] Comparative Example 3

[0079] The only difference between this comparative example and Example 1 is that the preparation method of the composite coated particles includes the following steps, by mass: S1: 3 parts mica powder, 2.5 parts magnesium fluoride and 2 parts alumina are added to a ball mill jar in proportion, 40 parts anhydrous ethanol is added to immerse the raw materials, 0.5 parts polyvinylpyrrolidone K30 is added, and the mixture is ball-milled at 400 rpm for 3 hours with a ball-to-material ratio of 5:1; S2: The ball-milled slurry is transferred to a spray dryer with an inlet air temperature of 200°C and an outlet air temperature of 100°C. The dried powder is collected, and the dried powder is added to a high-speed mixer with 1.4 parts polytetrafluoroethylene and 0.5 parts nano titanium dioxide. The mixture is mixed at 1500 rpm and 30°C for 30 minutes to obtain a mixed powder; S3: The mixed powder is placed in a muffle furnace and heated to 360°C at 5°C / min, held for 2 hours, and then naturally cooled to room temperature. The powder is then passed through an 850-mesh sieve to obtain the final product.

[0080] Comparative Example 4

[0081] The only difference between this comparative example and Example 1 is that the average particle size of the nano-titanium dioxide is 60 nm.

[0082] The average particle size of mica powder is 20.5 μm; the average particle size of alumina is 55 nm.

[0083] The average particle size of the polytetrafluoroethylene is 3.5 μm, and the corresponding particle size product was purchased from China Baiyi New Material Technology (Dongguan) Co., Ltd.

[0084] Comparative Example 5

[0085] The only difference between this comparative example and Example 1 is that the dispersant is a composition of isomeric 13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether in a mass ratio of 6:1.

[0086] Comparative Example 6

[0087] The only difference between this comparative example and Example 1 is that the dispersant is a composition of isomeric 13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether in a mass ratio of 1:1.

[0088] Furthermore, the isomeric 13 fatty alcohol polyoxyethylene ether was purchased from E-1302 product sold by Haian Guoyun Chemical, with an average hydroxyl value of 195 mg KOH / g.

[0089] Comparative Example 7

[0090] The only difference between this comparative example and Example 1 is that the cetearyl alcohol polyoxyethylene ether was purchased from O-9 product sold by Haian Guoyun Chemical, with an average hydroxyl value of 86 mgKOH / g.

[0091] Performance Evaluation

[0092] 1. The coatings prepared in the examples and comparative examples were subjected to cathodic disbondment resistance test according to the standard SY / T0315-1997. The test conditions were: 1.5V, 20℃, 28d. The results are recorded in Table 1.

[0093] 2. The coatings prepared according to the examples and comparative examples were used to prepare fusion-bonded coatings with a thickness of 400 μm. The surface water contact angle of the fusion-bonded coatings prepared according to the examples and comparative examples was tested using the seat drop method: 1.5 μL, time 10 s. The measured values ​​were the average of 10 tests and recorded in Table 1.

[0094] 3. The coatings prepared according to the examples and comparative examples were used to prepare fusion-bonded coatings with a thickness of 400 μm. The coating samples were placed in a constant temperature and humidity chamber at 65±2℃ and 75% humidity for 28 days. The coatings were subjected to a flattening test according to the method of CJ / T120-2016 to observe whether cracks and peeling phenomena appeared in the coatings. The test results were recorded in Table 1.

[0095] Table 1 Performance Evaluation Results

[0096] From the embodiments and comparative examples of this application, as well as the data results in Table 1, it can be seen that Examples 1 and 2 have significant performance advantages over Comparative Examples 1 to 7 in terms of waterproofness, corrosion resistance, and aging resistance. The composite dispersant adopted in Examples 1 and 2 with better technical solutions can not only effectively help the dispersion of composite coated particles in the epoxy resin system, but also effectively improve the waterproof and aging resistance of the coating. The addition of the composite dispersant can achieve the intercalation of epoxy resin segments with different hydroxyl values ​​and different chain lengths, thereby forming a denser three-dimensional network structure through the combination of long and short chain segments, increasing the entanglement strength between chain segments and the intermolecular forces, reducing the steric hindrance between molecules, thereby increasing the penetration resistance and path length of active molecules, and thus maintaining good property stability even in harsh environments.

