Porous negative electrode material, preparation method thereof, negative electrode sheet, secondary battery, and electric device
By employing porous anode materials in lithium-ion batteries, the volume expansion problem of graphite anodes is solved by utilizing the internal network porous hard carbon structure, maintaining high specific capacity and coulombic efficiency, improving energy density and reducing cost.
Patent Information
- Application Number
- CN202410281490.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-11
AI Technical Summary
How to improve the volume expansion problem of lithium-ion battery anodes without reducing the capacity of graphite, especially the volume expansion and SEI film thickening caused by lithium ion intercalation during charging, which leads to particle breakage and capacity decay.
The anode material is porous. It is formed by porous hard carbon with a network structure inside the secondary particles. The porosity is 15%-28%. The internal pore structure cannot contact the electrolyte, thus avoiding the formation of SEI film. The hard carbon precursor is mixed with carbon-based materials and pyrolyzed to form a porous structure, maintaining high coulombic efficiency and specific capacity.
It effectively alleviates the volume expansion of graphite anodes, maintains high specific capacity and high coulombic efficiency, while improving energy density and reducing active lithium loss and material costs.
Smart Images

Figure CN120637385B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium-ion battery technology, and in particular to a porous negative electrode material and its preparation method, a negative electrode sheet, a secondary battery, and an electrical device. Background Technology
[0002] The statements herein are provided only as background information in connection with this application and do not necessarily constitute prior art.
[0003] In recent years, with the increasingly wide application of lithium-ion batteries, they have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace.
[0004] During lithium-ion battery charging, the graphite anode inevitably expands in volume due to lithium-ion intercalation. During cycling, this repeated volume expansion causes the SEI film to thicken continuously, while also increasing stress within the anode material particles, ultimately leading to particle breakage and capacity decay. Reducing the degree of graphitization, thus decreasing the proportion of graphite participating in the lithium intercalation reaction, is an effective way to mitigate volume expansion; however, this also negatively impacts lithium intercalation capability and reduces specific capacity.
[0005] Therefore, how to improve the volume expansion of carbon-based anodes without reducing the specific capacity of carbon-based materials is a key issue facing lithium-ion batteries. Summary of the Invention
[0006] This application provides a porous anode material that can improve the volume expansion of graphite anodes while taking into account the specific capacity of graphite, as well as its preparation method, anode sheet, secondary battery, and power device.
[0007] To achieve the above objectives, a first aspect of this application provides a porous negative electrode material comprising secondary particles having an internal pore structure, the secondary particles comprising a plurality of primary particles, the primary particles comprising a carbon-based material, and porous hard carbon filling the spaces between adjacent primary particles, the porous hard carbon comprising the secondary particles forming a network structure, and the porosity of the porous negative electrode material being 15%-28%.
[0008] Therefore, the porous anode material in this application includes secondary particles with an internal pore structure. The porous hard carbon filling the spaces between the multiple primary particles forms a network structure, and the porosity of the porous anode material is 15%-28%. Thus, the porous and loose hard carbon structure within the porous anode material not only provides a buffer zone for the volume expansion of the carbon-based material, helping to stabilize the internal and surface structure of the particles, but also does not affect the specific capacity of the anode material. Furthermore, the internal pore structure of the porous anode material cannot directly contact the electrolyte, thus preventing the loss of active lithium due to the formation of an SEI film, thereby reducing the loss of coulombic efficiency and specific capacity. In addition, the reduced specific surface area of the porous anode material including secondary particles is beneficial for improving its coulombic efficiency. Simultaneously, because the secondary particles are more compact, their compaction density is significantly higher than that of the primary particles, thereby increasing the energy density of the material.
[0009] In some embodiments of this application, the porosity of the porous negative material is 18%-27%.
[0010] In some embodiments of this application, the average pore size of the internal pore structure contained in the porous negative electrode material is 2.8 nm-5.2 nm, and can be optionally 3.0 nm-4.5 nm.
[0011] In some embodiments of this application, the porous negative electrode material contains internal pore structures including micropores with a pore size of less than 2 nm, mesopores with a pore size of 2 nm-50 nm, and macropores with a pore size of greater than 50 nm.
[0012] Optionally, the number of micropores in the internal pore structure accounts for 55%-70%, and optionally 58%-68%;
[0013] Optionally, the mesopores account for 20%-35% of the total number of the internal pore structure, and optionally 22%-32%.
[0014] Optionally, the number of large holes in the internal hole structure accounts for 3%-10%, and optionally 4%-8%.
[0015] In some embodiments of this application, the porous negative electrode material contains an internal pore volume of 0.05 cm³. 3 / g-0.35cm 3 / g, can be selected as 0.08cm 3 / g-0.32cm 3 / g.
[0016] In some embodiments of this application, the volume average particle size Dv50 of the porous negative electrode material is 15μm-25μm, and can be selected as 16μm-24μm.
[0017] In some embodiments of this application, the mass ratio of the porous hard carbon to the carbon-based material contained in the porous negative electrode material is 1:(5-50), and can be optionally 1:(20-35).
[0018] In some embodiments of this application, the carbon-based material includes one or more of artificial graphite, natural graphite, hard carbon, and soft carbon; optionally, the carbon-based material includes artificial graphite.
[0019] The second aspect of this application provides a method for preparing the porous negative electrode material of the first aspect of this application, comprising the following steps:
[0020] A mixture of carbon-based material precursors and hard carbon precursors is prepared by crushing the mixture.
[0021] The mixture is subjected to pyrolysis and granulation to prepare an intermediate.
[0022] The intermediate is post-processed to prepare the porous anode material.
[0023] Therefore, this application mixes a carbon-based material precursor with a hard carbon precursor, followed by crushing and pyrolysis granulation. The hard carbon precursor adheres to the surface of the carbon-based material precursor particles, aggregating smaller primary particles to form secondary particles. During pyrolysis granulation and subsequent heat treatment, the hard carbon precursor is converted into hard carbon, and the released gas forms porous hard carbon. This preparation method does not increase the specific surface area of the particles, thus avoiding the increase in active sites that would lead to a decrease in coulombic efficiency and an increase in lithium consumption. The resulting porous anode material with an internal porous structure alleviates volume expansion while maintaining specific capacity, and simultaneously possesses high compaction density, high energy density, and high coulombic efficiency. Furthermore, this preparation method does not require improvement of the formed carbon-based material; only the processing of the carbon-based material is improved, directly obtaining an anode material with an internal porous structure, significantly reducing costs.
[0024] In some embodiments of this application, the hard carbon precursor includes one or more of resins, organic polymers, biomass, and carbohydrates;
[0025] Optionally, the resin includes one or more of phenolic resin, epoxy resin, and polyfurfuryl alcohol resin;
[0026] Optionally, the organic polymer includes one or more of polyacrylonitrile, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl chloride, polyvinylidene fluoride, and bitumen;
[0027] Optionally, the biomass includes one or more of cellulose and lignin;
[0028] Optionally, the carbohydrate includes one or more of sucrose and glucose.
[0029] In some embodiments of this application, a pulverizer is used for the crushing process;
[0030] Optionally, the rotation speed of the pulverizer is 10,000 rpm to 25,000 rpm, and can be selected as 12,000 rpm to 25,000 rpm;
[0031] Optionally, the crushing process takes 5-10 minutes, or 8-10 minutes.
[0032] In some embodiments of this application, the mass ratio of the hard carbon precursor to the carbon-based material precursor is 1:(5-50), and optionally 1:(20-35).
[0033] In some embodiments of this application, the carbon-based material precursor includes one or more of activated carbon, coke, carbon black, charcoal, bio-coke, and coal coke.
[0034] In some embodiments of this application, the post-processing includes graphitization;
[0035] Optionally, the graphitization temperature is 2000℃-3300℃, and optionally 2500℃-3200℃;
[0036] Optionally, the graphitization time is 300h-800h, or optionally 500h-800h.
