An alpha-lipoic acid liposome photothermal response type hydrogel coating capable of inhibiting scars and promoting wound healing, and a preparation method and application thereof

By preparing α-lipoic acid liposome photothermal responsive hydrogel coatings, the shortcomings of existing technologies in inhibiting scarring and promoting wound healing have been overcome. Controlled release, antioxidant and lubricating properties have been improved, making it suitable for multiple applications in the biomedical field.

CN120605367BActive Publication Date: 2026-11-24SHANDONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510754506.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-06
Publication Date
2026-11-24
Estimated Expiration
2045-06-06

AI Technical Summary

Technical Problem

Existing hydrogel coatings that inhibit scarring and promote wound healing have shortcomings in terms of patient experience, wound healing rate, and controlled drug release. Anti-inflammatory and antibacterial effects lead to a poor experience, the wound healing rate is low, the electric current affects the body's internal circulation, and ordinary thioctic acid hydrogels cannot achieve controlled release and have poor bio-drag reduction properties.

Method used

An α-lipoic acid liposome photothermal responsive hydrogel coating is used. The active hydroxyl groups are activated by plasma treatment of the substrate surface, and KH570 and TPO-L are combined to form an initiator layer. Ultraviolet light initiates the polymerization of methacrylate gelatin and methacrylate sulfobetaine. MXene is added to achieve photothermal responsive controllable release of α-lipoic acid, which enhances lubrication performance and mechanical durability.

Benefits of technology

It achieves controlled release of α-lipoic acid, improves wound healing rate, enhances antioxidant and lubricating properties, has good bio-drag reduction properties, provides a good patient experience, and is suitable for multiple applications in the biomedical field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005438306980000011
    Figure HDA0005438306980000011
  • Figure HDA0005438306980000012
    Figure HDA0005438306980000012
  • Figure HDA0005438306980000021
    Figure HDA0005438306980000021
Patent Text Reader

Abstract

This invention provides an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing, along with its preparation method and applications. The preparation method of the hydrogel coating includes the following steps: plasma treatment of the substrate, immersion in KH570 solution, immersion in TPO-L ethyl acetate solution, and finally immersion in a hydrogel precursor solution, followed by reaction to obtain the final product. The hydrogel coating of this invention exhibits the effects of inhibiting scarring, promoting tissue regeneration and wound healing, accelerating the wound healing rate, and providing a better patient experience. Furthermore, the introduction of MXene into the hydrogel coating results in excellent photothermal responsiveness, thereby enabling the controlled release of α-lipoic acid liposomes. The hydrogel coating of this invention not only possesses excellent antioxidant properties but also good lubrication properties and mechanical durability, exhibiting good bio-drag reduction properties, making it promising for applications in the biomedical field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the fields of biomedicine and hydrogels, specifically relating to an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing, as well as its preparation method and application. Background Technology

[0002] Hydrogel coatings, combining the functions of hydrogels and substrates, have shown great potential in biomedical applications. Currently, hydrogel coating technologies targeting scar inhibition and wound healing can effectively suppress scar formation and promote wound healing through various mechanisms (such as anti-inflammatory, antioxidant, antibacterial, and angiogenesis-promoting effects). These hydrogel coatings have wide applications in the clinical treatment of chronic wounds and scar management. For example, Chinese patent document CN118949107A discloses an antibacterial dressing for promoting wound healing, its preparation method, and the application method. This invention, in principle, uses gelatin and quaternary ammonium salts to form a gel copolymer network, and adds long-chain polyhydroxy alcohols to it. The hydroxyl groups of the alcohol endow the hydrogel with water and oxygen adsorption properties, which can increase the oxygen concentration at the wound site, thus promoting the healing of tissues outside the injury. In addition, there are also reports of hydrogels that promote wound healing through a dual method of electric current and electro-controlled drug release using electro-assisted means. For example, Chinese patent document CN119184963A discloses an electro-controlled drug release hydrogel patch for wound healing. In this hydrogel patch, the surface of the conductive hydrogel exposed and fitted with a sheet-like electrode with a central opening serves as the treatment surface facing the wound. This allows for long-term, continuous replenishment of medication within the hydrogel and programmed drug release, promoting wound healing through the synergistic effect of electrical stimulation and drug release. While the above patents primarily achieve wound healing through anti-inflammatory and antibacterial mechanisms, these methods can lead to a poor patient experience, slower wound healing rates, and potential impacts on the body's internal circulation from the electrical current.

[0003] Inflammation is a crucial mechanism in scar formation. Hydrogel coatings can effectively reduce inflammation by regulating the release of inflammatory factors, thereby inhibiting scar formation. Recently, Liu et al. developed a tough, antibacterial, and antioxidant hydrogel dressing that accelerates wound healing and inhibits hypertrophic scar formation in infected wounds. This hydrogel dressing, through its dual-network structure combining polyvinyl alcohol (PVA) and agarose, exhibits excellent anti-inflammatory properties, significantly reducing inflammation in infected wounds and thus inhibiting scar hyperplasia (Liu X, Sun Y, Wang J, et al. A tough, antibacterialand antioxidant hydrogel dressing accelerates wound healing and suppresses hypertrophic scar formation in infected Wounds [J]. Bioactive Materials, 2024, 34:269–281.). Besides inflammation, oxidative stress is also an important mechanism in scar formation. Hydrogel coatings can inhibit scar formation by scavenging reactive oxygen species (ROS) and reducing oxidative stress-induced tissue damage. Recently, Zhang et al. constructed a biodegradable hydrogel (VP-gel) loaded with verteporfin, which can continuously release antioxidants, effectively scavenge ROS, promote wound healing and reduce scar formation (Zhang C, Yang D, Wang TB, et al. Biodegradablehydrogels with photodynamic antibacterial activity promote wound healing and mitigate scar Formation [J]. Biomaterials Science, 2023, 11(1): 288–297.).

[0004] Furthermore, hydrogel coatings can effectively inhibit scar formation through multiple mechanisms, including antibacterial activity, promotion of angiogenesis, and regulation of collagen synthesis and degradation. Their multifunctional synergistic effect provides an ideal environment for wound healing. Hydrogel coatings have shown great potential in clinical applications, especially in the aforementioned wound healing and scar inhibition aspects.

