Spherical aluminum oxide and silicon rubber heat-conducting composite material thereof

By modifying spherical alumina with an amphiphilic fluorosilicone thermal conductive interface enhancer, the problems of interface thermal resistance and mechanical properties of spherical alumina and silicone rubber composite materials are solved, and the synergistic gain of thermal conductivity, insulation and flexibility is achieved. It is suitable for power battery pack heat dissipation gaskets, high-frequency circuit packaging and wearable devices.

CN120623576AActive Publication Date: 2025-09-12JIAN YUSHUN NEW MATERIALS CO LTD

Patent Information

Application Number
CN202511069218.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-31
Publication Date
2025-09-12
Estimated Expiration
2045-07-31

AI Technical Summary

Technical Problem

In the existing technology, spherical alumina and silicone rubber composites have problems in interface thermal resistance, mechanical properties and multi-level filler dispersion, resulting in low thermal conductivity, deteriorated mechanical properties and poor dispersion, making it difficult to meet the requirements of high thermal conductivity, good insulation and mechanical flexibility.

Method used

The surface of spherical alumina is modified with an amphiphilic fluorosilicone thermal conductive interface enhancer. By constructing a multifunctional block enhancer containing fluorine chain ion blocks and reactive siloxane end groups, combined with spherical alumina powder with three-level particle sizes, interface bridging and cross-linking enhancement are achieved, thereby enhancing thermal conductivity and improving mechanical properties.

Benefits of technology

It significantly improves the thermal conductivity of the composite material, reduces the interfacial thermal resistance, and increases the tensile strength and breakdown voltage, meeting the needs of power battery pack heat dissipation gaskets, high-frequency circuit packaging and wearable devices, and the process is compatible with industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120623576A_ABST
    Figure CN120623576A_ABST
Patent Text Reader

Abstract

The invention discloses spherical aluminum oxide and a silicone rubber heat conduction composite material thereof, and belongs to the technical field of functional polymer materials. The spherical aluminum oxide is subjected to surface modification through an amphiphilic fluorosilicone heat conduction interface synergist; comprising the following raw materials in parts by weight: 100-200 parts of vinyl silicone oil, 1-6 parts of side hydrogen-containing silicone oil, 1-6 parts of end hydrogen-containing silicone oil, 0.2-2 parts of a platinum catalyst, 0.01-0.1 part of an inhibitor and 2500-6000 parts of amphiphilic fluorine-silicon heat-conducting interface synergistic spherical aluminum oxide powder. Through surface modification of spherical aluminum oxide, the prepared silicone rubber heat-conducting composite material realizes synergistic gain of heat conduction, insulation and flexibility, and can meet the requirements of multiple fields such as power battery pack heat dissipation gaskets, high-frequency circuit packaging and wearable equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional polymer materials, and in particular relates to a spherical alumina and a silicone rubber heat-conducting composite material. Background Art

[0002] With the development of 5G communications, new energy vehicle power modules, and high-density electronic devices, heat dissipation materials need to take into account high thermal conductivity, good insulation, mechanical flexibility, and flame retardancy. Silicone rubber has become an ideal matrix due to its weather resistance, insulation, and processability, while spherical alumina has been widely used due to its high thermal conductivity and low cost. Although research has made progress, the following problems remain to be solved: (1) Interface thermal resistance problem: Traditional silane coupling agent modification cannot completely eliminate the interface energy barrier between Al2O3 and silicone oil. When the filling is high, the interfacial air gap leads to low thermal conductivity; (2) Deterioration of mechanical properties: Increased filler content leads to material embrittlement and increased hardness, which limits flexible installation scenarios; (3) Poor dispersion of multi-level fillers: Mixed particle size fillers are prone to stratification due to density differences, reducing the packing density.

[0003] The low hydrogen content in commercially available poly(methylhydrogensiloxane) limits the number of hydrosilylation reaction sites, preventing a significant increase in the mesogenic grafting density, and thus limiting the enhancement of the intrinsic thermal conductivity of polydimethylsiloxane. In recent years, ring-opening polymerization has been widely used in the synthesis of high-performance polydimethylsiloxane. By precisely controlling the type and feed ratio of cyclosiloxane monomers, ring-opening polymerization can introduce specific functional groups into the polydimethylsiloxane molecular chain, fine-tuning the chain structure, significantly increasing the grafting density of these groups, and efficiently obtaining the desired product. Summary of the Invention

[0004] To overcome the shortcomings of the above-mentioned prior art, the present invention provides a spherical alumina and silicone rubber thermal conductive composite material, which achieves synergistic gains in thermal conductivity, insulation, and flexibility through the innovative design of an amphiphilic fluorosilicone thermal conductive interface synergist. The technical solution to achieve the purpose of the present invention is as follows:

[0005] The present invention provides a spherical alumina, wherein the spherical alumina is surface-modified with an amphiphilic fluorosilicone thermal conductive interface synergist, and the structure of the amphiphilic fluorosilicone thermal conductive interface synergist is shown in Formula 1:

[0006] Among them, a:b:c=(1~100):(1~100):(1~10), e:f=1:(1~4).

[0007] Preferably, in parts by weight, the spherical alumina includes 1 to 5 parts of spherical alumina with an average particle size of 3 to 10 μm, 5 to 10 parts of spherical alumina with an average particle size of 20 to 40 μm, and 10 to 15 parts of spherical alumina with an average particle size of 90 to 140 μm.