[0037] In some embodiments of this application, the post-processing includes carbonization.
[0038] Optionally, the carbonization temperature is 1500℃-2000℃;
[0039] Optionally, the carbonization process takes 15-40 hours.
[0040] In some embodiments of this application, the carbon-based material includes one or more of flake graphite and microcrystalline graphite.
[0041] In some embodiments of this application, the post-processing includes spheroidization.
[0042] Optionally, the rotational speed of the spheroidizing process is 2000 rpm to 8000 rpm;
[0043] Optionally, the spheroidization process takes 5-15 minutes.
[0044] Optionally, the spheroidizing process may be performed using at least one of air jet milling and mechanical milling.
[0045] In some embodiments of this application, the carbon-based material includes one or more of bitumen, paraffin wax, biomass, biomass extracts, and artificial organic polymers.
[0046] In some embodiments of this application, the post-processing includes carbonization.
[0047] Optionally, the carbonization temperature is 800℃-1600℃;
[0048] Optionally, the carbonization process takes 2-15 hours.
[0049] In some embodiments of this application, the pyrolysis granulation temperature is 600℃-1600℃, optionally 800℃-1200℃; and / or
[0050] The pyrolysis granulation time is 0.5h-6h, and can be selected as 2h-5h.
[0051] A third aspect of this application provides a negative electrode sheet, comprising:
[0052] Negative electrode current collector; and
[0053] A negative electrode active material layer is located on at least one side of the negative electrode current collector. The negative electrode active material layer comprises the porous negative electrode material of the first aspect of this application or the porous negative electrode material prepared by the preparation method of the second aspect of this application.
[0054] In some embodiments of this application, the compaction density of the negative electrode sheet is 1.4 g / cm³. 3 -1.65g / cm 3 .
[0055] In some embodiments of this application, the negative electrode active material layer further includes a conductive agent, a dispersant, and a binder;
[0056] Optionally, the conductive agent includes one or more of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene, and carbon nanotubes.
[0057] Optionally, the dispersant includes one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, sodium dodecyl sulfate, methylpentanol, cellulose derivatives, polyacrylamide, and polyvinylpyrrolidone;
[0058] Optionally, the adhesive includes one or more of polyimide resin, acrylic resin, polyvinylidene fluoride, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene rubber;
[0059] Optionally, the porous anode material accounts for 95.5%-97% of the mass of the anode active material layer;
[0060] Optionally, the conductive agent accounts for 0.8%-1.2% of the mass of the negative electrode active material layer;
[0061] Optionally, the dispersant accounts for 0.5%-1% of the mass of the negative electrode active material layer;
[0062] Optionally, the binder accounts for 1.2%-1.8% of the mass of the negative electrode active material layer.
[0063] The fourth aspect of this application provides a secondary battery, including the negative electrode sheet of the third aspect of this application.
[0064] A fifth aspect of this application provides an electrical device comprising a secondary battery according to a fourth aspect of this application. The secondary battery of this application comprises the porous negative electrode material of this application, exhibiting excellent coulombic efficiency and specific capacity, and high energy density.
[0065] The electrical device of this application includes the secondary battery provided in this application, and therefore has at least the same advantages as the secondary battery.
[0066] Details of one or more embodiments of this application are set forth in the following drawings and description. Other features, objects, and advantages of this application will become apparent from the specification, drawings, and claims. Attached Figure Description
[0067] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:
[0068] Figure 1 This is a schematic diagram of the structure of a porous negative electrode material according to an embodiment of this application.
[0069] Figure 2 This is a schematic diagram of a battery cell according to one embodiment of this application.
[0070] Figure 3 for Figure 2 An exploded view of a battery cell according to one embodiment of this application is shown.
[0071] Figure 4 This is a schematic diagram of a battery module according to one embodiment of this application.
[0072] Figure 5 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0073] Figure 6 for Figure 5 An exploded view of a battery pack according to one embodiment of this application is shown.
[0074] Figure 7 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to an embodiment of this application.
[0075] Explanation of reference numerals in the attached figures:
[0076] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate; 6 Electrical device. Detailed Implementation
[0077] The following describes in detail, with appropriate reference to the accompanying drawings, some embodiments of the porous negative electrode material, its preparation method, negative electrode sheet, secondary battery, and power application device of this application. However, some unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0078] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values 1 and 2 are listed, and maximum range values 3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0079] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.
[0080] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0081] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.
[0082] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0083] In this application, open-ended technical features or solutions described using terms such as "containing," "comprising," or "including" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, if A includes a1, a2, and a3, it may also include other members or exclude additional members unless otherwise specified. This can be considered as providing both the feature or solution that "A consists of a1, a2, and a3" and the feature or solution that "A includes not only a1, a2, and a3, but also other members." In this application, unless otherwise specified, A (e.g., B) indicates that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0084] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.
[0085] How to reduce the volume expansion of graphite anodes without decreasing their specific capacity is a key challenge currently facing lithium-ion batteries. Pore-forming treatment of graphite is an effective method to reduce its volume expansion. While creating pores on the surface of graphite particles increases porosity and specific surface area, when used as a lithium-ion battery anode material, this porous surface provides too many active sites, consuming more active lithium, leading to a decrease in coulombic efficiency and an increase in the thickness of the SEI film.
[0086] Creating pores inside graphite particles not only provides a buffer zone for the volume expansion of graphite, helping to stabilize the internal and surface structure of the particles, but also prevents the internal pore structure from directly contacting the electrolyte, thus preventing the formation of an SEI film and the loss of active lithium.
[0087] Based on this, this application improves the pretreatment step in the preparation process of carbon-based materials by adding a hard carbon precursor in the pretreatment step. The hard carbon precursor binds the primary carbon-based material precursor particles into secondary particles. During the pyrolysis granulation process, the hard carbon precursor is carbonized into a hard carbon structure at high temperature. The released gas gives the hard carbon a porous structure, and finally a porous anode material with an internal pore structure is prepared. The porous anode material has a high degree of graphitization, which can alleviate the volume expansion of carbon-based materials while taking into account the specific capacity. It also has high compaction density, high energy density and high coulombic efficiency.
[0088] The first aspect of this application provides a porous negative electrode material, which includes secondary particles with an internal pore structure, the secondary particles comprising a plurality of primary particles, the primary particles comprising a carbon-based material, the spaces between adjacent primary particles being filled with porous hard carbon, the porous hard carbon contained in the secondary particles forming a network structure, and the porosity of the porous negative electrode material being 15%-28%.
[0089] It should be noted that "internal pore structure" refers to the pore structure located inside the secondary particles and not extending to the surface of the secondary particles. The secondary particles of the porous anode material mentioned above only have pore structures located inside them, and the surface of the secondary particles does not have pore structures.
[0090] Understandably, the porous anode material in this application includes secondary particles with internal pore structures. The porous hard carbon filling the spaces between the multiple primary particles forming the secondary particles creates a network structure, and the porosity of the porous anode material is 15%-28%. Therefore, the porous and loose hard carbon structure within the porous anode material not only provides a buffer zone for the volume expansion of the carbon-based material, helping to stabilize the internal and surface structures of the particles, but also does not affect the specific capacity of the anode material. Furthermore, the internal pore structure of the porous anode material cannot directly contact the electrolyte, thus preventing the loss of active lithium due to the formation of an SEI film, thereby reducing the loss of coulombic efficiency and specific capacity. In addition, the reduced specific surface area of the porous anode material including secondary particles is beneficial for improving its coulombic efficiency. Simultaneously, because the secondary particles are more compact, their compaction density is significantly higher than that of the primary particles, thereby increasing the energy density of the material.