[0005] Reported scar-inhibiting hydrogel coatings mainly rely on the regulation of inflammatory responses; or on the structural treatment of the hydrogel coating by synthesizing reducing molecules to enable the hydrogel coating to scavenge ROS; or on drug sustained release through electro-assisted methods. Alpha-lipoic acid, as a potent antioxidant, has received increasing attention in the biomedical field in recent years. To improve its bioavailability and stability, researchers have developed various nanocarrier systems, including liposomes and hydrogels, and have initially applied them to biological systems. For example, Chinese patent document CN115232329A discloses a lipoic acid hydrogel, its preparation method, and its applications. The lipoic acid hydrogel prepared by this invention can achieve efficient self-healing, and has injectability, high self-healing efficiency, and temperature sensitivity, and can be used in adhesives and dressings. The lipoic acid hydrogel obtained by this patent achieves the expected wound healing through an antioxidant pathway, but it does not solve the problem of controlled release of lipoic acid. Chinese patent document CN 115337446A discloses a method for preparing a bio-based adhesive hydrogel patch that promotes wound healing, its products, and its applications. The preparation method of this hydrogel patch involves reacting a mixture of lipoic acid and cytosine to obtain lipoic acid cytosine; reacting a mixture of gelatin and methacrylic anhydride to obtain methacrylated gelatin (GelMA); and blending lipoic acid cytosine and GelMA and heating the mixture to polymerize and obtain a bio-based adhesive hydrogel patch. The hydrogel patch prepared by this invention combines the natural molecules lipoic acid and cytosine with gelatin, which can effectively promote wound healing. However, this system does not contain any material components that can respond to external stimuli, preventing the hydrogel patch from responsively releasing lipoic acid under photothermal or other external stimuli; furthermore, the bio-drag-reducing properties of the lipoic acid component in this invention need further improvement.

[0006] In summary, existing hydrogels that inhibit scarring and promote wound healing mainly achieve the desired wound healing through anti-inflammatory, antibacterial, and antioxidant pathways. However, while anti-inflammatory and antibacterial hydrogels achieve the desired wound healing through anti-inflammatory and antibacterial pathways, the anti-inflammatory and bactericidal effects can lead to a poor patient experience, a slower wound healing rate, and potential impacts on the body's internal circulation from the electrical current. Ordinary thioctic acid hydrogel coatings have the ability to scavenge ROS and can inhibit scar formation, but they cannot achieve controlled release and have poor bio-drag reduction properties. Summary of the Invention

[0007] To address the shortcomings of existing technologies in terms of patient experience, wound healing rate, and controlled drug release, this invention provides an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing, along with its preparation method and applications. The preparation method and raw material composition of the α-lipoic acid liposome hydrogel coating of this invention are simple, low-cost, scalable, environmentally friendly, easy to clean, and recyclable. The α-lipoic acid liposome hydrogel coating of this invention utilizes the ROS-scavenging properties of α-lipoic acid to inhibit scarring, promote tissue regeneration, and accelerate wound healing, resulting in a better patient experience. Furthermore, the introduction of MXene into the α-lipoic acid liposome hydrogel coating, with its excellent photothermal responsiveness, enables the controlled release of α-lipoic acid liposomes. The α-lipoic acid liposome hydrogel coating prepared by this invention not only possesses excellent antioxidant properties but also good lubrication and mechanical durability, exhibiting excellent bio-drag reduction properties, making it promising for broad applications in the biomedical field.

[0008] The technical solution of the present invention is as follows.

[0009] A method for preparing an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing includes the following steps:

[0010] (1) The substrate was subjected to plasma treatment, then immersed in propyl 3-(trimethyloxysilyl)methacrylate (KH570) solution and dried to obtain a KH570 treated substrate;

[0011] (2) The KH570-treated substrate was soaked in an ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) ethyl acetate solution and dried to obtain an initiator-treated substrate;

[0012] (3) The substrate treated with the initiator was immersed in the hydrogel precursor solution, and the reaction was carried out to obtain an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing.

[0013] The hydrogel precursor solution is a dispersion of methacrylated gelatin (GeLMA), methacrylate sulfobetaine, α-lipoic acid liposomes, MXene, and water.

[0014] According to a preferred embodiment of the present invention, in step (1), the substrate material is selected from polyethylene terephthalate or high-density polyethylene.

[0015] According to a preferred embodiment of the present invention, step (1) further includes the following steps before plasma treatment: ultrasonically cleaning the substrate to remove impurities on the surface and drying it in clean air.

[0016] According to a preferred embodiment of the present invention, in step (1), the conditions for plasma treatment are: pressure 5-20 Pa, power 5-20 W, and plasma treatment time 3-8 minutes, preferably 5 minutes.

[0017] According to a preferred embodiment of the present invention, in step (1), the solvent used for the 3-(trimethyloxysilyl)methacrylate (KH570) solution is a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1-2:1; the content of 3-(trimethyloxysilyl)methacrylate in the 3-(trimethyloxysilyl)methacrylate (KH570) solution is 1-5 wt%. The amount of 3-(trimethyloxysilyl)methacrylate (KH570) solution used is only enough to submerge the substrate.

[0018] According to a preferred embodiment of the present invention, in step (1), the soaking temperature is room temperature and the soaking time is 1-5 hours.

[0019] According to a preferred embodiment of the present invention, in step (2), the concentration of the ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) ethyl acetate solution is 1-5 wt%. The amount of ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) ethyl acetate solution used is only enough to submerge the substrate.

[0020] According to a preferred embodiment of the present invention, in step (2), the immersion temperature is room temperature and the immersion time is 20-40 seconds. After immersion, as the solvent evaporates, a stable initiator layer is formed on the substrate surface.

[0021] According to a preferred embodiment of the present invention, in step (3), the α-lipoic acid liposomes are composed of α-lipoic acid and a lipid membrane coated on the surface of α-lipoic acid, the lipid membrane being composed of soybean lecithin and cholesterol; the α-lipoic acid liposomes are added to the system in the form of an α-lipoic acid liposome suspension, wherein the solvent of the α-lipoic acid liposome suspension is a phosphate buffer solution with pH 7.4, and the concentration of the α-lipoic acid liposomes is 7-7.5 g / L.