[0008] Preferably, the step of surface modification of the spherical alumina with an amphiphilic fluorosilicone thermal conductive interface synergist is:

[0009] (1) baking the spherical alumina to remove moisture, cooling and sealing for later use;

[0010] (2) preparing a 0.1% to 1% by mass isopropoxy distearate acyloxyaluminate solution in anhydrous toluene; immersing the baked spherical alumina in the solution, ultrasonically dispersing, stirring, filtering, and drying to obtain a primary modified spherical alumina;

[0011] (3) preparing a silane coupling agent solution with a mass fraction of 0.1% to 1% using ethanol; immersing the primary modified spherical alumina obtained in step (2) in the silane coupling agent solution, ultrasonically dispersing, stirring, filtering, and drying to obtain a double-modified spherical alumina;

[0012] (4) The amphiphilic fluorosilicone thermal conductive interface enhancer is prepared into a hexafluoroisopropanol solution with a mass fraction of 0.5-0.8%, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are added, ultrasonic-assisted dissolution is carried out, the temperature is raised to 45-50°C for activation, and water and oxygen are removed to obtain a treatment agent solution; the double-modified spherical alumina obtained in step (3) is slowly added to the treatment agent solution, triethylamine is added to adjust the pH to 7.5-8.5, the temperature is maintained at 35-45°C, ultrasonically dispersed by stirring, filtered, purified by precipitation with cold ether and n-hexane, and Soxhlet extracted with a mixed solution of methanol and chloroform in a volume ratio of 1:2 for 40-48 hours to remove small molecular impurities, and vacuum dried to obtain spherical alumina with amphiphilic fluorosilicone thermal conductive interface enhancer.

[0013] Preferably, the silane coupling agent is 3-aminopropyltriethoxysilane.

[0014] Preferably, the preparation method of the amphiphilic fluorosilicone thermal conductive interface synergist comprises the following steps:

[0015] (1) Preparation of perfluoropolyether methacrylate: 1 eq of perfluoropolyether alcohol was mixed with 1.2-1.3 eq of triethylamine previously dehydrated with calcium hydride in dichloromethane, and the mixture was cooled to 0°C in an ice bath. 1.2-1.3 eq of a dichloromethane solution of methacryloyl chloride was slowly added dropwise. After 30 minutes of addition, the mixture was allowed to react at the same temperature for 2-3 hours, then the mixture was allowed to warm to room temperature and the reaction was continued for 10-12 hours. The mixture was filtered and subjected to silica gel column chromatography to obtain the product, perfluoropolyether methacrylate.

[0016] (2) Synthesis of PMAA-PDMA-PFPE zwitterionic block copolymer: 1 eq methacrylic acid, 0.02 eq RAFT agent, 0.004 eq initiator, 3A molecular sieve and deionized water were added to a 50 mL double-necked flask, the mixture was deoxygenated by nitrogen bubbling for 20 to 30 min, and reacted at 70 ° C for 3 to 4 h to obtain PMAA block; in a sealed bottle protected by nitrogen, 1 eq dimethylaminoethyl methacrylate, 0.0067 eq RAFT agent, 1.0 eq sodium hydroxide and 5.53 g deionized water were mixed and deoxygenated for 30 to 40 min, and then the mixture was injected into the PMAA reaction system under nitrogen atmosphere, and reacted at 65 to 75 ° C for 9 to 10 h. The final solution pH was 8 to 9, and a viscous yellow dispersion was obtained; the reaction system was cooled to 40 ° C. The mixture was heated to 40-45° C., water was removed by distillation under reduced pressure, 20 mL of hexafluoroisopropanol and 3A molecular sieves were added, the polymer was dissolved by stirring, and 0.5 eq of triethylamine was added until the pH was 7 to neutralize the residual carboxylic acid. In a sealed bottle under nitrogen protection, 1 eq of perfluoropolyether methacrylate, 0.002 eq of V-70 and 10 mL of hexafluoroisopropanol were mixed, and after ultrasonic deoxygenation for 10-15 minutes, the mixture was injected into the main reaction system and reacted at 60-65° C. in the dark for 12-16 hours. After the reaction, liquid nitrogen was quenched, the reaction was terminated by air, and a mixed solution of cold ether and n-hexane in a volume ratio of 1:1 was added dropwise. The precipitate was collected by centrifugation, and the precipitate was repeatedly dissolved in hexafluoroisopropanol and cold ether three times. The mixture was vacuum dried at 35-45° C. for 20-24 hours to obtain a PMAA-PDMA-PFPE zwitterionic block copolymer.

[0017] Preferably, the RAFT agent is selected from 4-cyano-4-[(2-phenylethyl)thio]thiooxymethyl]thio]-pentanoic acid; and the initiator is selected from 4,4'-azobis(4-cyanopentanoic acid).

[0018] (3) Take 1eq of the above-mentioned PMAA-PDMA-PFPE zwitterionic block copolymer, add anhydrous hexafluoroisopropanol to dissolve it, then add 3A molecular sieves, and bubbling nitrogen for 20 to 30 minutes to remove water; cool to 0°C in an ice bath, add 1.2eq of condensing agent and 0.1eq of catalyst in sequence; slowly drop 1.5eq of hexafluoroisopropanol solution of enol, raise the temperature to 30°C, stir in the dark for 20 to 24 hours, and use 30W low-frequency ultrasound to assist diffusion; filter after the reaction, add 10 times the volume of -20°C n-pentane to the reaction solution, and collect the precipitate by centrifugation; dissolve the precipitate in tetrahydrofuran, and use a mixture of THF and water in a volume ratio of 1:1 The solution was dialyzed for 40 to 48 hours and vacuum-dried to obtain an olefinic zwitterionic block copolymer; 1 eq of the olefinic zwitterionic block copolymer was dissolved in 450 eq of deionized water to prepare a 0.5% aqueous solution, 1 eq of hydrazine hydrate was added to 30 eq of deionized water to prepare a hydrazine hydrate solution, the hydrazine hydrate solution was added to the olefinic zwitterionic block copolymer solution, the temperature was controlled at 20 to 25° C., the pH was adjusted to 8.5 to 9.5, the mixture was allowed to stand for 10 to 20 minutes to precipitate, the supernatant was decanted, the precipitate was washed three times with deionized water at pH 6, and the mixture was vacuum-dried to obtain an olefinic zwitterionic block copolymer with trithiocarbonate end groups removed;