[0091] It should be noted that the voids between adjacent primary particles in the secondary particles can be partially filled by porous hard carbon, or they can be completely filled by porous hard carbon. For example, Figure 1 This is a structural schematic diagram of a porous negative electrode material provided in one embodiment of this application, with reference to... Figure 1 The gaps between adjacent primary particles (blue part in the figure) formed by carbon-based materials are completely filled by porous hard carbon (dark gray part), and the porous hard carbon contained in the secondary particles forms a network structure.
[0092] As an example, the porosity of porous anode materials can be, but is not limited to, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, or any two of the above values. When the porosity of the porous anode material is within the above range, it can effectively alleviate the volume expansion of carbon-based materials while also maintaining the coulombic efficiency of the porous anode material.
[0093] As one possible implementation, the porosity of the porous negative electrode material is 18%-27%.
[0094] As an example, the porosity of the aforementioned porous negative electrode material can be determined using mercury porosimetry. The specific method involves cutting the porous negative electrode material into small pieces, placing them in a sample container, using a glass cone probe as the sample container, applying pressure to the sample, and then measuring. The parameters of the mercury porosimeter are set as follows: approximately 0.6 to 50 PSI (corresponding to pore diameters from 355 to 4 micrometers) applied in the low-pressure station (LP), and approximately 20 to 60,000 PSI (corresponding to pore diameters from 10 to 0.004 micrometers) applied in the high-pressure station (HP). A PoreMaster 60GT mercury porosimeter from the USA can be used.
[0095] In some embodiments, the average pore size of the internal pore structure of the porous anode material is 2.8 nm to 5.2 nm; for example, it can be, but is not limited to, 2.8 nm, 3 nm, 3.2 nm, 3.4 nm, 3.6 nm, 3.8 nm, 4 nm, 4.2 nm, 4.4 nm, 4.6 nm, 4.8 nm, 5 nm, 5.2 nm, or any range between two of the above pore sizes. When the average pore size of the internal pore structure of the porous anode material is within the above range, it is beneficial to effectively alleviate the volume expansion of the carbon-based material and also beneficial to the stability of the particle structure of the porous anode material.
[0096] In some alternative embodiments, the porous anode material contains an internal pore structure with an average pore size of 3.0 nm to 4.5 nm.
[0097] In some alternative embodiments, the porous anode material contains internal pore structures including micropores with a pore size of less than 2 nm, mesopores with a pore size of 2 nm to 50 nm, and macropores with a pore size of more than 50 nm.
[0098] As one possible implementation, the proportion of micropores in the internal pore structure is 55%-70%; for example, it can be, but is not limited to, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, or any range between two of the above values. Optionally, the proportion of micropores in the internal pore structure is 58%-68%.
[0099] As one possible implementation, the proportion of mesopores in the internal pore structure is 20%-35%; for example, it can be, but is not limited to, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, or any range between two of the above values. Optionally, the proportion of mesopores in the internal pore structure is 22%-32%.
[0100] As one possible implementation, the number of macropores in the internal hole structure accounts for 3%-10%; for example, it can be, but is not limited to, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any range between two of the above values. Optionally, the number of macropores in the internal hole structure accounts for 4%-8%.
[0101] When the proportions of micropores, mesopores, and macropores in the internal pore structure of porous anode materials are within the above-mentioned ranges, it can alleviate the volume expansion of carbon-based materials while improving the mechanical strength of the secondary particles.
[0102] It should be noted that the pore size and the proportion of micropores, mesopores, and macropores in the internal pore structure of the porous anode material mentioned above can be determined using nitrogen adsorption curves. Specifically, the following method can be used:
[0103] The test sample is placed in a sample tube, first degassed by vacuum, and then the entire system is brought to the required vacuum level. The sample tube is then immersed in a liquid nitrogen bath and filled with a known amount of gas. The adsorbent adsorbs the gas, causing a pressure drop. After adsorption equilibrium is reached, the equilibrium pressure of the gas is measured, and the adsorption amount can be calculated based on the pressure change of the system before and after adsorption. The amount of adsorbate gas is gradually increased into the system to change the pressure, and the above operation is repeated to test the adsorption-desorption isotherms. Then, the pore size distribution of the test sample is equivalently determined using the Barrett-Joyner-Halenda model.
[0104] In some embodiments, the porous negative electrode material contains an internal pore volume of 0.05 cm³. 3 / g-0.35cm 3 / g; for example, it can be, but is not limited to, 0.05cm. 3 / g, 0.07cm 3 / g, 0.1cm 3 / g, 0.13cm 3 / g, 0.15cm 3 / g, 0.18cm 3 / g, 0.2cm 3 / g, 0.23cm 3 / g, 0.25cm 3 / g, 0.28cm 3 / g, 0.3cm 3 / g, 0.33cm 3 / g, 0.35cm 3 / g or any range between the two pore volumes mentioned above. When the pore volume of the internal pore structure is within the above range, it alleviates the volume expansion of the carbon-based material while benefiting the mechanical strength of the secondary particles. Optionally, the porous anode material contains an internal pore volume of 0.08 cm³. 3 / g-0.32cm 3 / g.
[0105] As an example, the pore volume of the aforementioned internal pore structure can be determined using nitrogen adsorption curves. Specifically, the following method can be used:
[0106] The test sample is placed in a sample tube, first degassed by vacuum, then the entire system is brought to the required vacuum level. The sample tube is then immersed in a liquid nitrogen bath and filled with a known amount of gas. The adsorbent adsorbs the gas, causing a pressure drop. After adsorption equilibrium is reached, the equilibrium pressure of the gas is measured, and the adsorption amount can be calculated based on the pressure change of the system before and after adsorption. The amount of adsorbate gas is gradually increased into the system to change the pressure, and the above operation is repeated to test the adsorption-desorption isotherms. Then, the pore volume of the test sample is equivalently calculated using the Barrett-Joyner-Halenda model.
[0107] In some embodiments, the volume average particle size Dv50 of the porous anode material is 15μm-25μm; for example, it can be, but is not limited to, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, or any range between two of the above particle sizes. Optionally, the volume average particle size Dv50 of the porous anode material is 16μm-24μm.
[0108] The Dv50 of a material has a well-known meaning in the art and can be tested using methods known in the art. For example, it can be determined using a laser particle size analyzer (such as the Malvern Master Size 3000) according to standard GB / T 19077-2016. The physical definitions of Dv50 are as follows:
[0109] Dv50: The particle size corresponding to a cumulative volumetric distribution percentage of 50% for the material.
[0110] In some embodiments, the mass ratio of porous hard carbon to carbon-based material in the porous anode material is 1:(5-50); for example, it can be, but is not limited to, 1:5, 1:7, 1:10, 1:13, 1:15, 1:18, 1:20, 1:23, 1:25, 1:28, 1:30, 1:33, 1:35, 1:38, 1:40, 1:43, 1:45, 1:48, 1:50, or any range between two of the above ratios. When the mass ratio of porous hard carbon to carbon-based material is within the above range, it is more conducive to the porous hard carbon playing an internal binding role, so that the final porous anode material has a suitable particle size. Optionally, the mass ratio of porous hard carbon to carbon-based material in the porous anode material is 1:(20-35).
[0111] As one possible implementation, carbon-based materials include one or more of artificial graphite, natural graphite, hard carbon, and soft carbon.
[0112] In some alternative implementations, the carbon-based material includes artificial graphite.
[0113] The second aspect of this application provides a method for preparing the porous anode material of the first aspect of this application, comprising the following steps: mixing a carbon-based material precursor and a hard carbon precursor and then crushing them to prepare a mixture; pyrolyzing and granulating the mixture to prepare an intermediate; and post-processing the intermediate to prepare the porous anode material.