[0022] According to a preferred embodiment of the present invention, in step (3), the preparation method of the α-lipoic acid liposome suspension is a membrane hydration method, comprising the following steps: dissolving soybean lecithin, cholesterol, and α-lipoic acid in dichloromethane, removing the dichloromethane by rotary evaporation to form a uniform thin lipid membrane; adding phosphate buffered saline (PBS) for hydration treatment; and then filtering to obtain the α-lipoic acid liposome suspension. Preferably, the mass ratio of soybean lecithin to cholesterol is 1-3:1, the total mass of soybean lecithin and cholesterol to the mass ratio of α-lipoic acid is 3-4:1; the mass ratio of α-lipoic acid to the volume ratio of dichloromethane is 2-3 g / L; the rotary evaporation temperature is 40℃; the pH of the phosphate buffer is 7.4, and the mass ratio of α-lipoic acid to the volume ratio of the phosphate buffer is 1.5-2 g / L; the hydration treatment method is as follows: ultrasonic treatment at 35-45℃ for 3-10 min, and then ultrasonic treatment at -5-5℃ for 15-25 min; the filter membrane has a specification of 0.45 μm.

[0023] According to a preferred embodiment of the present invention, in step (3), the mass ratio of methacrylated gelatin (GeLMA), methacrylate sulfobetaine, α-lipoic acid liposomes, and MXene is 8-12:4-8:2-3:0.01-0.2, preferably 10:5:2-3:0.01-0.1, and more preferably 10:5:2.5:0.1.

[0024] According to a preferred embodiment of the present invention, in step (3), the mass ratio of MXene to water is 1-5 mg / mL.

[0025] According to a preferred embodiment of the present invention, in step (3), the reaction conditions are as follows: reaction under ultraviolet light irradiation for 20-50 seconds, then the ultraviolet light is removed, and the mixture is left to stand at room temperature for 5-50 seconds; the ultraviolet light irradiation power is 800-1200W. Under ultraviolet light irradiation, the free radicals generated by the oil-soluble TPO-L initiator promote the growth of the hydrogel coating from the substrate surface, thereby forming a uniform and stable α-lipoic acid liposome hydrogel coating.

[0026] An α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing was prepared by the above method.

[0027] The above-mentioned α-lipoic acid liposome photothermal responsive hydrogel coating, which can inhibit scarring and promote wound healing, is used in the preparation of drugs or dressings that can inhibit scarring and promote wound healing.

[0028] The technical features and beneficial effects of this invention are as follows:

[0029] 1. This invention utilizes plasma treatment of the substrate surface to activate the active hydroxyl groups. The treated substrate is then immersed in a KH570 solution. The silanol functional groups hydrolyzed by KH570 undergo a condensation reaction with the active hydroxyl groups to form covalent siloxane bonds. After the siloxane bonds are formed, the treated substrate is immersed in an ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) ethyl acetate solution. As the solvent evaporates, a stable initiation layer gradually forms on the substrate surface. The substrate containing the initiation layer was then immersed in a hydrogel precursor solution and irradiated with ultraviolet light. Oil-soluble TPO-L, acting as an initiator, generated free radicals, promoting the graft polymerization of methacrylated gelatin (GeLMA) and methacrylate sulfonate betaine from the substrate surface (the covalent siloxane bonds formed by KH570 treatment of the substrate can undergo graft polymerization with GeLMA and methacrylate sulfonate betaine). Further free radical polymerization resulted in a network structure, yielding a uniform and stable α-lipoic acid liposome hydrogel coating. α-lipoic acid liposomes and MXene were uniformly dispersed within the α-lipoic acid liposome hydrogel coating. This invention provides a simple, low-cost, scalable, environmentally friendly, easy-to-clean, and recyclable method for preparing the α-lipoic acid liposome hydrogel coating.

[0030] 2. In the α-lipoic acid liposome hydrogel coating of this invention, GelMA and sulfobetaine methacrylate form covalent bonds through free radical polymerization. α-Lipoic acid liposomes and MXene are uniformly dispersed in the three-dimensional network hydrogel obtained by the polymerization of GelMA and sulfobetaine methacrylate. In addition to the covalent bonds between GelMA and sulfobetaine methacrylate, electrostatic interactions and hydrogen bonds exist between the α-lipoic acid liposomes and the backbone structures of GelMA and sulfobetaine methacrylate, enhancing the interactions between the hydrogel components. The polymerization of GelMA and sulfobetaine methacrylate together constitutes the network backbone structure of the α-lipoic acid liposome hydrogel coating, giving the hydrogel stability and allowing for molding. The incorporation of α-lipoic acid liposomes not only improves the coating's lubrication properties but also imparts antioxidant and antibacterial properties. The photothermal responsiveness of MXene allows the α-lipoic acid liposome hydrogel coating of this invention to absorb light energy and convert it into heat energy under NIR irradiation, enabling the α-lipoic acid liposomes to release α-lipoic acid in a controlled manner.

[0031] 3. The α-lipoic acid liposome hydrogel coating of this invention utilizes the ROS-scavenging properties of α-lipoic acid to inhibit scarring, promote tissue regeneration, and promote wound healing. Through the NIR photothermal effect, α-lipoic acid molecules can be continuously and controllably released to clear excess ROS, reduce the level of reactive oxygen species around the wound, and decrease local tissue inflammation. α-Lipoic acid can also promote the proliferation of endothelial cells and smooth muscle cells, while inhibiting the fibrosis process, thus promoting wound healing, tissue regeneration, and inhibiting scar formation. Through the encapsulation of α-lipoic acid liposomes and hydrogel, the stability, bioavailability, and targeting of α-lipoic acid are improved. The α-lipoic acid liposomes and hydrogel demonstrate potential applications in clinical treatment across multiple fields, including wound healing, anti-oxidation, antibacterial, and skin care.