[0019] (4) 1 eq of the product of step (3) was dissolved in toluene, and 0.25 eq to 1 eq of 1,3,5,7-tetramethylcyclotetrasiloxane and Karstedt platinum catalyst were added under a nitrogen atmosphere, and the mixture was refluxed at 100 to 110° C. for 20 to 24 h; the reaction solution was adsorbed on activated carbon for 10 to 12 h, filtered, and the filtrate was concentrated by rotary evaporation and vacuum dried at 80 to 85° C. overnight to obtain a cyclosiloxane graft copolymer having the following structure:

[0020]

[0021] (5) Preparation of dimethylsiloxane oligomer catalyst: 1.0 eq of tetramethylammonium hydroxide and 1.1-1.2 eq of octamethylcyclotetrasiloxane were added to a 250 mL three-necked flask, and 4.0 eq of cyclohexane was injected. The mixture was stirred at 80°C for 24 h under nitrogen protection. The crystallization water and condensation water were monitored and removed in real time by a Dean-Stark water trap. After the reaction was completed, nitrogen was bubbled at 85°C for 1 h to remove the residual cyclohexane, thereby obtaining the dimethylsiloxane oligomer catalyst TMAS.

[0022] (6) 1 eq of cyclosiloxane graft copolymer and 0.4-0.5 eq of tetramethylcyclotetrasiloxane were added to the reaction flask, and oxygen was removed by repeated nitrogen replacement and vacuum extraction. The temperature was raised to 85°C under nitrogen protection, and a 0.01 eq of TMAS catalyst tetrahydrofuran solution was injected with a pipette. The mixture was vigorously stirred and polymerized at 100-105°C for 20-24 hours; the temperature was then raised to 130-140°C to decompose the residual catalyst, and low molecular weight by-products were removed by nitrogen bubbling at 160-170°C; the crude product was dissolved in dichloromethane, purified by precipitation with 6 times the volume of methanol, and vacuum dried at 80°C for 2 hours to obtain a brown solid; the solid was placed in a preheated mold, melted at 70-75°C for 15-25 minutes, and naturally cooled and demolded to obtain an amphiphilic fluorosilicone thermal conductive interface enhancer, the structure of which is shown below:

[0023]

[0024] Preferably, the condensing agent is N,N'-diisopropylcarbodiimide; the catalyst is 4-dimethylaminopyridine; the enol is one or more of propenol, butenol, and pentenol; and the concentration of the hexafluoroisopropanol solution of the enol is 1 mol / L.

[0025] Another object of the present invention is to provide a silicone rubber thermal conductive composite material, which comprises the following raw materials, in parts by weight: 100 to 200 parts of vinyl silicone oil, 1 to 6 parts of side hydrogen-containing silicone oil, 1 to 6 parts of end hydrogen-containing silicone oil, 0.2 to 2 parts of platinum catalyst, 0.01 to 0.1 parts of inhibitor, and 2500 to 6000 parts of spherical alumina surface-modified with an amphiphilic fluorosilicone thermal conductive interface enhancer.

[0026] Preferably, the vinyl content of the vinyl silicone oil is 0.21% to 1.4 wt%.

[0027] Preferably, the hydrogen content of the side hydrogenated silicone oil is 0.05% to 1.2 wt%.

[0028] Preferably, the hydrogen content of the hydrogen-terminated silicone oil is 0.05% to 1.0 wt%.

[0029] Preferably, the inhibitor is one or more of 3-methyl-1-butyn-3-ol, 1-ethynylcyclohexanol, 3-propyl-1-butyn-3-ol, and 3-octyl-1-butyn-3-ol.

[0030] Preferably, the platinum catalyst is a platinum compound or complex with a platinum content of 1000 to 5000 ppm.

[0031] The present invention also provides a method for preparing a silicone rubber thermally conductive composite material, comprising the following steps:

[0032] S1. Weigh the raw materials in parts by weight and stir the vinyl silicone oil, inhibitor, and platinum catalyst in a preparation container;

[0033] S2. Add hydrogen silicone oil to the container and stir evenly at the end;

[0034] S3. Amphiphilic fluorine-silicone thermally conductive interface enhancing spherical alumina powder was added to step S2 in batches and mixed, and evacuated to a vacuum degree of ≤10 kPa to obtain a uniformly mixed thermally conductive base material;

[0035] S4. Place the thermally conductive base material between two fluoroplastic films, press the sheet through a calender, and cure it in a vulcanization furnace to obtain a spherical alumina silicone rubber thermally conductive composite material.

[0036] Beneficial effects

[0037] The present invention has achieved significant technological breakthroughs and multiple beneficial effects through the innovative design of amphiphilic fluorosilicone thermal conductive interface synergist: its core lies in constructing a multifunctional block synergist containing fluorine chain ion blocks and reactive siloxane end groups, and combining it with a three-level particle size dense stacking model of 3-10μm / 20-40μm / 90-140μm, which simultaneously solves a series of pain points of traditional solutions - by bridging the three-dimensional interface through the synergist, the thermal conductivity is improved and the interface thermal resistance is effectively reduced; with the synergistic effect of the three-level particle size and the synergist, the filling amount is increased, and the problem of deterioration of fluidity caused by high filling is improved; the siloxane end groups are used to participate in cross-linking to enhance interface bonding, thereby improving tensile strength and alleviating the degradation of mechanical properties; the hydrophobic coating of the fluorine chain blocks the adsorption of water molecules, thereby increasing the breakdown voltage and improving electrical insulation; at the same time, the high-density stacking of alumina forms a ceramic barrier to achieve a high flame retardant grade.