[0114] The hard carbon precursor used in this application contains a large number of heteroatoms such as H, O, and N, which hinders the formation of crystallization regions during heat treatment, making it difficult to graphitize even at high temperatures above 2500℃. Therefore, the hard carbon precursor added in this application not only acts as a binder, but also aggregates the primary particles of the carbon-based material precursor into secondary particles at room temperature or high temperature. At the same time, the hard carbon precursor cannot be completely graphitized at ultra-high temperatures (above 2500℃), ultimately forming a hard carbon structure, and the released internal porous structure forms porous hard carbon.
[0115] The microstructure of porous hard carbon consists of short-range ordered microregions formed by the random, disordered stacking of curved graphene-like sheets, leaving numerous nanopores. Compared to graphite, porous hard carbon has shorter graphene layers, approximately 1 nm in diameter, which can be a single layer or formed by stacking two or three graphene layers to create the basic structure of the material. Compared to soft carbon (graphitizable carbon), porous hard carbon exhibits more disordered structure, higher defect concentration, higher heteroatom content, larger distances between graphene layers, and a more closed pore structure.
[0116] Understandably, this application involves mixing a carbon-based material precursor with a hard carbon precursor, followed by crushing and pyrolysis granulation. The hard carbon precursor adheres to the surface of the carbon-based material precursor particles, aggregating smaller primary particles to form secondary particles. During pyrolysis granulation and subsequent heat treatment, the hard carbon precursor transforms into hard carbon, and the released gas forms porous hard carbon. This preparation method does not increase the specific surface area of the particles, thus avoiding an increase in active sites that would lead to reduced coulombic efficiency and increased lithium consumption. The resulting porous anode material with an internal porous structure alleviates volume expansion while maintaining specific capacity, exhibiting high compaction density, high energy density, and high coulombic efficiency. Furthermore, this preparation method does not require improvement of the formed carbon-based material; only the processing of the carbon-based material is modified, directly obtaining an anode material with an internal porous structure, significantly reducing costs.
[0117] In some embodiments, the hard carbon precursor includes one or more of resins, organic polymers, biomass, and carbohydrates.
[0118] In some alternative embodiments, the resin includes one or more of phenolic resin, epoxy resin, and polyfurfuryl alcohol resin. As one possible embodiment, the organic polymer includes one or more of polyacrylonitrile, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl chloride, polyvinylidene fluoride, and bitumen.
[0119] In some exemplary embodiments, biomass includes one or more of cellulose and lignin. For example, biomass includes cellulose and lignin contained in plant residues and husks.
[0120] In some of these embodiments, the carbohydrates include one or more of sucrose and glucose.
[0121] In some embodiments, depending on the pyrolysis carbonization temperature, the hard carbon precursor includes high-temperature pyrolysis carbon with a pyrolysis carbonization temperature between 1000°C and 1400°C and low-temperature pyrolysis carbon with a pyrolysis carbonization temperature between 500°C and 1000°C.
[0122] As one possible implementation method, a pulverizer is used for crushing. Crushing helps to break down large particles, resulting in carbon-based material precursors and hard carbon precursors in a dry, fine powder form.
[0123] In some optional embodiments, the crusher operates at a speed of 10,000 rpm to 25,000 rpm during the crushing process; for example, it can be, but is not limited to, 10,000 rpm, 11,000 rpm, 12,000 rpm, 13,000 rpm, 14,000 rpm, 15,000 rpm, 16,000 rpm, 17,000 rpm, 18,000 rpm, 19,000 rpm, 20,000 rpm, 21,000 rpm, 22,000 rpm, 23,000 rpm, 24,000 rpm, 25,000 rpm, or any range between two of the above speeds. A crusher speed within the above range is more conducive to obtaining crushed particles of uniform and suitable size. Optionally, the crusher operates at a speed of 12,000 rpm to 25,000 rpm during the crushing process.
[0124] As one possible implementation, the crushing process takes 5-10 minutes; for example, it can be, but is not limited to, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, or any range between two of the above times. A crushing process within this range is more conducive to obtaining crushed particles of uniform and suitable size. Optionally, the crushing process takes 8-10 minutes.
[0125] In some embodiments, the carbon-based material precursor and the hard carbon precursor are mixed by stirring to ensure uniform mixing. As an example, the type of stirrer used can be, but is not limited to, turbine, paddle, propeller, screw, or planetary types. The stirring speed is 10 rpm to 300 rpm; for example, it can be, but is not limited to, 10 rpm, 30 rpm, 50 rpm, 70 rpm, 100 rpm, 130 rpm, 150 rpm, 180 rpm, 200 rpm, 230 rpm, 250 rpm, 280 rpm, 300 rpm, or any range between two of the above speeds. The stirring time is 0.25 h to 12 h; for example, it can be, but is not limited to, 0.25 h, 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, or any range between two of the above times.
[0126] In some embodiments, the mass ratio of hard carbon precursor to carbon-based material precursor is 1:(5-50); for example, it can be, but is not limited to, 1:5, 1:7, 1:10, 1:13, 1:15, 1:18, 1:20, 1:23, 1:25, 1:28, 1:30, 1:33, 1:35, 1:38, 1:40, 1:43, 1:45, 1:48, 1:50, or any range between two of the above ratios. When the mass ratio of hard carbon precursor to carbon-based material precursor is within the above range, it is more conducive to the porous hard carbon acting as an internal binder, so that the final porous anode material has a suitable particle size. Optionally, the mass ratio of hard carbon precursor to carbon-based material precursor is 1:(20-35).
[0127] As one possible implementation, the carbon-based material precursor includes one or more of activated carbon, coke, carbon black, charcoal, bio-coke, and coal coke. Accordingly, the carbon-based material in the resulting porous anode material is artificial graphite or soft carbon.
[0128] In some alternative embodiments, when the carbon-based material in the porous anode material is artificial graphite, the post-processing in the preparation of the porous anode material includes graphitization.
[0129] In some optional embodiments, the graphitization temperature is 2000℃-3300℃; for example, it can be, but is not limited to, 2000℃, 2100℃, 2200℃, 2300℃, 2400℃, 2500℃, 2600℃, 2700℃, 2800℃, 2900℃, 3000℃, 3100℃, 3200℃, 3300℃, or any range between two of the above temperatures. Optionally, the graphitization temperature is 2200℃-3200℃; further optionally, the graphitization temperature is 2500℃-3200℃; and even more optionally, the graphitization temperature is 2600℃-3000℃.
[0130] In some optional embodiments, the graphitization time is 300h-800h; for example, it can be, but is not limited to, 300h, 350h, 400h, 450h, 500h, 550h, 600h, 650h, 700h, 750h, 800h, or any range between two of the above times. Optionally, the graphitization time is 500h-800h.
[0131] In some embodiments, when the carbon-based material in the porous anode material is soft carbon, the post-processing in the preparation of the porous anode material includes carbonization.
[0132] As one possible implementation, when the carbon-based material in the porous anode material is soft carbon, the carbonization temperature during the preparation of the porous anode material is 1500℃-2000℃; for example, it can be, but is not limited to, 1500℃, 1600℃, 1700℃, 1800℃, 1900℃, 2000℃ or any two of the above temperatures.
[0133] As one possible implementation, when the carbon-based material in the porous anode material is soft carbon, the carbonization treatment time during the preparation of the porous anode material is 15h-40h; for example, it can be, but is not limited to, 15h, 18h, 20h, 23h, 25h, 28h, 30h, 33h, 35h, 37h, 40h or any range between the above two times.
[0134] In some embodiments, the carbon-based material includes one or more of flake graphite and microcrystalline graphite. Accordingly, the carbon-based material in the resulting porous anode material is natural graphite.
[0135] In some optional embodiments, when the carbon-based material in the porous anode material is natural graphite, the post-processing in the preparation process of the porous anode material includes spheroidization.