[0032] 4. The α-lipoic acid liposome hydrogel coating prepared by this invention not only possesses excellent antioxidant properties but also exhibits good lubrication properties and mechanical durability, making it promising for broad applications in the biomedical field. The α-lipoic acid liposome hydrogel coating of this invention has an ultra-low coefficient of friction (0.001) and a high surface grafting density. The hydrophobicity of α-lipoic acid liposomes enhances the lubrication properties of the coating, resulting in an ultra-low coefficient of friction and excellent bio-drag reduction performance. Because the interaction between the α-lipoic acid liposome hydrogel coating and the substrate surface consists of stronger covalent bonds, the coating exhibits excellent mechanical durability, maintaining structural integrity even after 24 hours of ultrasonic cleaning (400 W) or 10,000 cycles of bending. In preparing the α-lipoic acid liposome hydrogel coating, the present invention uses a photoinitiation method to graft and polymerize the hydrogel precursor on the substrate surface. The photoinitiated grafting polymerization and the presence of the initiation layer on the substrate surface increase the reaction sites on the substrate, giving the α-lipoic acid liposome hydrogel coating of the present invention a high surface grafting density.

[0033] 5. The α-lipoic acid liposome hydrogel coating prepared by this invention has the ability to controllably release α-lipoic acid. The mechanism is that MXene has good photothermal responsiveness, which enables the controllable release of α-lipoic acid liposomes: when the α-lipoic acid liposome hydrogel coating is irradiated with NIR, due to the photothermal effect, MXene absorbs light energy and converts it into heat energy, thereby releasing α-lipoic acid and achieving controllable release.

[0034] 6. In the preparation method of this invention, if plasma treatment is not performed, the active hydroxyl groups on the substrate surface cannot be activated and cannot undergo a condensation reaction with KH570 to form siloxane bonds. Similarly, without KH570 treatment, a condensation reaction cannot occur to form siloxane bonds. If sulfobetaine methacrylate is not added, the hydrogel network framework structure is unstable and cannot be formed. In the hydrogel precursor solution, the ratio of raw materials methacrylated gelatin (GeLMA), sulfobetaine methacrylate, α-lipoic acid liposomes, and MXene needs to be appropriate. If too much MXene is added, it will overheat under NIR irradiation; if α-lipoic acid liposomes are replaced with α-lipoic acid, the lubrication performance of the hydrogel coating will decrease. Attached Figure Description

[0035] Figure 1 The curves show the relationship between the storage modulus (G') and loss modulus (G") of the hydrogel coatings obtained in Comparative Examples 1 and 3.

[0036] Figure 2 The appearance of the α-lipoic acid liposome hydrogel coating (substrate is PET) prepared for Comparative Example 1 after 10,000 cycles of bending (the left image is in the stretched state after 10,000 cycles of bending, and the right image is in the contracted state after 10,000 cycles of bending).

[0037] Figure 3 The appearance of the α-lipoic acid liposome hydrogel coating (substrate: PET) prepared in Comparative Example 1 before and after 24 hours of ultrasonic cleaning (ultrasonic power: 400W).

[0038] Figure 4 The image shows a comparison of the water contact angle of the α-lipoic acid liposome hydrogel coating (PET substrate) prepared in Comparative Example 1 before and after 10,000 cyclic bending cycles and ultrasonic cleaning.

[0039] Figure 5 (a) is a graph showing the hemolytic ability of hydrogel samples from Examples 1, 2, and 3 on fresh rat erythrocytes; (b) and (c) are schematic diagrams showing the viability and proliferation capacity of DF cells during the quantitative proliferation process obtained by the CCK-8 assay of hydrogel samples from Examples 1, 2, and 3; (d) and (e) are graphs showing the ROS level of DF cells in hydrogel samples from Examples 1, 2, and 3; (f) is a graph showing the quantitative determination of the expression levels of COL1A1 and MKi67 by immunofluorescence staining of hydrogel samples from Examples 1, 2, and 3.

[0040] Figure 6(a) A full-thickness resection model of mouse wounds in the hydrogel sample groups of Example 1, Comparative Example 2, and Comparative Example 3; (b) Immunofluorescence staining images of MYHI1+ in the hydrogel sample groups of Example 1, Comparative Example 2, and Comparative Example 3 on days 5 and 10 post-injury; (c) Immunofluorescence staining images of MKi67+ (proliferating cells) in the hydrogel sample groups of Example 1, Comparative Example 2, and Comparative Example 3 on days 5 and 10 post-injury; (d) Images of C in the hydrogel sample groups of Example 1, Comparative Example 2, and Comparative Example 3. Immunofluorescence staining images of NN1+ (smooth muscle cells) on day 5 and day 10 after injury; (e) a graph showing the changes in CD45+, CD31+, and MKi67+ cells over time in Example 1, Comparative Example 2, and Comparative Example 3; (f) a comparison of mRNA levels of fibrosis-related genes (Col1a1, Col3a1, Co3a1, Postn, Ctgf) and inflammatory factors (Mcp1, Tnfa, IL6) in Example 1, Comparative Example 2, and Comparative Example 3.

[0041] Figure 7 The images show the adsorption of Staphylococcus aureus on the surfaces of surgical sutures (blank sample), surgical sutures coated with hydrogels prepared by the method of Comparative Example 4 (GelMA) without NIR irradiation, surgical sutures coated with α-lipoic acid liposome hydrogels prepared by the method of Example 1 (Ge@PS-L-MX1) without NIR irradiation, and surgical sutures coated with α-lipoic acid liposome hydrogels prepared by the method of Example 1 (NIR-irradiated Ge@PS-L-MX1).

[0042] Figure 8 (a) is a schematic diagram of the friction test of the hydrogel coating; Figure 8 (b) and Figure 8 (c) The coefficient of friction of the hydrogel coatings prepared by the methods of Comparative Example 4 (GelMA), Comparative Example 3 (Ge@PS) and Comparative Example 1 (Ge@PS-L) under a constant normal force of 1 N and a constant rotation speed of 30 rad / min; Figure 8 (d) shows the friction coefficient of the hydrogel coatings prepared by the method of Example 1 (Ge@PS-L-MX1) and Comparative Example 1 (Ge@PS-L) under a constant normal force of 1 N and a constant rotation speed of 30 rad / min.