[0038] The present invention achieves synergistic gains in thermal conductivity, insulation, and flexibility, and can meet the needs of multiple fields such as power battery pack heat dissipation gaskets, high-frequency circuit packaging, and wearable devices. The process is compatible with industrial production, and the chemically bonded interface can ensure long life. Its dual innovations of molecular-level interface design and micro-nanoscale stacking optimization provide strong support for the commercial application of next-generation thermal management materials in new energy, consumer electronics, and aerospace fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a synthetic route for amphiphilic fluorosilicone thermal conductive interface synergist;

[0040] Figure 2 Infrared spectra of PMAA-PDMA-PFPE zwitterionic block copolymer, cyclosiloxane graft copolymer 1, and amphiphilic fluorosilicone thermal conductive interface enhancer 1. DETAILED DESCRIPTION

[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention.

[0042] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0043] The raw materials and equipment used in the embodiments and comparative examples are described below:

[0044] Perfluoropolyether methacrylate: homemade, the preparation method is as follows:

[0045] 1 eq of perfluoropolyether alcohol was mixed with 1.2-1.3 eq of triethylamine previously dehydrated with calcium hydride in dichloromethane, and the mixture was cooled to 0°C in an ice bath. 1.2-1.3 eq of a dichloromethane solution of methacryloyl chloride was slowly added dropwise. After 30 minutes of complete addition, the mixture was allowed to react at the same temperature for 2-3 hours, then the mixture was allowed to warm to room temperature and the reaction was continued for 10-12 hours. The mixture was filtered and subjected to silica gel column chromatography to obtain the product, perfluoropolyether methacrylate.

[0046] PMAA-PDMA zwitterionic block copolymer: homemade, the preparation method is as follows:

[0047] 1eq methacrylic acid, 0.02eq RAFT agent, 0.004eq initiator, 3A molecular sieve and deionized water were added to a 50mL two-necked flask, the mixture was deoxygenated by nitrogen bubbling for 20-30min, and reacted at 70°C for 3-4h to obtain PMAA block; in a sealed bottle protected by nitrogen, 1eq dimethylaminoethyl methacrylate, 0.0067eq RAFT agent, 1.0eq sodium hydroxide and 5.53g deionized water were mixed and deoxygenated for 30-40min, and then the mixture was injected into the PMAA reaction system under nitrogen atmosphere, reacted at 65-75°C for 9-10h, and the final solution pH was 8-9 to obtain PMAA-PDMA zwitterionic block copolymer;

[0048] PMAA-PDMA-PFPE zwitterionic block copolymer: homemade. The preparation method is different from that of PMAA-PDMA zwitterionic block copolymer. The difference is that after obtaining PMAA-PDMA zwitterionic block copolymer, the following operations are also performed:

[0049] The reaction system was cooled to 40-45°C, water was removed by distillation under reduced pressure, 20 mL of hexafluoroisopropanol and 3A molecular sieves were added, the polymer was dissolved by stirring, and 0.5 eq of triethylamine was added until the pH was 7 to neutralize the residual carboxylic acid; in a sealed bottle protected by nitrogen, 1 eq of perfluoropolyether methacrylate, 0.002 eq of V-70 and 10 mL of hexafluoroisopropanol were mixed, and after ultrasonic deoxygenation for 10-15 minutes, the mixture was injected into the main reaction system and reacted at 60-65°C in the dark for 12-16 hours; after the reaction, liquid nitrogen was quenched, the reaction was terminated by air, and a mixed solution of cold ether and n-hexane in a volume ratio of 1:1 was added dropwise, the precipitate was collected by centrifugation, and the precipitate was repeatedly dissolved in hexafluoroisopropanol and cold ether three times, and vacuum dried at 35-45°C for 20-24 hours to obtain PMAA-PDMA-PFPE zwitterionic block copolymer;

[0050] Dimethylsiloxane oligomer catalyst: homemade, preparation method is as follows:

[0051] 1.0 eq of tetramethylammonium hydroxide and 1.1-1.2 eq of octamethylcyclotetrasiloxane were added to a 250 mL three-necked flask, and 4.0 eq of cyclohexane was added. The mixture was stirred at 80°C for 24 h under nitrogen protection. Crystallization water and condensation water were monitored and removed in real time using a Dean-Stark water trap. After the reaction, nitrogen was bubbled at 85°C for 1 h to remove residual cyclohexane, thereby obtaining a dimethylsiloxane oligomer catalyst.

