Negative active material, method for preparing the same, negative electrode sheet, secondary battery, and device

By using porous graphite particles and metal single-atom modified negative electrode active materials in lithium-ion batteries, the problem of insufficient high-rate charging capability of lithium-ion batteries has been solved, improving the charging performance and safety of the batteries.

CN120613367BActive Publication Date: 2026-11-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410256644.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2026-11-24
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

The insufficient high-rate charging capability of lithium-ion batteries has limited the development of fields such as electric vehicles.

Method used

By employing porous graphite particles and metal single-atom-modified anode active materials, the transport dynamics of Li⁺ are enhanced by increasing the Li⁺ insertion channels and lowering the insertion energy barrier.

Benefits of technology

It improves the dynamic performance of the negative electrode, enhances the high-rate charging capability of the secondary battery, reduces negative electrode polarization, and reduces the risk of lithium plating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120613367B_ABST
    Figure CN120613367B_ABST
Patent Text Reader

Abstract

This application provides a negative electrode active material, its preparation method, a negative electrode sheet, a secondary battery, and an apparatus. The negative electrode active material comprises porous graphite particles and metal single atoms disposed on the porous graphite particles. When applied to a secondary battery, this negative electrode active material exhibits good high-rate charging capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of secondary battery technology, and in particular to a negative electrode active material and its preparation method, a negative electrode sheet, a secondary battery, and a device. Background Technology

[0002] The statements herein are provided only as background information in connection with this application and do not necessarily constitute prior art.

[0003] In recent years, the application of secondary batteries such as lithium-ion batteries has become increasingly widespread. They are widely used in energy storage systems for hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and many other fields. However, the high-rate charging capability of secondary batteries such as lithium-ion batteries has severely restricted the development of fields such as electric vehicles, thus placing higher demands on their high-rate charging capabilities. Summary of the Invention

[0004] This application is made in view of the above-mentioned issues, and one of its objectives includes: providing a negative electrode active material and its preparation method, a negative electrode sheet, a secondary battery and a device, wherein the negative electrode active material, when applied to a secondary battery, has good high-rate charging capability.

[0005] The first aspect of this application provides a negative electrode active material, comprising porous graphite particles and metal single atoms disposed on the porous graphite particles.

[0006] Therefore, taking lithium-ion batteries as an example, and not wanting to be limited to any theory, the negative electrode active material described in this application includes porous graphite particles and metal single atoms disposed on the porous graphite particles. It is a porous graphite material modified with metal single atoms. Because it has a porous structure, it can not only increase the Li-ion battery's performance but also enhance its overall performance. + The embedded channel can also shorten the Li + The embedding path, thereby improving Li + Transport dynamics on the graphite surface. Furthermore, metal single atoms deposited on porous graphite particles can improve the local charge distribution on the surface of porous graphite particles and reduce Li... + The embedding energy barrier on the graphite surface accelerates Li + The embedding rate into the porous graphite particle bulk phase. Thus, the aforementioned anode active material synergistically enhances the Li-... + The transport dynamics on the surface of the negative electrode active material reduce negative electrode polarization, improve the dynamic performance of the negative electrode, and thus improve the high-rate charging capability of the secondary battery.

[0007] In some embodiments of this application, the crystalline material surface of the porous graphite particles has a base surface and an end face connected to the base surface, the end face having a porous structure, and the end face having the metal single atom.

[0008] In some embodiments of this application, the base surface is also provided with the metal single atom.

[0009] In some embodiments of this application, the negative electrode active material satisfies at least one of the following conditions:

[0010] (1) The specific surface area of ​​the negative electrode active material is 1.2 m². 2 ·g -1 ~5.0 m 2 ·g -1 ;

[0011] (2) The Dv50 particle size of the porous graphite particles is 5μm~50μm;

[0012] (3) The porous graphite particles include at least one of artificial graphite and natural graphite.

[0013] In some embodiments of this application, the negative electrode active material satisfies at least one of the following conditions:

[0014] (1) In the negative electrode active material, the mass content of the metal single atom is 0.01wt%~0.5wt%;

[0015] (2) The degree of graphitization of the negative electrode active material is 90%~97%.

[0016] In some embodiments of this application, the metal single atom includes at least one of transition metals and alkaline earth metals.

[0017] In some embodiments of this application, the types of the metal single atoms include one or more of Fe, Co, Ni, Cu, Zn, Mn, Mg and Sc.

[0018] In some embodiments of this application, the negative electrode active material further includes at least one of nitrogen element and amorphous carbon doped on the surface of the porous graphite particles.

[0019] A second aspect of this application provides a method for preparing a negative electrode active material, comprising the following steps:

[0020] Porous graphite particles are obtained by mixing graphite particles with an alkaline ligand solution and then drying them.

[0021] The porous graphite particles are mixed with a metal salt solution, dried, and then heat-treated in a reducing atmosphere to obtain the negative electrode active material. The metal ions in the metal salt can form complexes with the ligands.

[0022] A second aspect of this application provides a method for preparing a negative electrode active material, comprising the following steps:

[0023] The graphite particles are mixed with an alkaline ligand solution and a metal salt solution, dried, and then heat-treated in a reducing atmosphere to obtain the negative electrode active material; wherein the metal ions in the metal salt can form a complex with the ligand.

[0024] In some embodiments of this application, the alkaline ligand solution comprises a first organic amine compound, wherein the functionality of the organic amine group in the first organic amine compound is >1, and the first organic amine compound is an alkaline compound.

[0025] In some embodiments of this application, the alkaline ligand solution further includes a second organic amine compound, wherein the functionality of the organic amine group in the second organic amine compound is 1.

[0026] In some embodiments of this application, the preparation method satisfies at least one of the following features:

[0027] (1) The pH value of the alkaline ligand solution is 8.0~14.0;

[0028] (2) The functionality of the organic amine group in the first organic amine compound is 2 to 5;

[0029] (3) The molar mass of the first organic amine compound is less than or equal to 1000 g / mol;

[0030] (4) The molar mass of the second organic amine compound is less than or equal to 1000 g / mol.

[0031] In some embodiments of this application, the preparation method satisfies at least one of the following features:

[0032] (1) The organic amine groups in the first organic amine compound and the second organic amine compound each independently include primary amine groups;

[0033] (2) The molar mass of the first organic amine compound is less than or equal to 500 g / mol;

[0034] (3) The molar mass of the second organic amine compound is less than or equal to 500 g / mol;

[0035] (4) The number of carbon atoms in the first organic amine compound and the second organic amine compound is 1 to 10.

[0036] In some embodiments of this application, the preparation method satisfies at least one of the following features:

[0037] (1) The first organic amine compound includes ethylenediamine;

[0038] (2) The second organic amine compound includes at least one of methylamine and ethylamine.

[0039] In some embodiments of this application, the metal salt solution satisfies at least one of the following characteristics:

[0040] (1) The metal elements in the metal salt solution include at least one of transition metals and alkaline earth metals;

[0041] (2) The metal salt in the metal salt solution includes one or more of hydrochloride, nitrate and sulfate;

[0042] (3) The concentration of the metal salt solution is 0.001 mol·L. -1 ~1mol·L -1 ;

[0043] (4) The mass ratio of the metal salt in the metal salt solution to the porous graphite particles is (0.5~5):100.

[0044] In some embodiments of this application, the graphite particles and the ligand solution are mixed under heating conditions, wherein the heating temperature is 50°C to 120°C and the heating time is 2 h to 72 h.