[0043] Figure 9 (a) Temperature variation of hydrogel coatings with different MXene contents under NIR irradiation (0.839 W); Figure 9 (b) Infrared thermal imaging of the hydrogel coatings prepared by the methods of Comparative Example 1 (Ge@PS-L-MX0) and Example 1 (Ge@PS-L-MX1) under NIR irradiation (0.839 W). Detailed Implementation

[0044] The present invention will be further described below through specific embodiments, but is not limited thereto.

[0045] Unless otherwise specified, all raw materials used in the embodiments are commercially available products; all equipment used is conventional equipment unless otherwise specified.

[0046] In the examples, methacrylated gelatin (molecular weight 100-200 kDa) was purchased from Aladdin Company. MXene was purchased from Fukuyama Information Technology Co., Ltd.

[0047] Example 1

[0048] Preparation of an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing:

[0049] (1) Before preparing the α-lipoic acid liposome hydrogel coating, the PET substrate was ultrasonically cleaned to remove impurities on the surface and dried with clean air.

[0050] (2) The PET substrate was subjected to plasma treatment in a vacuum (pressure of 10 Pa) and a power of 10 W for 5 minutes, and then immersed in a KH570 solution with a concentration of 3 wt% (the solvent is a mixture of ethanol and water, with a volume ratio of ethanol to water of 1:1) at room temperature for 2 hours (the amount of KH570 solution used is only enough to submerge the PET substrate). The PET substrate was then removed and dried at room temperature to obtain the KH570 treated PET substrate.

[0051] (3) The KH570-treated PET substrate was placed in an ethyl acetate solution containing 1 wt% ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) (the amount of ethyl acetate solution containing ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) was only enough to submerge the PET substrate), and immersed at room temperature for 30 seconds. After that, the PET substrate was removed and allowed to evaporate and dry to obtain the initiator-treated PET substrate. As the solvent evaporated, a stable initiator layer was formed on the surface of the PET substrate.

[0052] (4) The PET substrate treated with the initiator was immersed in a hydrogel precursor solution, which was a dispersion of GeLMA, methacrylic acid sulfobetaine, α-lipoic acid liposome suspension, MXene and water, wherein the mass ratio of GeLMA, methacrylic acid sulfobetaine, α-lipoic acid liposome and MXene was 10:5:2.5:0.1; and the mass ratio of MXene to the volume ratio of the above water was 1 mg / mL.

[0053] α-Lipoic acid liposomes consist of α-lipoic acid and a lipid membrane coating the surface of α-lipoic acid. The lipid membrane is composed of soybean lecithin and cholesterol. The α-lipoic acid liposome suspension was prepared using a thin-film hydration method, with the following steps: Soybean lecithin and cholesterol were weighed at a mass ratio of 2:1 (total mass 0.168 g), and dissolved together with 0.05 g of α-lipoic acid in 20 mL of dichloromethane, placed in a round-bottom flask. The dichloromethane was evaporated at 40°C using a rotary evaporator, forming a uniform thin lipid membrane on the inner wall of the flask. Subsequently, at the same temperature, the lipid membrane was hydrated with 30 mL of pH 7.4 phosphate-buffered saline (PBS). The hydration treatment method was as follows: ultrasonic treatment at 40°C (ultrasonic power 200 W) for 5 min; then, it was placed in an ice-water bath and treated with probe ultrasonic treatment (40% amplitude, 20 min), with the probe tip slightly below the liquid surface (immersion depth approximately 3-5 mm). Finally, the obtained liposome dispersion was filtered through a 0.45 μm filter membrane to obtain a uniform liposome suspension, which was then stored at 4 °C.

[0054] (5) The reaction was carried out at room temperature for 30 seconds under ultraviolet light irradiation (1000W) until the initiation layer was formed, and then allowed to stand at room temperature (without ultraviolet light irradiation) for 10 seconds to obtain the α-lipoic acid liposome hydrogel coating. The free radicals generated by the oil-soluble TPO-L initiator promoted the growth of the hydrogel coating from the PET substrate surface, thereby forming a uniform and stable α-lipoic acid liposome hydrogel coating.

[0055] Example 2

[0056] The preparation of an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing is as described in Example 1, except that: in step (4), the concentration of MXene is 0.5 mg / ml (the mass ratio of MXene to the volume ratio of water); other steps and conditions are the same as in Example 1.

[0057] Example 3

[0058] The preparation of an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing is as described in Example 1, except that: in step (4), the concentration of MXene is 0.1 mg / ml (the mass ratio of MXene to the volume ratio of water); other steps and conditions are the same as in Example 1.

[0059] Comparative Example 1

[0060] The preparation of an α-lipoic acid liposome hydrogel coating is as described in Example 1, except that: in step (4) the hydrogel precursor solution, MXene is not added; other steps and conditions are the same as in Example 1.

[0061] Comparative Example 2

[0062] The preparation of an α-lipoic acid liposome hydrogel coating is as described in Example 1, except that: in step (4), no α-lipoic acid liposome suspension is added to the hydrogel precursor solution; the other steps and conditions are the same as in Example 1.

[0063] Comparative Example 3

[0064] The preparation of an α-lipoic acid liposome hydrogel coating is as described in Example 1, except that: in step (4) the α-lipoic acid liposome suspension and MXene are not added to the hydrogel precursor solution; the other steps and conditions are the same as in Example 1.

[0065] Comparative Example 4

[0066] The preparation of an α-lipoic acid liposome hydrogel coating is as described in Example 1, except that: in step (4) the hydrogel precursor solution, methacrylic acid sulfobetaine, α-lipoic acid liposome suspension and MXene are not added; other steps and conditions are the same as in Example 1.

[0067] Experimental Example 1

[0068] Rheological measurements of α-lipoic acid liposome hydrogel coating

[0069] like Figure 1 As shown, the mechanical properties of the α-lipoic acid liposome hydrogel coating were determined at the microscale through rheological experiments. Strain amplitude scanning was performed, with strain increasing from 1% to 1000%. Within a linear strain range of 3%, the storage modulus (G') and loss modulus (G") of the Comparative Example 1 α-lipoic acid liposome hydrogel coating (Ge@PS-L) were both greater than those of the Comparative Example 3 (Ge@PS) hydrogel coating. These results indicate that the hydrogen bonds between the α-lipoic acid liposomes and the hydrogel network significantly improve the mechanical properties of the α-lipoic acid liposome hydrogel coating.