[0052] Double modified spherical alumina 3-10μm / 20-40μm / 90-140μm: homemade, preparation method is as follows:

[0053] The spherical alumina with a size of 3 to 10 μm, 20 to 40 μm, and 90 to 140 μm is baked to remove moisture, cooled, and sealed for later use; an isopropoxy distearate acyloxyaluminate solution with a mass fraction of 0.1% to 1% isopropoxy distearate acyloxyaluminate is prepared with anhydrous toluene; the baked spherical alumina with a size of 3 to 10 μm, 20 to 40 μm, and 90 to 140 μm is immersed in the prepared coupling agent solution by ultrasonication and stirring to disperse; the obtained soaked spherical alumina with a size of 3 to 10 μm, 20 to 40 μm, and 90 to 140 μm is filtered to obtain a dispersed and soaked coupling agent solution. The invention discloses a method for preparing a first modified spherical alumina with a size of 3 to 10 μm, a size of 20 to 40 μm, and a size of 90 to 140 μm by mixing a silane coupling agent powder and baking it to obtain a first modified spherical alumina with a size of 3 to 10 μm, a size of 20 to 40 μm, and a size of 90 to 140 μm; a silane coupling agent solution with a mass fraction of 0.1% to 1% is prepared with ethanol; the first modified spherical alumina with a size of 3 to 10 μm, a size of 20 to 40 μm, and a size of 90 to 140 μm is immersed in the silane coupling agent solution, ultrasonicated, and stirred for dispersion; the second immersed spherical alumina powder is filtered and baked to obtain a double modified spherical alumina with a size of 3 to 10 μm, a size of 20 to 40 μm, and a size of 90 to 140 μm;

[0054] Platinum catalyst: 3000 ppm, purchased from Dongguan Maiteng Rubber and Plastic Materials Co., Ltd.;

[0055] Silane coupling agent: 3-aminopropyltriethoxysilane, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0056] Vinyl silicone oil: vinyl content 0.63%, commercially available;

[0057] Side hydrogenated silicone oil: hydrogen content 0.36wt%, commercially available;

[0058] End-hydrogenated silicone oil: hydrogen content 0.18wt%, commercially available;

[0059] Inhibitor: 1-ethynylcyclohexanol, purchased from Wuhan Kemik Biopharmaceutical Technology Co., Ltd.;

[0060] RAFT agent: 4-cyano-4-[(2-phenylethyl)thio]thioxomethyl]thio]-pentanoic acid, commercially available;

[0061] Initiator: 4,4'-azobis(4-cyanovaleric acid), commercially available;

[0062] Condensation agent: N,N'-diisopropylcarbodiimide, commercially available;

[0063] Catalyst: 4-dimethylaminopyridine, commercially available;

[0064] Enol: Propylene alcohol, commercially available;

[0065] Perfluoropolyether alcohol: purchased from Suzhou Cangmu New Materials Co., Ltd.

[0066] Methacryloyl chloride: Product No. M109517, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0067] 1,3,5,7-Tetramethylcyclotetrasiloxane: purchased from Hubei Xinliheng Chemical Co., Ltd.

[0068] Karstedt platinum catalyst: platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane, 20 ppm Pt, commercially available;

[0069] Preparation Example

[0070] Preparation Example 1

[0071] Amphiphilic fluorosilicone thermal conductive interface enhancer 1: Homemade, preparation method is as follows:

[0072] (1) Take 1eq of PMAA-PDMA-PFPE zwitterionic block copolymer, add anhydrous hexafluoroisopropanol to dissolve, then add 3A molecular sieves, and remove water by nitrogen bubbling for 20-30 min; cool to 0°C in an ice bath, add 1.2eq of condensing agent and 0.1eq of catalyst in sequence; slowly add 1.5eq of hexafluoroisopropanol solution of enol, heat to 30°C, stir in the dark for 20-24h, and use 30W low-frequency ultrasound to assist diffusion; after the reaction is completed, filter, add 10 times the volume of -20°C n-pentane to the reaction solution, and collect the precipitate by centrifugation; dissolve the precipitate in tetrahydrofuran and dialyze it for 4 minutes with a mixed solution of THF and water with a volume ratio of 1:1. 0 to 48 hours, and vacuum drying to obtain an olefinic zwitterionic block copolymer; dissolving 1 eq of the above olefinic zwitterionic block copolymer in 450 eq of deionized water to prepare an aqueous solution with a mass fraction of 0.5%, taking 1 eq of hydrazine hydrate and 30 eq of deionized water to prepare a hydrazine hydrate solution, adding the hydrazine hydrate solution to the olefinic zwitterionic block copolymer solution, controlling the temperature at 20 to 25° C., adjusting the pH to 8.5 to 9.5, standing for 10 to 20 minutes to precipitate, decanting the supernatant, washing the precipitate three times with deionized water at pH = 6, and vacuum drying to obtain an olefinic zwitterionic block copolymer 1 with trithiocarbonate end groups removed;

[0073] (2) 1 eq of the product from the previous step was dissolved in toluene, and 0.25 eq to 1 eq of 1,3,5,7-tetramethylcyclotetrasiloxane and Karstedt platinum catalyst were added under a nitrogen atmosphere, and the mixture was refluxed at 100-110° C. for 20-24 h. The reaction solution was adsorbed on activated carbon for 10-12 h, filtered, and the filtrate was concentrated by rotary evaporation and vacuum dried at 80-85° C. overnight to obtain a cyclosiloxane graft copolymer 1.

[0074] (3) 1 eq of cyclosiloxane graft copolymer 1 and 0.4-0.5 eq of tetramethylcyclotetrasiloxane were added to the reaction flask, and oxygen was removed by repeated nitrogen replacement and vacuum extraction. The temperature was raised to 85°C under nitrogen protection, and 0.01 eq of TMAS catalyst tetrahydrofuran solution was injected with a pipette, and the polymerization was vigorously stirred at 100-105°C for 20-24 hours; then the temperature was raised to 130-140°C to decompose the residual catalyst, and then nitrogen was bubbled at 160-170°C to remove low molecular weight by-products; the crude product was dissolved in dichloromethane, purified by precipitation with 6 times the volume of methanol, and vacuum dried at 80°C for 2 hours to obtain a brown solid; the solid was placed in a preheated mold, melted at 70-75°C for 15-25 minutes, and naturally cooled and demolded to obtain an amphiphilic fluorosilicone thermal conductive interface enhancer 1.