[0136] In some exemplary embodiments, the rotational speed of the spheroidizing process is 2000rpm-8000rpm; for example, it can be, but is not limited to, 2000rpm, 3000rpm, 4000rpm, 5000rpm, 6000rpm, 7000rpm, 8000rpm or any range between two of the above rotational speeds.
[0137] In some alternative implementations, the spheroidization process takes 5-15 minutes; for example, it can be, but is not limited to, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, or any range between any two of the above times.
[0138] As one possible implementation, spheroidization is performed using at least one of air jet milling and mechanical milling.
[0139] In some embodiments, the carbon-based material includes one or more of bitumen, paraffin wax, biomass, biomass extracts, and synthetic organic polymers. Accordingly, the carbon-based material in the resulting porous anode material is hard carbon.
[0140] In some optional embodiments, when the carbon-based material in the porous anode material is hard carbon, the post-processing in the preparation process of the porous anode material includes carbonization treatment.
[0141] As one possible implementation, when the carbon-based material in the porous anode material is hard carbon, the carbonization temperature during the preparation of the porous anode material is 800℃-1600℃; for example, it can be, but is not limited to, 800℃, 900℃, 1000℃, 1100℃, 1200℃, 1300℃, 1400℃, 1500℃, 1600℃ or any two of the above temperatures.
[0142] In some exemplary embodiments, when the carbon-based material in the porous anode material is hard carbon, the carbonization treatment time during the preparation of the porous anode material is 2h-15h; for example, it can be, but is not limited to, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h or any range between the above two times.
[0143] In some embodiments, the pyrolysis granulation temperature is 600℃-1600℃; for example, it can be, but is not limited to, 600℃, 700℃, 800℃, 900℃, 1000℃, 1100℃, 1200℃, 1300℃, 1400℃, 1500℃, 1600℃, or any range between two of the above temperatures. Optionally, the pyrolysis granulation temperature is 800℃-1200℃.
[0144] As an example, during pyrolysis granulation, the heating method includes at least one of continuous heating and stepped heating.
[0145] As one possible implementation, the pyrolysis granulation time is 0.5h-6h; for example, it can be, but is not limited to, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, or any range between two of the above times. Optionally, the pyrolysis granulation time is 2h-5h.
[0146] In some embodiments, when the carbon-based material in the porous anode material is artificial graphite, the method for preparing the porous anode material includes the following steps:
[0147] S1. A mixture of carbon-based material precursor and hard carbon precursor is prepared by mixing with stirring and then crushing. The hard carbon precursor includes one or more of resin, organic polymer, biomass, and carbohydrates. The carbon-based material precursor includes one or more of activated carbon, coke, carbon black, charcoal, bio-coke, and coal coke. The mass ratio of hard carbon precursor to carbon-based material precursor is 1:(5-50). The type of stirrer used can be, but is not limited to, turbine, paddle, propeller, screw, or planetary. The stirring speed is 10 rpm-300 rpm, and the stirring time is 0.25 h-12 h. The crushing process is carried out using a pulverizer; the pulverizer speed is 10000 rpm-25000 rpm; and the crushing time is 5 min-10 min.
[0148] S2. The mixture is subjected to pyrolysis granulation to prepare an intermediate; the pyrolysis granulation temperature is 600℃-1600℃. The pyrolysis granulation time is 0.5h-5h.
[0149] S3. The intermediate is graphitized to prepare a porous anode material. The graphitization temperature is 2000℃-3300℃; the graphitization time is 300h-800h.
[0150] In some embodiments, when the carbon-based material in the porous anode material is soft carbon, the method for preparing the porous anode material includes the following steps:
[0151] S1. A mixture of carbon-based material precursor and hard carbon precursor is prepared by mixing with stirring and then crushing. The hard carbon precursor includes one or more of resin, organic polymer, biomass, and carbohydrates. The carbon-based material precursor includes one or more of activated carbon, coke, carbon black, charcoal, bio-coke, and coal coke. The mass ratio of hard carbon precursor to carbon-based material precursor is 1:(5-50). The type of stirrer used can be, but is not limited to, turbine, paddle, propeller, screw, or planetary. The stirring speed is 10 rpm-300 rpm, and the stirring time is 0.25 h-12 h. The crushing process is carried out using a pulverizer; the pulverizer speed is 10000 rpm-25000 rpm; and the crushing time is 5 min-10 min.
[0152] S2. The mixture is subjected to pyrolysis granulation to prepare an intermediate; the pyrolysis granulation temperature is 600℃-1600℃. The pyrolysis granulation time is 0.5h-5h.
[0153] S3. Carbonize the intermediate to prepare a porous anode material. The carbonization temperature is 1500℃-2000℃; the carbonization time is 15h-40h.
[0154] In some embodiments, when the carbon-based material in the porous anode material is hard carbon, the method for preparing the porous anode material includes the following steps:
[0155] S1. A mixture of carbon-based material precursor and hard carbon precursor is prepared by mixing with agitation and then crushing. The hard carbon precursor includes one or more of resin, organic polymer, biomass, and carbohydrates. The carbon-based material precursor includes one or more of asphalt, paraffin wax, biomass, biomass extracts, and artificial organic polymers. The mass ratio of hard carbon precursor to carbon-based material precursor is 1:(5-50). The agitator used can be, but is not limited to, turbine, paddle, propeller, screw, or planetary types. The agitation speed is 10 rpm-300 rpm, and the agitation time is 0.25 h-12 h. A pulverizer is used for the crushing process; the pulverizer speed is 10000 rpm-25000 rpm; and the crushing time is 5 min-10 min.
[0156] S2. The mixture is subjected to pyrolysis granulation to prepare an intermediate; the pyrolysis granulation temperature is 600℃-1600℃. The pyrolysis granulation time is 0.5h-6h.
[0157] S3. Carbonize the intermediate to prepare a porous anode material. The carbonization temperature is 800℃-1600℃; the carbonization time is 2h-15h.
[0158] In some embodiments, when the carbon-based material in the porous anode material is natural graphite, the method for preparing the porous anode material includes the following steps:
[0159] S1. A mixture of carbon-based material precursor and hard carbon precursor is prepared by mixing with stirring and then crushing. The hard carbon precursor includes one or more of resin, organic polymer, biomass, and carbohydrates. The carbon-based material precursor includes one or more of flake graphite and microcrystalline graphite. The mass ratio of hard carbon precursor to carbon-based material precursor is 1:(5-50). The type of stirrer used can be, but is not limited to, turbine, paddle, propeller, screw, or planetary. The stirring speed is 10 rpm-300 rpm, and the stirring time is 0.25 h-12 h. The crushing process is carried out using a pulverizer; the pulverizer speed is 10000 rpm-25000 rpm; and the crushing time is 5 min-10 min.
[0160] S2. The mixture is subjected to pyrolysis granulation to prepare an intermediate; the pyrolysis granulation temperature is 600℃-1600℃. The pyrolysis granulation time is 0.5h-5h.
[0161] S3. The intermediate is spheroidized to prepare a porous negative electrode material. The spheroidizing speed is 2000rpm-8000rpm; the spheroidizing time is 5min-15min; at least one of air jet milling and mechanical milling is used for spheroidizing.
[0162] In addition, the secondary battery and power-consuming device of this application will be described below with appropriate reference to the accompanying drawings.
[0163] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.
[0164] The secondary battery of this application includes the porous negative electrode material of this application, which has excellent coulombic efficiency and specific capacity, and high energy density.
[0165] Negative electrode sheet
[0166] The negative electrode sheet includes a negative current collector and a negative active material layer located on at least one side of the negative current collector. The negative active material layer includes the porous negative electrode material of the first aspect of this application or the porous negative electrode material prepared by the preparation method of the second aspect of this application.