[0045] In some embodiments of this application, the preparation method satisfies at least one of the following features:

[0046] (1) The time for mixing the porous graphite particles with the metal salt solution is 0.5h to 2h;

[0047] (2) The reducing atmosphere includes at least one of nitrogen and argon, as well as hydrogen;

[0048] (3) The temperature of the heat treatment is 400℃~1000℃ and the time is 2h~24h;

[0049] (4) The heating rate to the heat treatment temperature is 1℃ / min to 10℃ / min.

[0050] In some embodiments of this application, the preparation method satisfies at least one of the following features:

[0051] (1) The volume percentage of hydrogen in the reducing atmosphere is 3.0%~10.0%;

[0052] (2) The heat treatment temperature is 700℃~800℃ and the time is 2h~5h;

[0053] (3) The heating rate to the heat treatment temperature is 2.0℃ / min to 5.0℃ / min.

[0054] A third aspect of this application provides a negative electrode sheet, comprising at least one of the negative electrode active material provided in the first aspect of this application and the negative electrode active material prepared by the preparation method provided in the second aspect of this application.

[0055] A fourth aspect of this application provides a secondary battery, including the negative electrode provided in the third aspect of this application.

[0056] A fifth aspect of this application provides an electrical device comprising at least one of the following: the negative electrode active material provided in the first aspect of this application, the negative electrode active material prepared by the preparation method provided in the second aspect of this application, the negative electrode sheet provided in the third aspect of this application, and the secondary battery provided in the fourth aspect of this application.

[0057] Details of one or more embodiments of this application are set forth in the following drawings and description. Other features, objects, and advantages of this application will become apparent from the specification, drawings, and claims. Attached Figure Description

[0058] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0059] Figure 1 This is a schematic diagram of a secondary battery according to one embodiment of this application.

[0060] Figure 2 yes Figure 1 An exploded view of a secondary battery according to one embodiment of this application is shown.

[0061] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.

[0062] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0063] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.

[0064] Figure 6 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.

[0065] Figure 7 This is a low-magnification SEM image of the negative electrode active material prepared in Example 1 of this application.

[0066] Figure 8 This is a high-magnification SEM image of the negative electrode active material prepared in Example 1 of this application.

[0067] Figure 9 This is a low-magnification SEM image of the negative electrode active material used in Comparative Example 1 of this application.

[0068] Figure 10 These are dark-field SEM and EDS mapping images of the negative electrode active material prepared in Example 1 of this application.

[0069] Figure 11 This is the Raman diagram of the negative electrode active material prepared in Example 1 of this application.

[0070] Figure 12 This is the XRD pattern of the negative electrode active material prepared in Example 1 of this application.

[0071] Figure 13 These are graphs showing the rate performance test results of the button cells prepared in Examples 1-3 and Comparative Examples 1-2 of this application.

[0072] Explanation of reference numerals in the attached figures:

[0073] 1. Battery pack; 2. Upper casing; 3. Lower casing; 4. Battery module; 5. Battery cell; 51. Housing; 52. Electrode assembly; 53. Cover plate; 6. Electrical device. Detailed Implementation

[0074] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0075] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this document; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, stating that a parameter is an integer ≥2 is equivalent to disclosing that the parameter is, for example, an integer 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, stating that a parameter is an integer selected from "2-10" is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0076] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0077] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0078] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0079] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0080] In this application, open-ended technical features or solutions described using terms such as "containing," "including," or "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, if A includes a1, a2, and a3, it may also include other members or exclude additional members unless otherwise specified. This can be considered as providing both the feature or solution that "A consists of a1, a2, and a3" and the feature or solution that "A includes not only a1, a2, and a3, but also other members."

[0081] In this application, unless otherwise specified, A (e.g., B) means that B is a non-limiting example of A, and it is understood that A is not limited to B.

[0082] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0083] One embodiment of this application provides a negative electrode active material, comprising porous graphite particles and metal single atoms disposed on the porous graphite particles.

[0084] Taking lithium-ion batteries as an example, graphite is a commonly used negative electrode active material. When lithium-ion batteries are charged at high rates, the lithium intercalation rate of graphite is lower than that of Li-ion batteries. + The transport rate in the electrolyte leads to the formation of Li on the negative electrode surface. + Accumulation of lithium leads to negative electrode polarization, posing a risk of lithium plating in lithium-ion batteries. Therefore, shortening the Li-ion plating time... + The embedding path, adding Li+ Embedded channels and reduced Li + The embedded energy barrier helps to improve the high-rate charging capability of graphite materials.

[0085] Taking lithium-ion batteries as an example, and not wanting to be limited to any theory, the negative electrode active material described in this application, including porous graphite particles and metal single atoms disposed on the porous graphite particles, is a porous graphite material modified with metal single atoms. Because of its porous structure, it can not only increase the Li-ion battery's... + The embedded channel can also shorten the Li + The embedding path, thereby improving Li + Transport dynamics on the graphite surface. Furthermore, metal single atoms deposited on porous graphite particles can improve the local charge distribution on the surface of porous graphite particles and reduce Li... + The embedding energy barrier on the graphite surface accelerates Li + The embedding rate into the porous graphite particle bulk phase. Thus, the aforementioned anode active material synergistically enhances the Li-... + The transport dynamics on the surface of the negative electrode active material reduce negative electrode polarization, improve the dynamic performance of the negative electrode, and thus improve the high-rate charging capability of the secondary battery.

[0086] It is understood that the secondary battery of this application includes, but is not limited to, lithium-ion batteries, and may also include, for example, sodium-ion batteries. Correspondingly, the aforementioned active ions, besides Li... + It can also be Na + .

[0087] It should be noted that a metallic monatomic atom refers to a metal existing in monatomic form. A monatomic atom is different from a metallic element; in a metallic element, metal atoms are connected to each other by metallic bonds, while adjacent sites of a monatomic atom are considered not to be connected by metallic bonds.

[0088] One embodiment of this application provides a method for preparing the above-mentioned negative electrode active material, which may include the following steps S10-S20:

[0089] S10. After mixing graphite particles with an alkaline ligand solution, the mixture is dried to obtain porous graphite particles.

[0090] S20. Porous graphite particles are mixed with a metal salt solution and dried, then heat-treated in a reducing atmosphere to obtain the negative electrode active material. The metal ions in the metal salt solution can form complexes with the ligands.

[0091] Furthermore, the alkaline ligand solution is an aqueous solution. The alkalinity of the ligand solution allows for the utilization of the abundant OH- ions within it. -The process involves reacting with defect sites on the graphite surface to etch the graphite particles, thereby forming porous graphite particles. The ligands within these particles adhere to the surface of the graphite particles and, in subsequent steps, coordinate with metal ions to form complexes, thus achieving the coordination and anchoring of metal atoms on the porous graphite particles. Furthermore, the ligands possess at least multiple coordinating groups.

[0092] Furthermore, the alkaline ligand solution includes a first organic amine compound, wherein the functionality of the organic amine group in the first organic amine compound is >1, and the first organic amine compound is a basic compound. It can be understood that the organic amine group is the coordinating group of the first organic amine compound.

[0093] It is understandable that the first organic amine compound hydrolyzes in aqueous solution to produce abundant OH-. - Therefore, it exhibits alkalinity; in other words, aqueous solutions of organic amines are alkaline. This innovative use of the abundant OH- ions in the aqueous solution of the first organic amine compound... - The reaction with the defect sites on the graphite surface achieves the etching of graphite particles, thereby forming porous graphite particles. At the same time, the first organic amine compound molecule has a strong interaction with the oxygen-containing functional groups on the surface of the graphite particles through the organic amine groups. Since the functionality of the organic amine groups in the first organic amine compound is >1, the organic amine groups can be "grafted" onto the graphite particles, so that the surface of the porous graphite particles is connected with free organic amine groups.