Claims

1. A corrosion-resistant fusion-bonded epoxy coating for tank passages, characterized in that: 78 parts epoxy resin, 3 parts accelerator, 20 parts composite coated particles, 6 parts dispersant, 6 parts curing agent, 2 parts leveling agent, 1 part defoamer, and 2 parts antioxidant. The epoxy resin is a composition of phenolic modified epoxy resin and bisphenol F epoxy resin, with a mass ratio of 1.2:4.

3. The phenolic modified epoxy resin is Baling Petrochemical 704 epoxy resin; the bisphenol F epoxy resin is Mitsubishi JER807F170, with an epoxy equivalent of 180 g / eq and an average viscosity of 3000 cps / 25℃. The accelerator is 2-methylimidazole; The preparation method of the composite coated particles includes the following steps, by mass: S1: 5.4 parts mica powder, 1.6 parts magnesium fluoride and 1.5 parts alumina are added to a ball mill jar in proportion, 40 parts anhydrous ethanol is added to immerse the raw materials, and 0.5 parts polyvinylpyrrolidone K30 is added. The mixture is ball-milled at 400 rpm for 3 hours with a ball-to-material ratio of 5:1; S2: The ball-milled slurry is transferred to a spray dryer with an inlet air temperature of 200℃ and an outlet air temperature of 100℃. The dried powder is collected, and the dried powder is added to a high-speed mixer with 2.8 parts polytetrafluoroethylene and 1.8 parts nano titanium dioxide. The mixture is mixed at 1500 rpm and 30℃ for 30 minutes to obtain a mixed powder; S3: The mixed powder is placed in a muffle furnace and heated to 360℃ at a rate of 5℃ / min. The temperature is maintained for 2 hours. After completion, the mixture is naturally cooled to room temperature and passed through an 850-mesh sieve to obtain the final product. The average particle size of the nano-titanium dioxide is 20 nm. The average particle size of the mica powder is 11.5 μm; The average particle size of the magnesium fluoride is 125 nm. The average particle size of the alumina is 55 nm; The average particle size of the polytetrafluoroethylene is 1.5 μm; The dispersant is a composition of isomeric 13 fatty alcohol polyoxyethylene ether and cetearyl alcohol polyoxyethylene ether, with a mass ratio of 2.8:

1. The isomeric 13 fatty alcohol polyoxyethylene ether is E-1312, with an average hydroxyl value of 78 mgKOH / g; The cetearyl alcohol polyoxyethylene ether is O-3, with an average hydroxyl value of 145 mgKOH / g; The curing agent is dicyandiamide curing agent K7108; The leveling agent is epoxidized soybean oil; The defoamer is organosilicon defoamer BYK-088; The antioxidant is antioxidant 1010.

2. A method for preparing a corrosion-resistant fusion-bonded epoxy coating for tank passages according to claim 1, characterized in that: S1: Weigh all raw materials according to the required weight proportions, mix them and add them to a high-speed mixer to mix evenly to obtain a mixture; S2: Add the mixture to a twin-screw extruder for melt extrusion at an extrusion temperature of 125℃ and an extrusion frequency of 70Hz. After extrusion, cool the material by pressing the rollers, grind and sieve it to obtain a fusion-bonded epoxy coating.

Citation Information

Patent Citations

  • Petroleum pipeline repair coating composition as well as preparation method and application thereof

    CN118956236A

  • High-performance scratch-resistant wear-resistant corrosion-resistant nylon material replacing steel with plastic