[0167] As a non-limiting example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0168] In some embodiments, the compaction density of the negative electrode sheet is 1.4 g / cm³. 3 -1.65g / cm 3 For example, it can be, but is not limited to, 1.4 g / cm³. 3 1.42g / cm 3 1.45g / cm 3 1.47 g / cm 3 1.5g / cm 3 1.52g / cm 3 1.55g / cm 3 1.57g / cm 3 1.6g / cm 3 1.62g / cm 3 1.65g / cm 3 Or the range between any two of the above compaction densities, etc.
[0169] In some optional embodiments, the porous anode material accounts for 95.5%-97% of the mass of the anode active material layer. For example, it can be, but is not limited to, 95.5%, 95.8%, 96%, 96.3%, 96.5%, 96.8%, 97%, or any range between two of the above values. Optionally, the porous anode material accounts for 96%-97% of the mass of the anode active material layer.
[0170] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on the polymeric material substrate. Non-limiting examples of the metal material in the negative electrode current collector may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the negative electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0171] In some embodiments, the negative electrode active material layer may also include other negative electrode active materials known in the art for use in batteries. As a non-limiting example, the negative electrode active material may also include one or more of the following materials: silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include one or more of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0172] In some embodiments, the negative electrode active material layer may optionally include a binder. Optionally, the binder may include one or more of polyimide resin, acrylic resin, polyvinylidene fluoride, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene rubber. The binder may also optionally include one or more of sodium polyacrylate (PAAS), polyacrylamide (PAM), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0173] In some embodiments, the binder accounts for 1.2%-1.8% of the mass of the negative electrode active material layer; for example, it can be, but is not limited to, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, or any range between any two of the above values.
[0174] In some embodiments, the negative electrode active material layer may optionally include a conductive agent. Optionally, the conductive agent may include one or more of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene, and carbon nanotubes.
[0175] In some alternative embodiments, the conductive agent accounts for 0.8%-1.2% of the mass of the negative electrode active material layer; for example, it can be, but is not limited to, 0.8%, 0.9%, 1%, 1.1%, 1.2%, or any range between two of the above values.
[0176] In some embodiments, the negative electrode active material layer may optionally include a dispersant. Optionally, the dispersant may include one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, sodium dodecyl sulfate, methylpentanol, cellulose derivatives, polyacrylamide, and polyvinylpyrrolidone.
[0177] In some optional embodiments, the mass percentage of the dispersant in the negative electrode active material layer is 0.5%-1%; for example, it can be, but is not limited to, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or any range between two of the above values.
[0178] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0179] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder, and any other components, in a solvent (a non-limiting example of a solvent is deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto at least one surface of a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing, and other processes. The surface of the negative electrode current collector coated with the negative electrode slurry can be a single surface of the negative electrode current collector or both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt%-60wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000mPa·s-10000mPa·s. When coating the negative electrode slurry, the coating unit areal density (excluding solvent) on a dry weight basis can be 0.05-0.18g / 1540.25mm. 2 The compaction density of the negative electrode sheet can be 1.0 g / cm³. 3 -1.8g / cm 3 .
[0180] Positive electrode sheet
[0181] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer including a positive active material.
[0182] As a non-limiting example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0183] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on a polymeric material substrate. Non-limiting examples of the metal material in the positive electrode current collector may include one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the positive electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0184] In some embodiments, the positive electrode active material may further include one or more of ternary materials and lithium manganese iron phosphate materials; wherein, the ternary material includes Li x (Ni a Co b Mn c )1-dM d O2-yA y (x is 0.2-1.2) and / or Li x A a (Ni a Co b Mn c )1-dM d O2-yA y (x+a is 0.2-1.2); Lithium manganese iron phosphate materials include Li a Mn 1-y B y P 1-z C z O 4-n D n (a is 0-1.1) and / or Li a A x Mn 1-y B y P 1-z C z O 4-n D n (a+x is 0-1.1).
[0185] It should be noted that the above limitation on x includes the molar content of Li under different charge and discharge states of the battery (typically the battery voltage is between 2-5V).
[0186] Understandably, lithium (Li) is intercalated and deintercalated during the charging and discharging process of a battery, and the Li content in the positive electrode varies depending on the state of discharge. Unless otherwise specified, the Li content in the examples of positive electrode materials listed in this application refers to the initial state of the material. When a positive electrode material is applied to a positive electrode in a battery system, the Li content in the positive electrode material typically changes after charge-discharge cycles. The Li content can be measured using molar content, but is not limited to this. Regarding "Li content refers to the initial state of the material," the initial state of the material refers to its state before being added to the positive electrode slurry. It is understood that new materials obtained by appropriately modifying the listed positive electrode materials are also within the scope of positive electrode materials. The aforementioned appropriate modification refers to acceptable modification methods for the positive electrode material; non-limiting examples include coating modification.
[0187] In the examples of cathode materials in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause changes in the molar content of oxygen, and the actual O content will fluctuate. The O content can be measured in molar content, but is not limited to this.
[0188] In some embodiments, the positive electrode active material may also employ other positive electrode active materials known in the art for use in batteries. As a non-limiting example, the positive electrode active material may include one or more of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, one or more of lithium cobalt oxides (such as LiCoO2), lithium nickel oxides, lithium manganese oxides, lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, lithium nickel cobalt manganese oxides, lithium nickel cobalt aluminum oxides, and their modified compounds. Non-limiting examples of lithium-containing phosphates with an olivine structure include, but are not limited to, one or more of lithium iron phosphate, lithium iron phosphate and carbon composites, lithium manganese phosphate, lithium manganese phosphate and carbon composites, lithium iron manganese phosphate, and lithium manganese iron phosphate and carbon composites. Non-limiting examples of lithium cobalt oxides may include LiCoO2; non-limiting examples of lithium nickel oxides may include LiNiO2; non-limiting examples of lithium manganese oxides may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 Examples of lithium nickel cobalt aluminum oxides include LiNi, etc. 0.80 Co 0.15 Al 0.05O2.
[0189] In some embodiments, the positive electrode active material layer may optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.
[0190] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0191] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as the positive electrode active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry; coating the positive electrode slurry onto at least one surface of the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing, and other processes. The solvent can be selected from, but is not limited to, any of the solvents described in the foregoing embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode current collector coated with the positive electrode slurry can be a single surface or both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt%-80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000 mPa·s-25000 mPa·s. When coating the positive electrode slurry, the coating areal density per unit area (dry weight, minus solvent) can be 0.2-0.45 g / 1540.25 mm. 2 The compaction density of the positive electrode sheet can be 3.0 g / cm³. 3 -3.6g / cm 3 3.3g / cm³ is an option. 3 -3.5g / cm 3 .
[0192] electrolytes
[0193] Electrolytes function to conduct ions between the positive and negative electrode plates. This application does not impose any particular restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or completely solid.
[0194] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0195] In some embodiments, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).
[0196] In some embodiments, the solvent may include ethylene carbonate (EC, ), propylene carbonate (PC, ), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butene carbonate Fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0197] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0198] In some embodiments, the additives in the electrolyte may include, but are not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethyl ethylene carbonate (TFPC), etc.
[0199] Separating membrane
[0200] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0201] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0202] In some embodiments, the thickness of the isolation membrane is 6μm-20μm, optionally 10-16μm.
[0203] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0204] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.
[0205] In some embodiments, the outer packaging of the secondary battery can be a rigid shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft pack, such as a pouch-type soft pack. The material of the soft pack can be plastic; further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0206] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.
[0207] In this application, unless otherwise specified, "cell battery" refers to the basic unit capable of converting chemical energy into electrical energy, and generally includes at least a positive electrode, a negative electrode, and an electrolyte. During the charging and discharging process of the battery, active ions move back and forth between the positive and negative electrode plates, inserting and extracting. The electrolyte acts as a conductor for the active ions between the positive and negative electrode plates.