[0094] The abundant organic amine groups on these porous graphite particles have strong coordination ability. By mixing the porous graphite particles with a metal salt solution, the organic amine groups can coordinate with the empty orbitals of the metal cations to form metal complexes, thus achieving coordination anchoring of the metal on the porous graphite particles. Then, heat treatment in a reducing atmosphere reduces the metal salt at the anchoring point to form metal single atoms.

[0095] As described above, the first organic amine compound in this application has at least two functions: first, it plays a role in etching graphite particles to form porous graphite particles in step S10; second, it plays a role in coordination anchoring and guiding the formation of metal single atoms in step S20.

[0096] Another embodiment of this application provides a method for preparing the above-mentioned negative electrode active material, which may include the following step S30:

[0097] Graphite particles are mixed with an alkaline ligand solution and a metal salt solution, dried, and then heat-treated in a reducing atmosphere to obtain the negative electrode active material. Furthermore, the ligand is in excess relative to the metal salt solution.

[0098] This preparation method simultaneously mixes an alkaline ligand solution and a metal salt solution with graphite particles. The coordination between cobalt ions and the ligands, as well as the etching of the graphite particles by the alkaline ligand solution, occur concurrently, allowing the metal ions to anchor onto the graphite surface. This results in graphite with single-atom sites on its surface, thus yielding the aforementioned negative electrode active material. However, compared to the aforementioned stepwise preparation method, its etching sites are limited, resulting in a lower content of single atoms. Not wishing to be limited by any theory, this application provides a method for preparing the aforementioned negative electrode active material that employs an etching-coordination anchoring strategy using ligands such as organic amines. The resulting negative electrode active material is modified graphite, specifically a porous graphite material modified with single metal atoms. This negative electrode active material can be used in secondary batteries, thereby improving the performance of Li-ion batteries. + By improving the transport dynamics of active ions on the surface of the negative electrode active material, negative electrode polarization can be reduced, the dynamic performance of the negative electrode can be improved, and thus the high-rate charging capability of the secondary battery can be enhanced.

[0099] In some embodiments of this application, the surface of the porous graphite particles has a basal plane and an end face connected to the basal plane. The end face has a porous structure and is provided with the aforementioned metal single atoms. Because the surface of the graphite particles has a basal plane and an end face connected to the basal plane, and the basal plane of the graphite particles is a complete six-membered ring structure, while the end face contains more abundant oxygen-containing functional groups, during the preparation process, OH groups in the solution... - The ligand solution can preferentially react with the defect sites on the end face of graphite particles. Therefore, after treatment with the ligand solution in step S10, porous graphite particles with porous end faces can be obtained. Furthermore, the ligand molecules, such as the first organic amine compound, have a strong interaction with the oxygen-containing functional groups on the end face, enabling preferential "grafting" of organic amine groups and other ligand groups on the end face. Thus, the aforementioned metal single atoms will preferentially form on the end face of the porous graphite particles.

[0100] It is understood that in some embodiments, after treatment with the ligand solution described above, a porous structure will also be formed on the basal surface. Correspondingly, the aforementioned metal single atoms will also be formed on the basal surface of the porous graphite particles.

[0101] In some embodiments of this application, the specific surface area of ​​the negative electrode active material is 1.2 m². 2 ·g -1 ~5.0 m 2 ·g -1 For example, it could be 1.2 m. 2 ·g -1 1.5 m 2 ·g -1 2 m 2 ·g -1 2.5 m 2 ·g -1 3 m 2 ·g-1 3.5m 2 ·g -1 4 m 2 ·g -1 4.5m 2 ·g -1 5 m 2 ·g -1 ; it can be further increased to 1.2 m 2 ·g -1 ~2.5 m 2 ·g -1 .

[0102] The specific test steps for specific surface area are as follows: 1. Pretreatment: Take an appropriate amount of sample in a special sample tube, heat and degas under vacuum for 2 hours, and weigh the total weight after cooling to room temperature. Subtract the mass of the sample tube to obtain the sample mass. 2. Test: Place the sample tube into the workstation and, under constant low temperature, determine the amount of gas adsorbed on the solid surface at the adsorption pressure. Based on the BET multilayer adsorption theory and its formula, calculate the monolayer adsorption amount of the sample, and thus calculate the specific surface area per unit mass of the solid sample. 3. Adsorbed gas: carbon dioxide; adsorption pressure points: 0.005, 0.010, 0.015, 0.020, 0.025, 0.030, 0.035, 0.040, 0.045, 0.050; test atmosphere: ice-water mixture.

[0103] In some embodiments of this application, the Dv50 particle size of the porous graphite particles is 5 μm to 50 μm. As an example, the Dv50 particle size of the porous graphite particles can be 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 50 μm.

[0104] Dv50 has a well-known meaning in the art and can be tested using methods known in the art. For example, it can be measured using a laser particle size analyzer (such as the Malvern Master Size 3000). Here, Dv50 represents the particle size at which the percentage of particle volume distribution accumulates to 50% based on the particle size distribution, starting from the smallest particle size.

[0105] Particle size distribution can be obtained by the following method: Take a clean beaker, add an appropriate amount of the sample to be tested, and sonicate thoroughly to ensure complete dispersion. The testing instrument is a Malvern 2000 (USA). After the sample is poured into the injection tower, it circulates with the solution to the test optical path system. Under the illumination of the laser beam, the particle size distribution characteristics can be obtained by receiving and measuring the energy distribution of the scattered light (opause: 8-12%). Particle size distribution diagrams are plotted based on the test data.

[0106] In some embodiments of this application, the porous graphite particles include at least one of artificial graphite and natural graphite. Correspondingly, the graphite particles in the preparation method include at least one of artificial graphite and natural graphite. The morphology of the porous graphite particles includes, but is not limited to, at least one of flake graphite, granular graphite, and spherical graphite. For example, it can be at least one of natural flake graphite, natural granular graphite, and artificial spherical graphite.

[0107] In some embodiments of this application, the mass content of metal single atoms in the negative electrode active material is 0.01wt%~0.5wt%, further 0.1wt%~0.5wt%, 0.2wt%~0.5wt%. Controlling the mass content of metal single atoms within this range ensures that the structural stability of the graphite particle bulk phase of the prepared negative electrode active material is essentially unaffected, and its graphitization degree is controlled within a high range. A higher degree of graphitization also helps to improve rate performance and reduce the occurrence of surface side reactions, thus playing a significant role in improving the kinetic performance of the negative electrode.

[0108] As an example, in the negative electrode active material, the mass content of metal single atoms can be 0.01wt%, 0.015wt%, 0.02wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, or 0.5wt%; in some embodiments, it can also be a range formed by any two of the above point values ​​as endpoints, and the same applies below.

[0109] In some embodiments of this application, the graphitization degree of the negative electrode active material is 90%~97%.

[0110] In some embodiments of this application, the type of metal single atom includes at least one of transition metals and alkaline earth metals. Further, the type of metal single atom includes one or more of Fe, Co, Ni, Cu, Zn, Mn, Mg, and Sc. It is understood that by controlling the type of metal salt, modification of the single atom site of one metal can be achieved, and anchoring of single atoms of multiple metals onto the surface of graphite particles, such as the end face of the graphite particles, can also be achieved. Optionally, the type of metal single atom includes one or more of Fe, Co, Ni, Cu, Zn, Mn, Mg, and Sc.

[0111] In some embodiments of this application, the negative electrode active material further includes at least one of nitrogen (N) and amorphous carbon doped onto the surface of porous graphite particles. The heat treatment in a reducing atmosphere is equivalent to thermal reduction calcination, which reduces the metal salt at the anchoring points to form metal single atoms while simultaneously thermally reducing and carbonizing the organic amine groups, thereby forming nitrogen and amorphous carbon doped onto the surface of the porous graphite particles.