[0075] Preparation Example 2

[0076] Amphiphilic fluorosilicone thermal conductive interface synergist 2: Homemade. The preparation method is similar to that of amphiphilic fluorosilicone thermal conductive interface synergist 1. The difference is that the PMAA-PDMA-PFPE zwitterionic block copolymer is replaced by the PMAA-PDMA zwitterionic block copolymer. Other conditions remain unchanged, and amphiphilic fluorosilicone thermal conductive interface synergist 2 is obtained.

[0077] Example

[0078] Example 1

[0079] Spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface enhancer 1: homemade, preparation method is as follows:

[0080] The amphiphilic fluorosilicone thermal conductive interface enhancer 1 was prepared into a hexafluoroisopropanol solution with a mass fraction of 0.5-0.8%, 1.2eq of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.5eq of N-hydroxysuccinimide were added, and the solution was dissolved with ultrasound assistance. The temperature was raised to 45-50°C and activated for 10-15 minutes. 3A molecular sieve was added, and nitrogen was bubbled for 15-20 minutes. The treatment agent solution was filtered to obtain the treatment agent solution. The double-modified spherical alumina 3 was added. ~10μm is slowly added to the treatment agent solution, 0.1eq triethylamine is added to adjust the pH to 7.5-8.5, the temperature is maintained at 35-45°C, and the dispersion is carried out by ultrasonication and stirring; the obtained spherical alumina is filtered, purified by precipitation with cold ether and n-hexane, and Soxhlet extraction is performed for 40-48h with a mixed solution of methanol and chloroform in a volume ratio of 1:2 to remove small molecular impurities, and after vacuum drying, spherical alumina 3-10μm modified with amphiphilic fluorosilicone thermal conductive interface enhancer 1 is obtained;

[0081] Example 2

[0082] Spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1: homemade. The preparation method is compared with the spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1. The difference is that the double-modified spherical alumina 3-10 μm is replaced by double-modified spherical alumina 20-40 μm. Other conditions remain unchanged, and spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is obtained.

[0083] Example 3

[0084] Spherical alumina 90-140 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1: homemade. The preparation method is compared with the spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1. The difference is that the double-modified spherical alumina 3-10 μm is replaced by double-modified spherical alumina 90-140 μm. Other conditions remain unchanged, and the spherical alumina 90-140 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is obtained.

[0085] Example 4

[0086] Spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 2: homemade. The preparation method is similar to that of spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1. The difference is that amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by amphiphilic fluorosilicone thermal conductive interface synergist 2, and other conditions remain unchanged, resulting in spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 2.

[0087] Example 5

[0088] Spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 2: homemade. The preparation method is similar to that of spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1. The difference is that amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by amphiphilic fluorosilicone thermal conductive interface synergist 2, and other conditions remain unchanged, resulting in spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 2.

[0089] Example 6

[0090] Spherical alumina 90-140 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 2: homemade. The preparation method is similar to that of spherical alumina 90-140 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1. The difference is that amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by amphiphilic fluorosilicone thermal conductive interface synergist 2, and other conditions remain unchanged, resulting in spherical alumina 90-140 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 2.

[0091] Application Examples

[0092] Application Example 1

[0093] Silicone rubber thermal conductive composite material 1: Homemade, preparation method is as follows:

[0094] S1. Weigh the raw materials according to the mixing ratio;

[0095] S2. In the preparation container, 150 parts of vinyl silicone oil, 0.05 parts of inhibitor, and 1.1 parts of platinum catalyst were stirred;

[0096] S3 was added to the container 3.5 parts of side hydrogen silicone oil, 3.5 parts of end hydrogen silicone oil and stirred;

[0097] S4. Add 578 parts of spherical alumina 3-10 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1, 1391 parts of spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1, and 2283 parts of spherical alumina 90-140 μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 in batches to step S4, mix, and evacuate to a vacuum degree of ≤10 kPa to obtain a uniformly mixed thermal conductive base material;

[0098] S5. Place the thermally conductive base material 1 between two fluoroplastic films, press the sheet through a calender, and cure it in a 120°C vulcanization furnace to obtain a spherical alumina silicone rubber thermally conductive composite material 1.

[0099] Application Example 2

[0100] Spherical alumina silicone rubber thermal conductive composite material 2: homemade, the preparation method is compared with the spherical alumina silicone rubber thermal conductive composite material 1, the difference is that the addition amount of spherical alumina 3-10μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by 157 parts, the addition amount of spherical alumina 20-40μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by 782 parts, the addition amount of spherical alumina 90-140μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by 1563 parts, the addition amount of vinyl silicone oil is replaced by 100 parts, the addition amount of side hydrogen-containing silicone oil is replaced by 1 part, the addition amount of end hydrogen-containing silicone oil is replaced by 1 part, the addition amount of platinum catalyst is replaced by 0.2 parts, the addition amount of inhibitor is replaced by 0.01 parts, and other conditions remain unchanged to obtain spherical alumina silicone rubber thermal conductive composite material 2.

[0101] Application Example 3

[0102] Spherical alumina silicone rubber thermal conductive composite material 3: homemade, the preparation method is compared with the spherical alumina silicone rubber thermal conductive composite material 1, the difference is that the addition amount of spherical alumina 3-10μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by 1000 parts, the addition amount of spherical alumina 20-40μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by 2000 parts, the addition amount of spherical alumina 90-140μm modified by amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by 3000 parts, the addition amount of vinyl silicone oil is replaced by 200 parts, the addition amount of side hydrogen-containing silicone oil is replaced by 6 parts, the addition amount of end hydrogen-containing silicone oil is replaced by 6 parts, the addition amount of platinum catalyst is replaced by 2 parts, the addition amount of inhibitor is replaced by 0.1 part, and other conditions remain unchanged to obtain spherical alumina silicone rubber thermal conductive composite material 3.