[0208] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 2 The example shown is a square-structured battery cell 5.
[0209] In some of these embodiments, reference is made to Figure 3 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be selected by those skilled in the art according to actual needs.
[0210] The secondary battery can be either battery module 4 or battery pack 1.
[0211] A battery module includes at least one battery cell. The number of battery cells in a battery module can be one or more, and those skilled in the art can select an appropriate number based on the application and capacity of the battery module.
[0212] Figure 4 This is battery module 4, used as an example. (See reference...) Figure 4 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.
[0213] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.
[0214] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more. Those skilled in the art can select an appropriate number according to the application and capacity of the battery pack.
[0215] Figure 5 and Figure 6 This is battery pack 1 as an example. (See reference...) Figure 5 and Figure 6 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0216] In addition, this application also provides an electrical device, which includes the secondary battery provided in this application. The secondary battery can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptops, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to.
[0217] As an electrical device, a rechargeable battery can be selected based on its usage requirements.
[0218] Figure 7 Here is an example of an electrical device 6. This electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this electrical device, a battery pack or battery module can be used.
[0219] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.
[0220] Example
[0221] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the technology or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0222] I. Preparation of porous anode materials
[0223] Example 1
[0224] Needle coke (as a precursor for carbon-based materials) and lignin (as a precursor for hard carbon) were mixed evenly using a turbine mixer to obtain a mixture with a mass ratio of lignin to needle coke of 1:30. The mixture was then crushed using a pulverizer at a speed of 15,000 rpm for 8 minutes.
[0225] The crushed mixture was pyrolyzed and granulated at 1000℃ for 5 hours to obtain an intermediate.
[0226] The intermediate was graphitized to prepare a porous anode material. The graphitization temperature was 3000℃ and the graphitization time was 800h.
[0227] Example 2-16
[0228] The preparation methods of Examples 2-16 are similar to those of Example 1, and the differences are detailed in Table 1.
[0229] Comparative Example 1
[0230] The preparation methods of Comparative Example 1 and Example 1 are similar, except that no lignin was added when preparing the porous negative electrode material in Comparative Example 1. All other aspects are the same; see Table 1 for details.
[0231] Comparative Example 2
[0232] The preparation methods of Comparative Example 2 and Example 2 are similar, except that no lignin was added when preparing the porous negative electrode material in Comparative Example 2. All other aspects are the same; see Table 1 for details.
[0233] Comparative Example 3
[0234] The preparation methods of Comparative Example 3 and Example 3 are similar, except that no lignin was added when preparing the porous negative electrode material in Comparative Example 3. All other aspects are the same; see Table 1 for details.
[0235] Comparative Example 4
[0236] The preparation methods of Comparative Example 4 and Example 4 are similar, except that no lignin was added when preparing the porous negative electrode material in Comparative Example 4, and everything else is the same; see Table 1 for details.
[0237] The preparation parameters for the above embodiments and comparative examples are shown in Table 1.
[0238] Table 1
[0239]
[0240] In Table 1, n represents the mass ratio of hard carbon precursor to carbon-based material precursor. Porosity refers to the porosity of porous anode material; average pore size refers to the average pore size of the internal pore structure contained in porous anode material.
[0241] The porosity of the aforementioned porous negative electrode material was determined using the following method: the porous negative electrode material was cut into small pieces and placed in a sample container. A glass cone probe was used as the sample container, and pressure was applied to the sample for measurement. The parameters of the mercury porosimeter were set as follows: the pressure applied in the low-pressure station (LP) was approximately 0.6 to 50 PSI (corresponding to a pore diameter of 355-4 micrometers), and the pressure applied in the high-pressure station (HP) was approximately 20 to 60,000 PSI (corresponding to a pore diameter of 10-0.004 micrometers). The mercury porosimeter used was a PoreMaster 60GT mercury porosimeter from the United States.
[0242] The average pore size of the aforementioned porous negative electrode material was determined using the following method:
[0243] The test sample is placed in a sample tube, first degassed by vacuum, and then the entire system is brought to the required vacuum level. The sample tube is then immersed in a liquid nitrogen bath and filled with a known amount of gas. The adsorbent adsorbs the gas, causing a pressure drop. After adsorption equilibrium is reached, the equilibrium pressure of the gas is measured, and the adsorption amount can be calculated based on the pressure change of the system before and after adsorption. The amount of adsorbate gas is gradually increased into the system to change the pressure, and the above operation is repeated to test the adsorption-desorption isotherms. Then, the pore size distribution of the test sample is equivalently determined using the Barrett-Joyner-Halenda model.
[0244] II. Preparation of Secondary Batteries
[0245] 1. Preparation of positive electrode sheet
[0246] Lithium iron phosphate, conductive carbon black (SP), and binder (PVDF) were dispersed in N-methylpyrrolidone solvent at a weight ratio of 96:2:2 and mixed evenly to obtain a positive electrode slurry. The positive electrode slurry was then uniformly coated onto both sides of a positive electrode current collector aluminum foil. After drying and cold pressing, a positive electrode sheet was obtained, with a coating weight per unit area of 0.30 g / 1540.25 mm² on both sides. 2 .
[0247] 2. Preparation of negative electrode sheet
[0248] Porous negative electrode material, sodium carboxymethyl cellulose dispersant, styrene-butadiene rubber binder, and acetylene black conductive agent were mixed in a mass ratio of 97:1:1:1. Deionized water was added, and the mixture was stirred under vacuum to obtain a negative electrode slurry. The negative electrode slurry was uniformly coated onto both sides of a copper foil. After the copper foil was dried at room temperature, it was transferred to a 120°C oven for 1 hour. Then, it was cold-pressed and slit to obtain negative electrode sheets, with a coating amount of 0.15 g / 1540.25 mm² on both sides. 2 .
[0249] 3. Separating membrane
[0250] A 12μm thick polyethylene separator film was selected.
[0251] 4. Preparation of electrolyte
[0252] The organic solvent was a mixture containing ethylene carbonate (EC) and diethyl carbonate (DEC), with a volume ratio of EC to DEC of 3:7. In an argon-atmosphere glove box with a water content of <10 ppm, thoroughly dried lithium salt LiPF6 was dissolved in the organic solvent, and 2 wt% of fluoroethylene carbonate (FEC) was added simultaneously. The mixture was thoroughly mixed to obtain the electrolyte. The concentration of the lithium salt was 1 mol / L.
[0253] 5. Battery manufacturing
[0254] The battery cell is formed by stacking or winding the positive electrode, separator, and negative electrode in sequence. The bare battery cell is then placed in an outer package, injected with the electrolyte, and sealed. After processes such as settling, hot and cold pressing, formation, clamping, and capacity testing, a secondary battery is obtained. The formation process involves charging at 0.04C to 30% of the remaining capacity (SOC).
[0255] III. Secondary Battery Performance Testing
[0256] 1. First-time effectiveness test
[0257] The secondary battery is charged at a constant current of 0.33C to 3.65V, and then charged at a constant voltage of 3.65V to 0.05C. The total capacity at this point is recorded as C0. It is then discharged at a constant current of 0.33C to 2.5V, and then discharged at a constant current of 0.04C to 2.0V. The total discharge capacity at this point is D0. D0 / C0 is the initial effective capacity.
[0258] 2. Cycle count test
[0259] The secondary battery is charged to 3.65V at a constant current of 0.33C, and then discharged to 2.5V at a constant current of 0.33C. This charge-discharge cycle is repeated multiple times until the battery's discharge capacity decays to 0.9D0. The number of cycles at this point is the number of cycles required to decay to 90% SOH.