[0112] In some embodiments of this application, the organic groups in the first organic amine compound in the above preparation method include primary amine groups. Primary amine groups have strong coordination ability and low steric hindrance, allowing for better coordination with metal ions.

[0113] It is understood that the functionality of the organic amine groups in the aforementioned first organic amine compound is >1, meaning there can be multiple organic amine groups. Functionality refers to the number of organic amine groups contained in one molecule of an organic amine compound. Having multiple organic amine groups in the aforementioned organic amine compound can improve its coordination and anchoring ability. In some embodiments of this application, the functionality of the organic amine groups in the aforementioned organic amine compound is ≥2, which constitutes an organic polyamine compound, for example, with a functionality of 2 to 5; for example, it can be 2, 3, 4, or 5.

[0114] In some embodiments, the alkaline ligand solution may further include a second organic amine compound, wherein the functionality of the organic amine group in the second organic amine compound is 1. Although the second organic amine compound cannot act as a coordination anchor for metal atoms on porous graphite particles, it can act as a regulator of the pH value of the ligand solution.

[0115] Understandably, the second organic amine compound can also be omitted.

[0116] In some embodiments of this application, in steps S10 and S30 of the above preparation method, the pH value of the alkaline ligand solution is 8.0~14.0, further 10.0~14.0, and even more further 11.0~14.0; as an example, the pH value of the alkaline ligand solution can be 8, 9, 10, 11, 12, 13, or 14. The pH value of the alkaline ligand solution can be controlled by controlling the concentration of the alkaline ligand solution. By controlling the pH value of the alkaline ligand solution, the degree of etching of the graphite particles by the alkaline ligand solution can be controlled, thereby controlling the pore size and specific surface area of ​​the porous graphite particles.

[0117] In some embodiments of this application, the first organic amine compound and the second organic amine compound are each independently small organic amine molecules, and the molar mass of the small organic amine molecule is less than or equal to 1000 g / mol, further less than or equal to 500 g / mol, and further may be less than or equal to 200 g / mol.

[0118] Furthermore, the aforementioned organic primary amine compound is a small organic amine molecule with a molar mass less than or equal to 1000 g / mol. As an example, the molar mass of the organic primary amine compound is less than or equal to 500 g / mol, and more specifically, less than or equal to 200 g / mol.

[0119] Furthermore, the organic amine groups in the first and second organic amine compounds each independently include primary amine groups. Furthermore, the functionality of the primary amine groups in the first organic amine compound is 2 to 5, and the functionality of the primary amine groups in the second organic amine compound is 1.

[0120] Furthermore, the number of carbon atoms in the first and second organic amine compounds mentioned above is independently 1 to 10.

[0121] Furthermore, the first organic amine compound includes ethylenediamine.

[0122] Furthermore, the second organic amine compound includes at least one of methylamine and ethylamine.

[0123] In some embodiments of this application, in steps S10 and S30 of the above preparation method, the graphite particles and the ligand solution are mixed under heating conditions. The heating temperature is 50℃~120℃, and the heating time is 2h~72h. As an example, the heating temperature can be 50℃, 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, or 120℃; as an example, the heating time can be 2h, 5h, 10h, 12h, 15h, 20h, 24h, 30h, 40h, 48h, 50h, 60h, 65h, 70h, or 72h.

[0124] Optionally, the heating temperature in steps S10 and S30 is 80℃~100℃, and the heating time is 12h~24h.

[0125] In some embodiments of this application, in steps S10, S20, and S30 of the above preparation method, solid-liquid separation can be performed after mixing by means of vacuum filtration, and the solid phase can be dried. Further, the drying temperature can be 60℃~100℃, and the drying time can be 2h~10h.

[0126] In some embodiments of this application, in steps S20 and S30 of the above preparation method, the metal element in the metal salt solution includes one or more of Fe, Co, Ni, Cu, Zn, Mn, Mg and Sc.

[0127] In some embodiments of this application, the metal salt in the metal salt solution includes one or more of hydrochloride, nitrate and sulfate.

[0128] The metal ions in metal salts are all in excess, and even when coordinated with ligands, they are difficult to completely transform into single-atom modifications on the end faces of porous graphite particles. One of the main factors determining the number of single-atom sites on the end faces of porous graphite is the number of defect sites on the end faces of porous graphite.

[0129] In some embodiments of this application, the concentration of the metal salt solution is 0.001 mol·L⁻¹. -1 ~1mol·L -1 For example, it could be 0.001 mol·L⁻¹ -1 0.01 mol·L -1 0.1 mol·L -1 0.2 mol·L -1 0.5 mol·L -1 0.8 mol·L -1 1 mol·L -1 Furthermore, it can be 0.1 mol·L⁻¹ -1 ~1mol·L -1 Furthermore, it is 0.2 mol·L⁻¹ -1 ~1mol·L -1 .

[0130] In some embodiments of this application, the mass ratio of the metal salt to the porous graphite particles in the metal salt solution is (0.5~5):100. As an example, this mass ratio can be 0.5:100, 1:100, 1.5:100, 1.8:100, 2:100, 3:100, 4:100, or 5:100.

[0131] In some embodiments of this application, in step S20 of the above preparation method, the porous graphite particles are mixed with the metal salt solution for 0.5 h to 2 h. The mixing temperature can be room temperature.

[0132] In some embodiments of this application, in step S20 of the above preparation method, the reducing atmosphere includes at least one of nitrogen and argon, as well as hydrogen. Further, the volume percentage of hydrogen in the reducing atmosphere is 3.0% to 10.0%. Optionally, the reducing atmosphere can be a mixture of hydrogen and argon.

[0133] In some embodiments of this application, in step S20 of the above preparation method, the heat treatment temperature is 400℃~1000℃, and the time is 2h~24h. Further, the heating rate to the above heat treatment temperature is 1℃ / min~10℃ / min.

[0134] As an example, in step S20 of the above preparation method, the heat treatment temperature can be 400℃, 500℃, 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, 900℃, or 1000℃; the time can be 2h, 5h, 10h, 12h, 15h, 20h, or 24h. As an example, the heating rate can be 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, 9℃ / min, or 10℃ / min.

[0135] Optionally, the heating rate is 2.0℃ / min to 5.0℃ / min; optionally, the heat treatment temperature is 600℃ to 1000℃, and more preferably 700℃ to 800℃; optionally, the heat treatment time is 2h to 10h, and more preferably 2h to 5h.

[0136] Furthermore, depending on the type of metal salt, the volume ratio of hydrogen in the reducing atmosphere and the temperature of the heat treatment can be adjusted to reduce different types of metal ions, form metal single atoms, and achieve the modification of different types of metal single atoms.

[0137] Another embodiment of this application provides a negative electrode sheet, comprising at least one of the above-described negative electrode active material and the negative electrode active material prepared by the above-described preparation method.

[0138] Another embodiment of this application provides a secondary battery. The secondary battery includes at least one of the above-described negative electrode active material, the negative electrode active material prepared by the above-described preparation method, and the above-described negative electrode sheet.

[0139] Another embodiment of this application provides an electrical device. The electrical device includes at least one of the above-described negative electrode active material, the negative electrode active material prepared by the above-described preparation method, the above-described negative electrode sheet, and the above-described secondary battery.

[0140] The secondary battery and power-consuming device of this application will be described below with appropriate reference to the accompanying drawings.

[0141] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0142] Negative electrode sheet

[0143] The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector. The negative electrode film layer includes the aforementioned negative electrode active material, namely the aforementioned modified graphite, specifically a porous graphite material modified with a single metal atom.