[0070] Experimental Example 2

[0071] Stability and durability tests of α-lipoic acid liposome hydrogel coatings

[0072] Comparative Example 1: An α-lipoic acid liposome hydrogel coating was applied to the surface of a PET material (i.e., the substrate was PET), which is easily bent. For example... Figure 2 and Figure 3 As shown, the material underwent 10,000 cycles of bending testing or 24 hours of ultrasonic cleaning (ultrasonic power of 400W). Figure 4 As shown, there were no significant changes in the bending position and the water contact angle on the surface of the α-lipoic acid liposome hydrogel coating before and after bending and ultrasonic cleaning.

[0073] Experimental Example 3

[0074] Hemolysis test of fresh rat erythrocytes coated with α-lipoic acid liposome hydrogel

[0075] The biocompatibility of the hydrogel samples was evaluated by assessing their hemolytic activity against fresh rat erythrocytes using the samples from Example 1 (Ge@PS-L-MX), Comparative Example 2 (Ge@PS-MX), and Comparative Example 3 (Ge@PS). Figure 5 As shown in (a), the samples were co-cultured with red blood cells for 24 h and then centrifuged. The supernatant of the positive control group (0.1% Triton X-100) was distinctly blood red, while the supernatant of the hydrogel sample group remained clear and colorless. The absorbance of the supernatant was measured, and the hemolysis rates of the hydrogel samples were calculated to be 2.18%, 3.05%, and 0.5% (corresponding to Example 1 (Ge@PS-L-MX), Comparative Example 2 (Ge@PS-MX), and Comparative Example 3 (Ge@PS), respectively), all below 5%. These results indicate that the sample has good blood compatibility.

[0076] Test Example 4

[0077] CCK-8 assay for α-lipoic acid liposome hydrogel coating

[0078] The number of viable cells during quantitative proliferation was assessed using the CCK-8 assay on hydrogel samples from Example 1 (Ge@PS-L-MX), Comparative Example 2 (Ge@PS-MX), and Comparative Example 3 (Ge@PS). Figure 5 As shown in (b) and 5(c), compared to Comparative Examples 2 and 3, Example 1 group significantly reduced the viability and proliferation capacity of DF cells. Comparative Example 2 group exhibited the strongest proliferation capacity. The number of surviving DF cells in Example 1 group was only two-thirds that of Comparative Examples 2 and 3. Furthermore, as... Figure 5 As shown in (d) and 5(e), compared to Comparative Examples 2 and 3, the ROS level of DF cells in Example 1 was significantly reduced, reaching half that of Comparative Examples 2 and 3. The ROS levels of DF cells in Comparative Examples 2 and 3 were both around 0.7, with very little difference. The ROS level of DF cells in Comparative Example 2 was slightly higher than that in Comparative Example 3. This indicates that Example 1 can significantly reduce oxidative stress.

[0079] Experimental Example 5

[0080] Immunofluorescence staining was used to quantitatively determine the expression levels of COL1A1 and MKi67 in α-lipoic acid liposome hydrogel coatings.

[0081] like Figure 5As shown in (f), the expression levels of COL1A1 and MKi67 were quantitatively determined by immunofluorescence staining. COL1A1, a key extracellular matrix (ECM) component, was significantly elevated in proliferative scar fibroblasts compared to healthy skin fibroblasts, highlighting its potential as a biomarker for skin fibrosis. Furthermore, MKi67 served as a proliferation marker specifically upregulated in activated fibroblasts during skin scar formation. Representative images show that the expression of COL1A1 and MKi67 in Example 1 (Ge@PS-L-MX) was significantly reduced compared to Comparative Example 2 (Ge@PS-MX) and Comparative Example 3 (Ge@PS) groups. The fluorescence expression of COL1A1 in Comparative Example 2 was stronger than that in Comparative Example 3, while the fluorescence expression of MKi67 was weaker in Comparative Example 2 than in Comparative Example 3. ROS levels were significantly increased in Comparative Example 2 and Comparative Example 3 groups, with the ROS level in Comparative Example 2 being slightly weaker than that in Comparative Example 3, and the fluorescence intensity difference was small. This suggests that oxidative stress may exacerbate the fibrotic process. These findings suggest that LA can inhibit cell proliferation and reduce ROS accumulation, implying its potential efficacy in inhibiting fibrotic scar formation.

[0082] Experimental Example 6

[0083] Experiment on the effects of α-lipoic acid liposome hydrogel coating on wound healing and fibrotic remodeling

[0084] A full-thickness resection wound model was established in mice (n=8 / group) to systematically evaluate the effects of comparative example 2 (Ge@PS-MX), comparative example 3 (Ge@PS), and example 1 (Ge@PS-L-MX) hydrogels on wound healing and fibrotic remodeling. The hydrogels were applied to the wound site during the experiment.