[0103] Application Example 4

[0104] Spherical alumina silicone rubber thermal conductive composite material 4; homemade, the preparation method is compared with the spherical alumina silicone rubber thermal conductive composite material 1, the difference is that the added amphiphilic fluorosilicone thermal conductive interface synergist 1 is replaced by amphiphilic fluorosilicone thermal conductive interface synergist 2, and other conditions remain unchanged to obtain spherical alumina silicone rubber thermal conductive composite material 4.

[0105] Comparative Example 1

[0106] Spherical alumina silicone rubber thermal conductive composite material 5: homemade. The preparation method is different from that of spherical alumina silicone rubber thermal conductive composite material 1. The difference is that the spherical alumina is not modified with amphiphilic fluorosilicone thermal conductive interface enhancer, and double-modified spherical alumina is directly used. Other conditions remain unchanged to obtain spherical alumina silicone rubber thermal conductive composite material 5.

[0107] Comparative Example 2

[0108] Spherical alumina silicone rubber thermal conductive composite material 6: homemade. The preparation method is compared with the spherical alumina silicone rubber thermal conductive composite material 1. The difference is that only 4250 parts of spherical alumina 20-40 μm modified by amphiphilic fluorosilicone thermal conductive interface enhancer 1 are added, and 3-10 μm and 90-140 μm are not added. Other conditions remain unchanged, and spherical alumina silicone rubber thermal conductive composite material 6 is obtained.

[0109] Table 1 Formulations of Application Examples 1 to 4 and Comparative Examples 1 to 2 (by weight)

[0110]

[0111]

[0112] The following are the test methods for the performance parameters involved in the present invention:

[0113] 1. Fourier transform infrared spectroscopy (FTIR): Spectrum two, PerkinElmer, USA; at 1015 cm -1 Si-O-Si peaks were observed at 1060 cm-1 and 1060 cm-1. Compared with the cyclosiloxane graft copolymer 1, the Si-O-Si absorption peak of the amphiphilic fluorosilicone thermal conductive interface synergist 1 is broader and shows a double peak. This characteristic double peak of linear polysilane proves the successful synthesis of the amphiphilic fluorosilicone thermal conductive interface synergist 1.

[0114] 2. Thermal conductivity test: Tested according to ASTM D5470 standard, the instrument is DRL-3 thermal conductivity tester, unit: W / (mk);

[0115] 3. Shore hardness test: Tested according to ASTM D2240 standard, the instrument is Shore 00 durometer;

[0116] 4. Tensile strength test: Tested according to ASTM D412 standard, the instrument is a universal tensile testing machine, unit: psi;

[0117] 5. Breakdown voltage test: Tested according to ASTM D149 standard, the instrument is a withstand voltage tester, unit: kV / mm;

[0118] 6. The vertical combustion method is adopted according to UL 94 standard, and the instrument is a vertical combustion tester.

[0119] Table 2 Performance test results of application examples 1 to 4 and comparative examples 1 to 2

[0120] Application Example 1 Application Example 2 Application Example 3 Application Example 4 Comparative Example 1 Comparative Example 2 Thermal conductivity (W / mk) 13.97 12.22 14.88 9.15 6.01 7.80 Shore hardness (00) 76 68 81 70 64 63 Tensile strength (psi) 10.1 9.7 10.2 8.4 7.6 7.3 Breakdown voltage (kV / mm) 5.6 5.3 5.9 5.1 5.0 4.9 Flame retardant grade (UL94) V-0 V-0 V-0 V-0 V-1 V-1

[0121] As shown in Table 2, Examples 1-3 utilize a multi-grade particle size (3-10 μm / 20-40 μm / 90-140 μm) to achieve dense packing of fillers and effectively reduce voids. The amphiphilic block structure (PMAA-PDMA-PFPE) of synergist 1 plays a key role. Its fluorine chains are highly compatible with silicone oil, while its ionic chains anchor alumina, significantly reducing interfacial thermal resistance. Example 3, with a total filler content of 6,000 parts, further increases the density of the thermal conduction paths. In contrast, the low thermal conductivity results from various defects: Comparative Example 1 is not modified with a synergist, resulting in residual voids in the coupling agent and high interfacial thermal resistance. Comparative Example 2 uses a single-particle filler, which is prone to void formation and has low packing efficiency. Synergist 2 in Example 4 lacks PFPE fluorine chains, reducing its compatibility with silicone oil and also contributing to poor thermal conductivity.

[0122] In terms of mechanical properties, Examples 1 and 3 exhibit high strength and hardness. Example 3 further improves rigidity due to the high filler ratio. Comparative Example 1 is prone to stress concentration and fracture due to weak interfacial bonding. In terms of electrical insulation, Examples 1, 3, and 4 have the advantage of high-voltage breakdown. The core of this is that the dense interfacial layer formed by the synergist-coated alumina can effectively block charge migration, and the PFPE fluorine chain can enhance hydrophobicity and reduce the water vapor conductive path. Comparative Example 2 has more voids formed by the single-particle filler, which makes it easier to generate discharge channels and reduces the breakdown voltage.