[0144] As a non-limiting example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0145] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on the polymeric material substrate. Non-limiting examples of the metal material in the negative electrode current collector may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the negative electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0146] In some embodiments, the negative electrode active material in the negative electrode film layer is only the modified graphite described above. In some embodiments, in addition to the negative electrode active material described above, the negative electrode film layer may also include other negative electrode active materials, such as those known in the art for use in batteries. As a non-limiting example, the negative electrode active material may include one or more of the following materials: unmodified artificial graphite, unmodified natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include one or more of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used.

[0147] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0148] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0149] In some embodiments, the negative electrode film may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose, CMC-Na).

[0150] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder, and any other components, in a solvent (a non-limiting example of a solvent is deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto at least one surface of a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing, and other processes. The surface of the negative electrode current collector coated with the negative electrode slurry can be a single surface of the negative electrode current collector or both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt%~60wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000~10000 mPa·s. When coating the negative electrode slurry, the coating unit areal density (dry weight, deducting solvent) can be 75~220 g / m². 2 The compaction density of the negative electrode sheet can be 1.0 g / cm³. 3 ~1.8 g / cm 3 .

[0151] Positive electrode sheet

[0152] The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector, the positive electrode film layer including a positive electrode active material.

[0153] As a non-limiting example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0154] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be obtained by forming a metal material on a polymer material substrate. Non-limiting examples of the metal material in the positive electrode current collector may include one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymer material substrate in the positive electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0155] In some embodiments, the positive electrode active material may be a known positive electrode active material for batteries. As a non-limiting example, the positive electrode active material may include one or more of the following materials: lithium phosphates with an olivine structure, lithium metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium metal oxides include, but are not limited to, one or more of lithium cobalt oxide (such as LiCoO2), lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Non-limiting examples of lithium phosphates with an olivine structure include, but are not limited to, one or more of lithium iron phosphate, lithium iron phosphate and carbon composites, lithium manganese phosphate, lithium manganese phosphate and carbon composites, lithium iron manganese phosphate, and lithium manganese iron phosphate and carbon composites. Non-limiting examples of lithium cobalt oxides may include LiCoO2; non-limiting examples of lithium nickel oxides may include LiNiO2; non-limiting examples of lithium manganese oxides may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 Examples of lithium nickel cobalt aluminum oxides include LiNi, etc. 0.8 Co 0.15 Al 0.05 O2.

[0156] In some embodiments, the positive electrode active material layer may optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.

[0157] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0158] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as the positive active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry; coating the positive electrode slurry onto at least one surface of the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing, and other processes. The solvent can be selected from, but is not limited to, any of the solvents described in the foregoing embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode current collector coated with the positive electrode slurry can be a single surface or both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt% to 80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000 mPa·s to 25000 mPa·s. When coating the positive electrode slurry, the areal density per unit area of ​​the coating, based on dry weight (excluding solvent), can be 15 mg / cm³. 2 ~35mg / cm 2 The compaction density of the positive electrode sheet can be 3.0 g / cm³. 3 ~3.6g / cm 3 3.3g / cm³ is an option. 3 ~3.5g / cm 3 .

[0159] electrolytes

[0160] Electrolytes function to conduct ions between the positive and negative electrode plates. This application does not impose any particular restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or completely solid.

[0161] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0162] In some embodiments, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).

[0163] In some embodiments, the solvent may include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butene carbonate, fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0164] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0165] In some embodiments, the additives in the electrolyte may include, but are not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethyl ethylene carbonate (TFPC), etc.

[0166] Separating membrane

[0167] In some embodiments, the secondary battery also includes a separator.

[0168] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0169] This application does not impose any particular restrictions on the type of separator membrane; any known porous separator membrane with good chemical and mechanical stability can be selected.

[0170] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0171] In some embodiments, the thickness of the isolation membrane is 6μm to 40μm, and optionally 12μm to 20μm.

[0172] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding process or a stacking process.

[0173] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.

[0174] In this application, unless otherwise specified, "cell battery" refers to the basic unit capable of converting chemical energy into electrical energy, and generally includes at least a positive electrode, a negative electrode, and an electrolyte. During the charging and discharging process of the battery, active ions move back and forth between the positive and negative electrode plates, inserting and extracting. The electrolyte acts as a conductor for the active ions between the positive and negative electrode plates.

[0175] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 The secondary battery shown is a single battery cell, which serves as an example of a square-structured battery cell.

[0176] In some embodiments, the secondary battery may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above. In some embodiments, the outer packaging of the secondary battery may be a rigid shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a flexible package, such as a pouch. The material of the flexible package may be plastic; further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0177] In some of these embodiments, reference is made to Figure 2The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be selected by those skilled in the art according to actual needs.

[0178] In some embodiments, the secondary battery can be a battery module or a battery pack. A battery module includes at least one battery cell. The number of battery cells in a battery module can be one or more, and those skilled in the art can select an appropriate number based on the application and capacity of the battery module.

[0179] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other way. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.

[0180] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0181] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more. Those skilled in the art can select an appropriate number according to the application and capacity of the battery pack.

[0182] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0183] In addition, one embodiment of this application also provides an electrical device, which includes the secondary battery provided in this application. The secondary battery can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptops, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to.

[0184] As an electrical device, a rechargeable battery can be selected based on its usage requirements.

[0185] Figure 6 Here is an example of an electrical device 6. This electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this electrical device, a battery pack or battery module can be used.

[0186] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0187] To make the technical problems, technical solutions, and beneficial effects solved by this application clearer, the application will be further described in detail below with reference to embodiments and accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit this application or its applications. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0188] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0189] Example 1

[0190] (1) Preparation of negative electrode active material:

[0191] 1.1 Preparation of porous graphite materials:

[0192] 500 mL of ethylenediamine was added to 5 L of deionized water (the pH of the resulting ethylenediamine aqueous solution was 12.36 according to a pH meter), and stirred for 5 min. Then, 1 kg of commercial graphite (artificial spherical graphite with a Dv50 particle size of 14.5 μm) was added, stirred, and the system temperature was controlled at 100 °C. After stirring for 24 h, the mixture was filtered, washed once with deionized water, and the solid was dried to obtain porous graphite material.

[0193] 1.2 End-face single-atom modified porous graphite materials:

[0194] 0.2 mol·L -1 500 mL of a cobalt nitrate aqueous solution was added to 5 L of deionized water and stirred for 5 min. Then, 1 kg of the porous graphite material prepared in the previous step was added, stirred for 2 h, filtered, washed once with deionized water, and the solid was dried. Finally, the porous graphite impregnated with cobalt metal cations was placed in a high-temperature furnace, and a hydrogen-argon mixture with a hydrogen volume concentration of 5% was introduced. The heating rate was controlled at 2.0 °C / min, and the heat treatment temperature was 700 °C for thermal reduction calcination for 2.0 h. After heat treatment, the material was allowed to cool naturally to obtain the porous graphite material with cobalt single-atom modification on the end face, i.e., the negative electrode active material.

[0195] (2) Preparation of negative electrode sheet:

[0196] 92.0g of the porous graphite material with cobalt single-atom modification on the end face obtained in step (1), 2.0g of conductive agent (0.5g carbon nanotubes, 1.5g acetylene black), and 6.0g of binder (PVDF) were added to a certain amount of NMP and mixed under vacuum stirring to obtain a negative electrode slurry. The negative electrode slurry was uniformly coated on one side of a copper foil. After the copper foil was dried at room temperature, it was transferred to a 120℃ oven to dry for 1 hour, and then cold-pressed and slit to obtain a negative electrode sheet, wherein the coating amount per unit area on one side was 0.17g / 1540.25mm. 2 .