[0085] Figure 6 (a) is a schematic diagram of a full-thickness resection model of a mouse wound. Figure 6(b) shows immunofluorescence staining images of MYHI1+ on days 5 and 10 after injury (the first row of images was taken on day 5 after injury, and the second row on day 10 after injury). Figure 6(c) shows immunofluorescence staining images of MKi67+ (proliferating cells) on days 5 and 10 after injury (the first row of images was taken on day 5 after injury, and the second row on day 10 after injury). Figure 6(d) shows immunofluorescence staining images of CNN1+ (smooth muscle cells) on days 5 and 10 after injury (the first row of images was taken on day 5 after injury, and the second row on day 10 after injury). Figure 6As shown in (b), 6(c), and 6(d), 5 days post-injury, the fluorescence intensity of αSMA and MKi67+ cells in Example 1 group was significantly higher than that in Comparative Example 3 group. These results indicate that MXene, under NIR irradiation (in the test experiment, continuous NIR irradiation was performed immediately after the hydrogel was applied to the wound, with an NIR irradiation power of 0.839 W, a wavelength of 350 nm, and an irradiation time of 600 s), activates myofibroblasts and accelerates their proliferation through a local photothermal effect. In Comparative Example 2 group, the density of vascular smooth muscle cells (MYH11+ or CNN1+ cells) and endothelial cells (CD31+ cells) increased synchronously, indicating that MXene-induced mild thermal stimulation enhanced angiogenesis. Furthermore, as Figure 6 As shown in (f), compared to Group 1, the mRNA levels of fibrosis-related genes (Col1a1, Col3a1, Co3a1, Postn, Ctgf) were significantly increased in Group 2, further confirming its pro-fibrotic characteristics. Group 1 showed lower expression levels of inflammatory factors (Mcp1, Tnfa, IL6) at the same time point (day 5), indicating that LA alleviates excessive inflammatory responses through its antioxidant and anti-inflammatory effects. Compared to Groups 2 and 3, Group 1 exhibited significant regulatory features on day 5. These features included significantly reduced fluorescence intensity in MYH11+ and MKi67+ cells, and decreased expression levels of fibrosis-related genes. Furthermore, the CD31 cell density in this group remained consistently high, accompanied by an increase in CNN1+ cells. This observation suggests that LA promotes angiogenesis maturation by facilitating endothelial-smooth muscle cell interactions rather than simply stimulating angiogenesis. Figure 6 (e) Quantitative analysis showed that the Example 1 group had the lowest number of CD45 and MKi67+ cells on days 5 and 10, respectively. Compared with Comparative Examples 2 and 3, Comparative Example 2 group had the highest number of MKi67+ cells on days 5 and 10, and the highest number of CD45 cells on day 5. Comparative Example 3 group had the highest number of CD45 cells on day 10. This demonstrates that the addition of α-lipoic acid liposomes in Example 1 can gradually release and significantly inhibit the growth of skin scars in mice, promote angiogenesis, and thus significantly promote wound healing.

[0086] Experimental Example 7

[0087] Antibacterial properties test of α-lipoic acid liposome hydrogel coating

[0088] The anti-adhesion properties of the hydrogel coatings prepared by the methods in Examples 1 and 4 against Staphylococcus aureus were investigated by forming a hydrogel coating on the surface of surgical sutures (preparation method was the same as in Example 1 and Comparative Example 4, except that the substrate was replaced with surgical sutures). Figure 7As shown on the left, the four groups of culture medium comparison images show the adhesion of Staphylococcus aureus to the surface of blank surgical sutures (blank sample), surgical sutures coated with hydrogel coating prepared by method 4 (GelMA) without NIR irradiation, surgical sutures coated with α-lipoic acid liposome hydrogel coating prepared by method 1 (Ge@PS-L-MX1) without NIR irradiation, and surgical sutures coated with α-lipoic acid liposome hydrogel coating prepared by method 1 (NIR-irradiated Ge@PS-L-MX1) under NIR irradiation conditions (NIR irradiation at the beginning of culture, power 0.839W, wavelength 350nm, irradiation time 600s). Figure 7 As shown on the right, the adhesion rates of Staphylococcus aureus on blank sutures, sutures coated in Comparative Example 4, sutures coated in Example 1 without NIR irradiation, and sutures coated in Example 1 under NIR irradiation were 100%, 25%, 7.5%, and 2.5%, respectively. The antibacterial experiment demonstrated that the α-lipoic acid liposome hydrogel coating of Example 1 can prevent bacterial adhesion. Furthermore, under NIR irradiation, the bacterial adhesion rate of the α-lipoic acid liposome hydrogel coating of Example 1 was further reduced to 2.5%, because MXene can absorb light energy and convert it into heat energy under NIR irradiation, leading to an increase in the surface temperature of the coating. This temperature increase not only controls drug release but also effectively kills bacteria attached to the surface.

[0089] Experimental Example 8

[0090] Lubrication performance test of α-lipoic acid liposome hydrogel coating

[0091] like Figure 8 As shown in (a), Figure 8 (a) is a schematic diagram of the method for measuring the friction coefficient of the hydrogel coatings of Comparative Example 1, Comparative Example 3, and Comparative Example 4 using a rheometer. Figure 8 (b) and Figure 8(c) The friction coefficients of the hydrogel coatings of Comparative Example 4 (GelMA), Comparative Example 3 (Ge@PS), and Comparative Example 1 (Ge@PS-L) under the conditions of a friction speed of 30 rad / min and a normal load of 1 N are 0.01, 0.007, and 0.002, respectively. The introduction of sulfobetaine methacrylate and α-lipoic acid liposomes reduced the friction coefficient of the α-lipoic acid liposome hydrogel coating of Comparative Example 1 by 5 times compared to that of the hydrogel coating of Comparative Example 4. This is because the sulfobetaine groups in PSBMA form hydrogen bonds with water molecules, forming a dense hydration layer; in addition, the phospholipid bilayer of the α-lipoic acid liposome has an amphiphilic structure, which is conducive to the formation of a self-lubricating layer, while the lubricating performance would decrease if the liposomes were replaced with lipoic acid. The presence of the dense hydration layer and the self-lubricating layer reduced the friction coefficient of the α-lipoic acid liposome hydrogel coating of Comparative Example 1 and improved its wear resistance. Figure 8 As shown in (d), Figure 8 (d) The friction coefficients of the hydrogel coatings of Example 1 (Ge@PS-L-MX1) and Comparative Example 1 (Ge@PS-L) were measured by a rheometer under a constant normal force of 1 N and a constant rotation speed of 30 rad / min. The friction performance of the hydrogel coatings with and without MXene was compared, and the difference in friction coefficients was not significant.