[0123] The preferred embodiments of the present invention disclosed above are intended only to help illustrate the present invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the present invention to the specific embodiments described. Obviously, many modifications and variations are possible based on the content of this specification. These embodiments are selected and described in detail in this specification to better explain the principles and practical applications of the present invention, thereby enabling those skilled in the art to better understand and utilize the present invention. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A spherical alumina, characterized in that: The spherical alumina is surface-modified with an amphiphilic fluorosilicone thermal conductive interface synergist, and the structure of the amphiphilic fluorosilicone thermal conductive interface synergist is shown in Formula 1: Among them, a:b:c=(1~100):(1~100):(1~10), e:f=1:(1~4).

2. The spherical alumina according to claim 1, wherein In parts by weight, the spherical alumina includes 1 to 5 parts of spherical alumina with an average particle size of 3 to 10 μm, 5 to 10 parts of spherical alumina with an average particle size of 20 to 40 μm, and 10 to 15 parts of spherical alumina with an average particle size of 90 to 140 μm.

3. The spherical alumina according to claim 1, wherein The step of surface modification of the spherical alumina with an amphiphilic fluorosilicone thermal conductive interface synergist is as follows: (1) baking the spherical alumina to remove moisture, cooling and sealing for later use; (2) preparing a 0.1% to 1% by mass isopropoxy distearate acyloxyaluminate solution in anhydrous toluene; immersing the baked spherical alumina in the solution, ultrasonically dispersing, stirring, filtering, and drying to obtain a primary modified spherical alumina; (3) preparing a silane coupling agent solution with a mass fraction of 0.1% to 1% using ethanol; immersing the primary modified spherical alumina obtained in step (2) in the silane coupling agent solution, ultrasonically dispersing, stirring, filtering, and drying to obtain a double-modified spherical alumina; (4) The amphiphilic fluorosilicone thermal conductive interface enhancer is prepared into a hexafluoroisopropanol solution with a mass fraction of 0.5-0.8%, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide are added, ultrasonic-assisted dissolution is carried out, the temperature is raised to 45-50°C for activation, and the treatment agent solution is obtained after dehydration and deoxygenation; the double-modified spherical alumina obtained in step (3) is slowly added to the treatment agent solution, triethylamine is added to adjust the pH to 7.5-8.5, the temperature is maintained at 35-45°C, ultrasonically dispersed by stirring, filtered, purified by precipitation with cold ether and n-hexane, and Soxhlet extracted with a mixed solution of methanol and chloroform in a volume ratio of 1:2 for 40-48 hours to remove small molecular impurities, and vacuum dried to obtain spherical alumina with amphiphilic fluorosilicone thermal conductive interface enhancer.

4. A silicone rubber thermally conductive composite material, characterized in that: The raw materials include, by weight: 100-200 parts of vinyl silicone oil, 1-6 parts of side hydrogen-containing silicone oil, 1-6 parts of end hydrogen-containing silicone oil, 0.2-2 parts of platinum catalyst, 0.01-0.1 parts of inhibitor, and 2500-6000 parts of spherical alumina as described in any one of claims 1 to 3.

5. The thermally conductive silicone rubber composite material according to claim 4, wherein: The vinyl content of the vinyl silicone oil is 0.21% to 1.4wt%.

6. The thermally conductive silicone rubber composite material according to claim 4, wherein: The hydrogen content of the side hydrogenated silicone oil is 0.05% to 1.2 wt%.

7. The thermally conductive silicone rubber composite material according to claim 4, wherein: The hydrogen content of the hydrogen-terminated silicone oil is 0.05% to 1.0 wt%.

8. The thermally conductive silicone rubber composite material according to claim 4, wherein: The inhibitor is one or more of 3-methyl-1-butyn-3-ol, 1-ethynylcyclohexanol, 3-propyl-1-butyn-3-ol, and 3-octyl-1-butyn-3-ol.

9. The thermally conductive silicone rubber composite material according to claim 4, wherein: The platinum catalyst is a platinum compound or complex with a platinum content of 1000 to 5000 ppm.

10. The method for preparing the silicone rubber thermally conductive composite material according to any one of claims 4 to 9, wherein: The following steps are involved: S1. Weigh the raw materials in parts by weight and stir the vinyl silicone oil, inhibitor, and platinum catalyst in a preparation container; S2. Add hydrogen silicone oil to the container and stir evenly at the end; S3. Amphiphilic fluorine-silicone thermally conductive interface enhancing spherical alumina powder was added to step S2 in batches and mixed, and evacuated to a vacuum degree of ≤10 kPa to obtain a uniformly mixed thermally conductive base material; S4. Place the thermally conductive base material between two fluoroplastic films, press the sheet through a calender, and cure it in a vulcanization furnace to obtain a spherical alumina silicone rubber thermally conductive composite material.

Citation Information

Patent Citations

  • Fluorine silicon tri-block copolymers and preparation method thereof

    CN101215364A

  • Insulating high-thermal-conductivity flexible silica gel gasket and preparation method thereof

    CN114752221A

  • Water-repellent and oil-repellent fabric finishing agent, finishing agent stock solution and preparation method of finishing agent stock solution

    CN115368575A

  • Spherical barium titanate / spherical aluminum oxide / silicone rubber heat-conducting and wave-absorbing composite material and preparation method thereof

    CN115449224A

  • Photochromic polydiorganosiloxane ethylene crosslinking agents

    CN115605529A

Cited By

  • High-temperature-resistant fluorine modified estersil and preparation method thereof

    CN121022116A

  • Spherical aluminum nitride silicone grease high-thermal-conductivity interface material composition

    CN121182215A

  • A spherical aluminum nitride silicon grease high thermal conductive interface material composition

    CN121182215B

  • High-purity spherical zinc oxide-silicon dioxide synergistic photocatalytic air purification material

    CN121266630A

  • High-purity spherical zinc oxide-silica synergistic photocatalytic air purification material

    CN121266630B