[0197] (3) Preparation of half-cells. The performance of the negative electrode was examined by preparing half-cells.

[0198] The negative electrode prepared in step (2) is assembled with a Li sheet (counter electrode), a separator (12 μm thick polypropylene separator) and an electrolyte (lithium salt LiPF6 concentration of 1 mol / L, solvent is EC, EMC and DEC in volume ratio of 20:20:60) into a coin cell.

[0199] Example 2

[0200] The process is basically the same as in Example 1, except that the cobalt nitrate aqueous solution in the preparation of the negative electrode active material in Example 1 (1) is replaced with an ferric chloride aqueous solution of the same molar concentration. All other conditions remain unchanged. Porous graphite material with iron single atom modification on the end face is obtained and a coin cell is obtained. The battery process and testing process remain unchanged.

[0201] Example 3

[0202] The process is basically the same as in Example 1, except that the cobalt nitrate aqueous solution in the preparation of the negative electrode active material in Example 1 (1) is replaced with copper chloride aqueous solution of the same molar concentration. All other conditions remain unchanged. Porous graphite material with copper single atom modification on the end face is obtained and a coin cell is obtained. The battery process and testing process remain unchanged.

[0203] Example 4

[0204] The process is basically the same as in Example 1, except that the cobalt nitrate aqueous solution in the preparation of the negative electrode active material in Example 1 (1) is replaced with nickel chloride aqueous solution of the same molar concentration. All other conditions remain unchanged. Porous graphite material with nickel single atom modification on the end face is obtained and a coin cell is obtained. The battery process and testing process remain unchanged.

[0205] Examples 5-8

[0206] The process is basically the same as in Example 1, except that the cobalt nitrate aqueous solution in the preparation of the negative electrode active material in Example 1 (1) is replaced with the metal salt aqueous solution in Table 1 with the same molar concentration. All other conditions remain unchanged. The corresponding end-face metal single-atom modified porous graphite material is obtained and a coin cell is obtained. The battery process and testing process remain unchanged.

[0207] Example 9

[0208] The process is basically the same as in Example 1, except that the amount of ethylenediamine used in the preparation of the negative electrode active material is increased (1) so that the pH value of the ethylenediamine aqueous solution is higher, as shown in Table 1.

[0209] Example 10

[0210] The process is basically the same as in Example 9, except that the molar concentration of the cobalt nitrate aqueous solution in the preparation of the negative electrode active material in Example 1 (1) is changed, as shown in Table 1. All other conditions remain unchanged, and the corresponding porous graphite material with single-atom cobalt metal modification on the end face is obtained. A coin cell is then obtained, and the battery process and testing process remain unchanged.

[0211] Examples 11-12

[0212] The process is basically the same as in Example 1, except that the molar concentration of the cobalt nitrate aqueous solution and the amount of ethylenediamine in the preparation of the negative electrode active material in Example 1 are changed to adjust the pH value of the ethylenediamine aqueous solution, as shown in Table 1. Other conditions remain unchanged, and the corresponding porous graphite material with cobalt metal single atom modification on the end face is obtained, and a button cell is obtained. The battery process and testing process remain unchanged.

[0213] Example 13

[0214] The process is basically the same as in Example 1, except that the heat treatment temperature in step 1.2 of (1) with end-face single-atom modified porous graphite material is changed to 800℃ and the heat treatment time is 5h. After the heat treatment is completed and the material is cooled naturally, the end-face cobalt single-atom modified porous graphite material, i.e., the negative electrode active material, can be obtained.

[0215] Example 14

[0216] The process is basically the same as in Example 1, except that the heat treatment temperature in step 1.2 of (1) with end-face single-atom modified porous graphite material is changed to 900℃ and the heat treatment time is 2.0h. After the heat treatment is completed and the material is allowed to cool naturally, the end-face cobalt single-atom modified porous graphite material, i.e., the negative electrode active material, can be obtained.

[0217] Example 15

[0218] The process is basically the same as in Example 4, except that the temperature of the heat treatment of the end-face single-atom modified porous graphite material in step 1.2 of (1) is changed to 400℃ and the heat treatment time is 24h. After the heat treatment is completed and the material is cooled naturally, the end-face cobalt single-atom modified porous graphite material, i.e., the negative electrode active material, can be obtained.

[0219] Example 16

[0220] The process is essentially the same as in Example 1, except for the preparation process of the negative electrode active material. Specifically, ethylenediamine solution and cobalt nitrate aqueous solution are simultaneously mixed with commercial graphite (artificial spherical graphite). The specific steps are as follows:

[0221] (1) Preparation of negative electrode active material:

[0222] Add 500 mL of ethylenediamine solution to 5 L of deionized water (the pH of the ethylenediamine solution is 12.36) and stir for 5 min; then, simultaneously add 0.2 mol·L⁻¹ -1A cobalt nitrate aqueous solution (500 mL) and 1 kg of commercial graphite (artificial spherical graphite) were mixed and stirred at 100℃ for 24 hours. The mixture was then filtered, washed once with deionized water, and the solid was dried. Finally, the dried graphite was placed in a high-temperature furnace, and a hydrogen-argon mixture with a hydrogen volume concentration of 5% was introduced. The heating rate was controlled at 2.0℃ / min, and the heat treatment was carried out at 700℃ for 2.0 hours. After heat treatment and natural cooling, the modified graphite material, i.e., the negative electrode active material, was obtained.

[0223] Comparative Example 1

[0224] The commercial graphite from Example 1 was directly fabricated into button cells, with the battery process and testing procedures remaining unchanged.

[0225] Comparative Example 2

[0226] The process is basically the same as in Example 1, except that the step of impregnating cobalt metal cations in the preparation of the negative electrode active material (1) is omitted. Instead, the porous graphite material obtained in step 1.1 of Example 1 is placed in a high-temperature furnace, and a hydrogen-argon mixture with a hydrogen volume concentration of 5% is introduced. The heating rate is controlled at 2.0℃ / min, the calcination temperature is 700℃, and the calcination time is 2.0h to obtain the final porous graphite material. The porous graphite is then used to prepare a coin cell, and the battery process and testing process remain unchanged.

[0227] Comparative Example 3

[0228] The process is basically the same as in Example 1, except that the preparation process of the negative electrode active material is different. Specifically, in step 1.1, sodium hydroxide solution is used instead of ethylenediamine solution, and a hydroxide solution with the same volume and pH value is used.

[0229] The following are performance tests.

[0230] (1) Scanning electron microscopy test.

[0231] The negative electrode active material prepared in Example 1 and the negative electrode active material used in Comparative Example 1 were subjected to scanning electron microscopy (SEM) tests to obtain... Figures 7-10 .

[0232] in, Figure 7 and Figure 8 These are low-magnification and high-magnification SEM images of the negative electrode active material prepared in Example 1 of this application. It can be seen that the microstructure of the end face of the porous graphite material in Example 1 is more porous, indicating that treatment with the organic amine solution produces corresponding etched pores on its end face, forming a porous end face structure.

[0233] Figure 9This is a low-magnification SEM image of the negative electrode active material used in Comparative Example 1 of this application. It can be seen from the image that the microstructure of the graphite end face is relatively dense.