[0092] Experimental Example 9

[0093] Photothermal performance test of α-lipoic acid liposome hydrogel coating

[0094] like Figure 9 As shown in (a) and 9(b), Figure 9 (a) Recordings of Comparative Example 1 (Ge@PS-L-MX0) and Example 3 (Ge@PS-L-MX0) under NIR irradiation (0.839 W, 350 nm) 0.1 Example 2 (Ge@PS-L-MX) 0.5 The temperature changes of the α-lipoic acid liposome hydrogel coatings of Comparative Example 1, Example 3, Example 2, and Example 1 over time were compared. After 600 s of NIR irradiation, the temperatures of the α-lipoic acid liposome hydrogel coatings of Comparative Example 1, Example 3, Example 2, and Example 1 were 30.5℃, 45℃, 58℃, and 68℃, respectively. Figure 9 (b) Infrared thermal images of Comparative Example 1 and Example 1 at 1 min, 2 min, 4 min, and 6 min under NIR irradiation (0.839 W, 350 nm). It can be seen that the photothermal conversion efficiency of the α-lipoic acid liposome hydrogel coating significantly increases with increasing MXene content; however, if the MXene content exceeds 1 mg / ml, overheating will occur under NIR irradiation.

[0095] The embodiments described above are merely illustrative of implementation methods of the present invention and should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the protection scope of the present invention.

Claims

1. A method for preparing an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing, comprising the following steps: (1) The substrate was subjected to plasma treatment, then immersed in propyl 3-(trimethyloxysilyl)methacrylate (KH570) solution and dried to obtain a KH570 treated substrate; (2) The KH570-treated substrate was soaked in an ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) ethyl acetate solution and dried to obtain an initiator-treated substrate; (3) The substrate treated with the initiator was immersed in the hydrogel precursor solution, and the reaction was carried out to obtain an α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing. The hydrogel precursor solution is a dispersion of methacrylated gelatin (GeLMA), methacrylate sulfobetaine, α-lipoic acid liposomes, MXene, and water.

2. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, In step (1), the substrate material is selected from polyethylene terephthalate or high-density polyethylene.

3. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, Step (1) includes one or more of the following conditions: i. Prior to plasma treatment, the following steps are also included: ultrasonically cleaning the substrate to remove impurities on the surface and drying it in clean air; ii. The conditions for plasma treatment are: pressure 5-20 Pa, power 5-20 W, and plasma treatment time 3-8 minutes.

4. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, In step (1), the solvent used for the 3-(trimethyloxysilyl)methacrylate (KH570) solution is a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1-2:1; the content of 3-(trimethyloxysilyl)methacrylate in the 3-(trimethyloxysilyl)methacrylate (KH570) solution is 1-5wt%; in step (1), the soaking temperature is room temperature and the soaking time is 1-5h.

5. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, In step (2), the concentration of the ethyl(2,4,6-trimethylbenzoyl)phenyl phosphate (TPO-L) ethyl acetate solution is 1-5 wt%; in step (2), the soaking temperature is room temperature and the soaking time is 20-40 s.

6. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, In step (3), the α-lipoic acid liposomes are composed of α-lipoic acid and a lipid membrane coating the surface of α-lipoic acid. The lipid membrane is composed of soybean lecithin and cholesterol. The α-lipoic acid liposomes are added to the system in the form of an α-lipoic acid liposome suspension, wherein the solvent of the α-lipoic acid liposome suspension is a phosphate buffer solution with pH 7.4, and the concentration of the α-lipoic acid liposomes is 7-7.5 g / L.

7. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 6, characterized in that, In step (3), the α-lipoic acid liposome suspension is prepared by a membrane hydration method, which includes the following steps: dissolving soybean lecithin, cholesterol and α-lipoic acid in dichloromethane, removing the dichloromethane by rotary evaporation to form a uniform thin lipid membrane; adding phosphate buffer (PBS) for hydration treatment; and then obtaining the α-lipoic acid liposome suspension by sonication and filtration; the mass ratio of soybean lecithin to cholesterol is 1-3:1, the total mass of soybean lecithin and cholesterol to the mass ratio of α-lipoic acid is 3-4:1; the mass ratio of α-lipoic acid to the volume ratio of dichloromethane is 2-3 g / L; the rotary evaporation temperature is 40℃; the pH of the phosphate buffer is 7.4, and the mass ratio of α-lipoic acid to the volume ratio of phosphate buffer is 1.5-2 g / L; the hydration treatment method is as follows: ultrasonic treatment at 35-45℃ for 3-10 min, and then ultrasonic treatment at -5-5℃ for 15-25 min; the filter membrane specification is 0.45 μm.

8. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, In step (3), the mass ratio of methacrylated gelatin (GeLMA), methacrylate sulfobetaine, α-lipoic acid liposomes, and MXene is 8-12:4-8:2-3:0.01-0.

2.

9. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 8, characterized in that, In step (3), the mass ratio of methacrylated gelatin (GeLMA), methacrylate sulfobetaine, α-lipoic acid liposomes, and MXene is 10:5:2-3:0.01-0.

1.

10. The method for preparing the α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing according to claim 1, characterized in that, Step (3) includes one or more of the following conditions: i. The mass ratio of MXene to water is 1-5 mg / mL; ii. The reaction conditions are as follows: react under ultraviolet light for 20-50 seconds, then remove the ultraviolet light and let it stand at room temperature for 5-50 seconds; the ultraviolet light irradiation power is 800-1200W.

11. An α-lipoic acid liposome photothermal responsive hydrogel coating that can inhibit scarring and promote wound healing, prepared by the method described in any one of claims 1-10.

12. The use of the α-lipoic acid liposome photothermal responsive hydrogel coating as described in claim 11, which can inhibit scarring and promote wound healing, in the preparation of a drug that can inhibit scarring and promote wound healing.

13. The application of the α-lipoic acid liposome photothermal responsive hydrogel coating as described in claim 11, which can inhibit scarring and promote wound healing, in the preparation of dressings that can inhibit scarring and promote wound healing.

Citation Information

Patent Citations

  • Lipoic acid hydrogel as well as preparation method and application thereof

    CN115232329A

  • Preparation method of bio-based adhesive hydrogel patch for promoting wound healing as well as product and application of bio-based adhesive hydrogel patch

    CN115337446A

  • Antibacterial dressing for promoting wound healing, preparation method and application

    CN118949107A

  • Drug electric controlled release hydrogel patch for wound healing

    CN119184963A

  • Patterned hydrogel coating based on synergism of surface laser ablation and surface-initiated grafting, preparation of patterned hydrogel coating and application of patterned hydrogel coating in drag reduction

    CN120460252A