[0234] Figure 10 These are dark-field SEM and EDS mapping images (EDS distribution diagram) of the negative electrode active material prepared in Example 1 of this application. The EDS mapping images show that Co elements tend to be distributed on the end faces of graphite, with a small amount also distributed on the basal face, but the distribution is more dense and concentrated on the end faces. This is because the end faces of graphite are richer in oxygen-containing functional groups than the basal faces, resulting in stronger van der Waals interactions with organic amines, thus enabling the preferential adsorption of organic amine groups on the graphite end faces. The organic amine groups adsorbed on the graphite end faces have a strong coordination interaction with metal cations, forming nitrogen-metal coordination bonds to anchor the metal ions; subsequent heat treatment in a reducing atmosphere reduces the metal ions to metal atoms.

[0235] (2) Raman spectroscopy and XRD tests.

[0236] The negative electrode active material prepared in Example 1 of this application was subjected to Raman spectroscopy testing, and the results are as follows: Figure 11 As shown.

[0237] From this, we can know that it is located at ~1580cm -1 The peak intensity of G at ~1380 cm⁻¹ is significantly greater than that at ~1380 cm⁻¹. -1 The intensity of the D peak at the 690 cm⁻¹ indicates that the porous graphite modified with cobalt single atoms at the end face has a high degree of graphitization. Further research shows that the characteristic Raman peak of the Co-O bond is at 690 cm⁻¹. -1 Position to the left and right, and Figure 11 The absence of a peak at this position indicates the absence of Co-O bonds.

[0238] The negative electrode active material prepared in Example 1 of this application was subjected to XRD testing, and the results are as follows: Figure 12 As shown, the XRD pattern only shows the characteristic peaks of graphite, and no diffraction peaks of elemental Co (Co-Co metallic bond) were observed.

[0239] from Figure 11 and Figure 12 It can be seen that the negative electrode active material prepared in Example 1 does not contain Co-Co bonds or Co-O bonds; combined with Figure 10 It can be seen that the Co element on the surface of the graphite material should be an individual atomic site, and there is no metallic bond between the atomic sites.

[0240] (3) Detection of the content of metal elements in the negative electrode active material.

[0241] The content of metal elements was determined using inductively coupled plasma atomic emission spectrometry (ICP). The specific procedure involved adding the negative electrode active material to a concentrated nitric acid solution, microwaving it, then removing the electrolyte and measuring the plasma atomic emission spectrum. The content of the corresponding metal element, i.e., the content of metal single-atom sites, was obtained by comparing the intensity of the spectral lines with a standard spectrum. The test results are shown in the table below.

[0242] (4) Graphitization degree test of negative electrode active material.

[0243] Methods for measuring the degree of graphitization of negative electrode active materials:

[0244] 1. Pretreatment: Add silicon powder; weigh the anode active material and silicon powder at a ratio of 5:1, grind them in a clean mortar for 50 minutes to ensure uniform mixing.

[0245] 2. Sample preparation: Powder, sample preparation method using a flat plate with a sample well depth of 0.5mm and a diameter of 25mm.

[0246] 3. Test: Starting angle 52°, ending angle 58°, step size 0.00836°, step duration 0.3s.

[0247] 4. Fixed core parameters: Voltage: 40KV, Current: 40mA, Anti-scattering slit: 1mm, 2Theta angle: 52-58°, Scan rate: 1° / min. The degree of graphitization was quantified based on the diffraction peak intensity around 54° of graphite. The test results are shown in the table below.

[0248] (5) Ratio performance test.

[0249] Using the LAND testing system, the coin cells prepared in each embodiment and comparative example were subjected to multi-stage charge-discharge rate tests. The specific test steps are as follows:

[0250] First stage: Let stand for 5 minutes, then discharge at a constant current of 0.05C to 0.005 V; after standing for 5 minutes, discharge at a constant current of 0.002mA to 0.005V; after standing for 5 minutes, charge at a constant current of 0.1C to 2.00 V, and repeat the cycle twice.

[0251] Second stage: Let stand for 5 minutes, then discharge at a constant current of 0.1C to 0.005 V; after standing for 5 minutes, charge at a constant current of 0.1C to 2.00V, and repeat five times.

[0252] Third stage: Let stand for 5 minutes, then discharge at a constant current of 0.33C to 0.005V; after standing for 5 minutes, charge at a constant current of 0.33C to 2.00V, and repeat five times.

[0253] Fourth stage: Let stand for 5 minutes, then discharge at a constant current of 0.5C to 0.005V; after standing for 5 minutes, charge at a constant current of 0.5C to 2.00V, and repeat five times.

[0254] Fifth stage: Let stand for 5 minutes, then discharge at a constant current of 1.0C to 0.005V; after standing for 5 minutes, charge at a constant current of 1.0C to 2.00V, and repeat five times.

[0255] Sixth step: Let stand for 5 minutes, then discharge at a constant current of 2.0C to 0.005V; after standing for 5 minutes, charge at a constant current of 2.0C to 2.00V, and repeat five times.

[0256] Seventh stage: Let stand for 5 minutes, then discharge at a constant current of 4.0C to 0.005V; after standing for 5 minutes, charge at a constant current of 4.0C to 2.00V, and cycle five times.

[0257] The rate performance test results of the coin cells prepared in Examples 1-3 and Comparative Examples 1-2 of this application are shown in the figure. Figure 13 As shown in the figure, it can be seen that, compared with Comparative Example 1, Comparative Example 2 obtains porous graphite by reacting organic amine aqueous solution with graphite and then etching it. Therefore, at higher discharge rates of 0.5C, 1C, and 2C, Comparative Example 2 has a higher specific capacity (i.e., specific capacity, unit: mAh·g). -1 Examples 1-3 showed significant advantages over Comparative Example 2 at a high discharge rate of 4C, indicating that introducing a porous structure can improve the fast charging performance of graphite.

[0258] Furthermore, after introducing end-face metal single atoms in Examples 1-3, the specific capacity of end-face single-atom graphite was significantly improved compared with the porous graphite of Comparative Example 2 at higher discharge rates of 0.5C, 1C, and 2C, as well as at a high discharge rate of 4C; indicating that the single atoms on the graphite end face can further improve the fast charging capability of graphite.

[0259] Furthermore, the ratio of 1C capacity to 0.33C capacity in each embodiment and comparative example was obtained. This ratio represents the 1C capacity utilization ratio with the capacity utilization at 0.33C as the baseline, as shown in Table 2, and is used as a rate performance parameter.

[0260] The parameters and test results of the above embodiments and comparative examples are shown in Tables 1 and 2 below. The method for testing the specific surface area of ​​the negative electrode active material is as described above.

[0261] Table 1

[0262]

[0263] Table 2

[0264]

[0265] Comparative Example 1 used commercial graphite; Comparative Example 2 used porous graphite without cobalt loading; Comparative Example 3 used sodium hydroxide etching to introduce sodium ions, making the graphite surface alkaline. When a metal salt solution was subsequently added, metal cations easily formed metal hydroxides on the surface of the graphite particles. After subsequent calcination, metal oxide residues may remain, or the hydroxides may agglomerate into metal oxide particles after calcination and decomposition. Metal ions in these metal oxide particles can dissolve during battery testing, triggering side reactions and causing micro-short circuits within the battery, thus degrading battery performance. Comparison of the various examples with the comparative examples shows that the rate performance of each example is superior to that of the comparative examples.

[0266] It should be noted that the degree of graphitization in Example 2 is higher than that in Example 1 because the types of metal sites are different. It should be that the Fe sites catalyze graphite crystallization during the subsequent calcination process, thereby improving the overall crystallinity.

[0267] Compared to Example 1, the ethylenediamine aqueous solution in Examples 9-10 has a higher pH value, higher etching effect on graphite, higher specific surface area of ​​graphite, more lithium ion channels inside graphite, and better rate performance at 1C.

[0268] Compared to Example 1, the ethylenediamine aqueous solution in Examples 11-12 has a lower pH value, a lower degree of graphite etching, and a lower specific surface area after etching. The metal salt in Examples 11-12 is in excess. Therefore, as the specific surface area of ​​graphite decreases, the metal element content in Examples 11-12 also decreases, thus reducing the rate performance of 1C.

[0269] Compared to Example 1, the calcination temperature of Example 15 is lower, and the surface layer may not be completely carbonized, resulting in a lower specific surface area and the presence of a small amount of incompletely reduced metal. Therefore, it is easy to trigger battery side reactions during battery operation, and the high-rate performance is reduced.

[0270] Example 16 uses a different preparation process. It mixes ethylenediamine solution and cobalt nitrate aqueous solution with commercial graphite. Cobalt ions coordinate with ethylenediamine, but the ethylenediamine is in excess. Excess ethylenediamine can still etch graphite. Therefore, compared with Example 1, only a small amount of metal ions are anchored on the graphite surface, and the final graphite surface has a small number of single-atom sites.

[0271] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0272] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A negative electrode active material, characterized in that, It includes porous graphite particles and metal single atoms disposed on the porous graphite particles; The porous graphite particles have a base surface and an end face connected to the base surface on the crystalline material surface. The end face has a porous structure and is provided with the metal single atom.

2. The negative electrode active material as described in claim 1, characterized in that, The base surface is also provided with the metal single atoms.

3. The negative electrode active material as described in claim 1, characterized in that, The negative electrode active material satisfies at least one of the following conditions: (1) The specific surface area of ​​the negative electrode active material is 1.2 m². 2 ·g -1 ~5.0 m 2 ·g -1 ; (2) The Dv50 particle size of the porous graphite particles is 5μm~50μm; (3) The porous graphite particles include at least one of artificial graphite and natural graphite.

4. The negative electrode active material according to any one of claims 1 to 3, characterized in that, The negative electrode active material satisfies at least one of the following conditions: (1) In the negative electrode active material, the mass content of the metal single atom is 0.01wt%~0.5wt%; (2) The degree of graphitization of the negative electrode active material is 90%~97%.

5. The negative electrode active material according to any one of claims 1 to 3, characterized in that, The types of metal single atoms include at least one of transition metals and alkaline earth metals.

6. The negative electrode active material as described in claim 5, characterized in that, The types of metal single atoms include one or more of Fe, Co, Ni, Cu, Zn, Mn, Mg, and Sc.

7. The negative electrode active material according to any one of claims 1 to 3 and 6, characterized in that, The negative electrode active material also includes at least one of nitrogen (N) and amorphous carbon doped onto the surface of the porous graphite particles.

8. A method for preparing a negative electrode active material, characterized in that, Includes the following steps: Graphite particles are etched by mixing them with an alkaline ligand solution and then dried to obtain porous graphite particles; the alkaline ligand includes an organic amine group, and the ligand is attached to the surface of the porous graphite particles. The porous graphite particles are mixed with a metal salt solution and dried, then heat-treated in a reducing atmosphere to obtain the negative electrode active material; wherein, the metal ions in the metal salt can form a complex with the organic amine groups in the ligands on the surface of the porous graphite particles.

9. A method for preparing a negative electrode active material, characterized in that, Includes the following steps: Graphite particles are mixed with an alkaline ligand solution and a metal salt solution, dried, and then heat-treated in a reducing atmosphere to obtain the negative electrode active material. The alkaline ligand solution etches the graphite particles to form porous graphite particles. The alkaline ligand includes an organic amine group. The ligand is attached to the surface of the porous graphite particles. The metal ions in the metal salt can form a complex with the organic amine group in the ligand on the surface of the porous graphite particles.

10. The method for preparing the negative electrode active material as described in claim 8 or 9, characterized in that, The first organic amine compound has an organic amine group with a functionality greater than 1, and the first organic amine compound is a basic compound.

11. The method for preparing the negative electrode active material according to claim 10, characterized in that, The alkaline ligand solution further includes a second organic amine compound, wherein the functionality of the organic amine group in the second organic amine compound is 1.

12. The method for preparing the negative electrode active material as described in claim 11, characterized in that, The preparation method satisfies at least one of the following characteristics: (1) The pH value of the alkaline ligand solution is 8.0~14.0; (2) The functionality of the organic amine group in the first organic amine compound is 2 to 5; (3) The molar mass of the first organic amine compound is less than or equal to 1000 g / mol; (4) The molar mass of the second organic amine compound is less than or equal to 1000 g / mol.

13. The method for preparing the negative electrode active material as described in claim 11, characterized in that, The preparation method satisfies at least one of the following characteristics: (1) The organic amine groups in the first organic amine compound and the second organic amine compound each independently include primary amine groups; (2) The molar mass of the first organic amine compound is less than or equal to 500 g / mol; (3) The molar mass of the second organic amine compound is less than or equal to 500 g / mol; (4) The number of carbon atoms in the first organic amine compound and the second organic amine compound is 1 to 10.

14. The method for preparing the negative electrode active material as described in claim 11, characterized in that, The preparation method satisfies at least one of the following characteristics: (1) The first organic amine compound includes ethylenediamine; (2) The second organic amine compound includes at least one of methylamine and ethylamine.

15. The method for preparing the negative electrode active material according to any one of claims 8 to 9, characterized in that, The metal salt solution satisfies at least one of the following characteristics: (1) The metal elements in the metal salt solution include at least one of transition metals and alkaline earth metals; (2) The metal salt in the metal salt solution includes one or more of hydrochloride, nitrate and sulfate; (3) The concentration of the metal salt solution is 0.001 mol·L. -1 ~1mol·L -1 ; (4) The mass ratio of the metal salt in the metal salt solution to the porous graphite particles is (0.5~5):

100.

16. The method for preparing the negative electrode active material according to any one of claims 8 to 9, characterized in that, The graphite particles and ligand solution are mixed under heating conditions, the heating temperature is 50℃~120℃, and the heating time is 2 h~72 h.

17. The method for preparing the negative electrode active material according to any one of claims 8 to 9, characterized in that, The preparation method satisfies at least one of the following characteristics: (1) The time for mixing the porous graphite particles with the metal salt solution is 0.5h to 2h; (2) The reducing atmosphere includes at least one of nitrogen and argon, as well as hydrogen; (3) The temperature of the heat treatment is 400℃~1000℃ and the time is 2h~24h; (4) The heating rate to the heat treatment temperature is 1℃ / min to 10℃ / min.

18. The method for preparing the negative electrode active material as described in claim 17, characterized in that, The preparation method satisfies at least one of the following characteristics: (1) The volume percentage of hydrogen in the reducing atmosphere is 3.0%~10.0%; (2) The heat treatment temperature is 700℃~800℃ and the time is 2h~5h; (3) The heating rate to the heat treatment temperature is 2.0℃ / min to 5.0℃ / min.

19. A negative electrode sheet, characterized in that, It includes the negative electrode active material according to any one of claims 1 to 7 or the negative electrode active material prepared by the preparation method according to any one of claims 8 to 18.

20. A secondary battery, characterized in that, Includes the negative electrode sheet as described in claim 19.

21. An electrical appliance, characterized in that, It includes the negative electrode active material according to any one of claims 1 to 7, the negative electrode active material prepared by the preparation method according to any one of claims 8 to 18, the negative electrode sheet according to claim 19, or the secondary battery according to claim 20.

Citation Information

Patent Citations

  • Alkali metal atom gas chamber

    CN216595920U

  • Method of synthesizing porous composite including single atom metal catalysts and nitrogen atoms in hierarchical carbon material from carbon dioxide containing gas