[0260] 3. Negative electrode rebound rate test
[0261] The thickness d0 of the negative electrode sheet after cold pressing was measured. After the cell performance decayed to 90% SOH, the cell was disassembled, and the electrode sheet was soaked in DMC for 10 minutes to wash away the residual electrolyte. It was then vacuum dried in an 80℃ oven for 10 minutes. The thickness d1 at this time was then recorded. (d1-d0) / d0 is the electrode sheet rebound rate at this time.
[0262] The test results of the above embodiments and comparative examples are shown in Table 2.
[0263] Table 2
[0264]
[0265] As can be seen from the comparison of the results in Table 2, compared with Comparative Examples 1-6, the overall rebound rate of the negative electrode sheet in Examples 1-16 is significantly reduced, and the overall cycle life of the battery is significantly increased while ensuring the first efficiency of the battery. This indicates that the porous negative electrode material provided in this application can effectively alleviate the volume expansion of carbon-based materials while ensuring the first efficiency, and has excellent cycle performance.
[0266] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.
[0267] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A porous negative electrode material, characterized in that, The porous anode material includes secondary particles with internal pore structures. Each secondary particle contains multiple primary particles, each primary particle containing a carbon-based material. Porous hard carbon is filled between adjacent primary particles. The porous hard carbon contained in the secondary particles forms a network structure. The porosity of the porous anode material is 15%-28%. The average pore size of the internal pore structure contained in the porous anode material is 3nm-5.2nm. The internal pore structure refers to the pore structure located inside the secondary particles and not extending to the surface of the secondary particles.
2. The porous negative electrode material as described in claim 1, characterized in that, The porosity of the porous negative electrode material is 18%-27%.
3. The porous negative electrode material as described in claim 1, characterized in that, The porous anode material contains an internal pore structure with an average pore size of 3.0 nm to 4.5 nm.
4. The porous negative electrode material according to any one of claims 1 to 3, characterized in that, The porous anode material contains internal pore structures including micropores with a diameter of less than 2 nm, mesopores with a diameter of 2 nm to 50 nm, and macropores with a diameter of more than 50 nm.
5. The porous negative electrode material as described in claim 4, characterized in that, The number of micropores in the internal pore structure accounts for 55%-70%.
6. The porous negative electrode material as described in claim 5, characterized in that, The number of micropores in the internal pore structure accounts for 58%-68%.
7. The porous negative electrode material as described in claim 4, characterized in that, The mesopores account for 20%-35% of the total number of internal pore structures.
8. The porous negative electrode material as described in claim 7, characterized in that, The mesopores account for 22%-32% of the total number of internal pore structures.
9. The porous negative electrode material as described in claim 4, characterized in that, The number of large holes in the internal hole structure accounts for 3%-10%.
10. The porous negative electrode material as described in claim 9, characterized in that, The number of large holes in the internal hole structure accounts for 4%-8%.
11. The porous negative electrode material according to any one of claims 1 to 3, characterized in that, The porous negative electrode material has an internal pore volume of 0.05 cm³. 3 / g -0.35 cm 3 / g.
12. The porous negative electrode material as described in claim 11, characterized in that, The porous negative electrode material has an internal pore volume of 0.08 cm³. 3 / g -0.32 cm 3 / g.
13. The porous negative electrode material according to any one of claims 1 to 3, characterized in that, The volume average particle size Dv50 of the porous anode material is 15μm-25μm.
14. The porous negative electrode material as described in claim 13, characterized in that, The volume average particle size Dv50 of the porous anode material is 16μm-24μm.
15. The porous negative electrode material according to any one of claims 1 to 3, characterized in that, The porous anode material contains porous hard carbon and carbon-based material in a mass ratio of 1:(5-50).
16. The porous negative electrode material as described in claim 15, characterized in that, The porous anode material contains porous hard carbon and carbon-based material in a mass ratio of 1:(20-35).
17. The porous negative electrode material according to any one of claims 1 to 3, characterized in that, The carbon-based material includes one or more of artificial graphite, natural graphite, hard carbon, and soft carbon.
18. The porous negative electrode material as described in claim 17, characterized in that, The carbon-based material includes artificial graphite.
19. A method for preparing a porous negative electrode material as described in any one of claims 1 to 18, characterized in that, Includes the following steps: A mixture of carbon-based material precursors and hard carbon precursors is prepared by crushing the mixture. The mixture is subjected to pyrolysis and granulation to prepare an intermediate. The intermediate is post-processed to prepare the porous anode material.
20. The method for preparing the porous negative electrode material as described in claim 19, characterized in that, The hard carbon precursor includes one or more of resins, organic polymers, biomass, and carbohydrates.
21. The method for preparing the porous negative electrode material as described in claim 20, characterized in that, The resin includes one or more of phenolic resin, epoxy resin, and polyfurfuryl alcohol resin.
22. The method for preparing the porous negative electrode material as described in claim 20, characterized in that, The organic polymer includes one or more of polyacrylonitrile, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl chloride, polyvinylidene fluoride, and asphalt.
23. The method for preparing the porous negative electrode material as described in claim 20, characterized in that, The biomass includes one or more of cellulose and lignin.
24. The method for preparing the porous negative electrode material as described in claim 20, characterized in that, The carbohydrates include one or more of sucrose and glucose.
25. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The crushing process is carried out using a pulverizer.
26. The method for preparing the porous negative electrode material as described in claim 25, characterized in that, The speed of the pulverizer is 10,000 rpm to 25,000 rpm.
27. The method for preparing the porous negative electrode material as described in claim 26, characterized in that, The speed of the pulverizer is 12,000 rpm to 25,000 rpm.
28. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The crushing process takes 5-10 minutes.
29. The method for preparing the porous negative electrode material as described in claim 28, characterized in that, The crushing process takes 8-10 minutes.
30. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The mass ratio of the hard carbon precursor to the carbon-based material precursor is 1:(5-50).
31. The method for preparing the porous negative electrode material as described in claim 30, characterized in that, The mass ratio of the hard carbon precursor to the carbon-based material precursor is 1:(20-35).
32. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The carbon-based material precursors include one or more of activated carbon, coke, carbon black, charcoal, bio-coke, and coal coke.
33. The method for preparing the porous negative electrode material as described in claim 32, characterized in that, The post-processing includes graphitization.
34. The method for preparing the porous negative electrode material as described in claim 33, characterized in that, The graphitization temperature is 2000℃-3300℃.
35. The method for preparing the porous negative electrode material as described in claim 34, characterized in that, The graphitization temperature is 2500℃-3200℃.
36. The method for preparing the porous negative electrode material as described in claim 33, characterized in that, The graphitization time is 300h-800h.
37. The method for preparing the porous negative electrode material as described in claim 36, characterized in that, The graphitization time is 500-800 hours.
38. The method for preparing the porous negative electrode material as described in claim 33, characterized in that, The post-processing includes carbonization.
39. The method for preparing the porous negative electrode material as described in claim 38, characterized in that, The carbonization process is carried out at a temperature of 1500℃-2000℃.
40. The method for preparing the porous negative electrode material as described in claim 38, characterized in that, The carbonization process takes 15-40 hours.
41. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The carbon-based material includes one or more of flake graphite and microcrystalline graphite.
42. The method for preparing the porous negative electrode material as described in claim 41, characterized in that, The post-processing includes spheroidization.
43. The method for preparing the porous negative electrode material as described in claim 42, characterized in that, The rotational speed for the spheroidizing process is 2000rpm-8000rpm.
44. The method for preparing the porous negative electrode material as described in claim 42, characterized in that, The spheroidization process takes 5-15 minutes.
45. The method for preparing the porous negative electrode material as described in claim 42, characterized in that, The spheroidizing process is performed using at least one of air jet milling and mechanical milling.
46. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The carbon-based material includes one or more of the following: bitumen, paraffin wax, biomass, biomass extracts, and artificial organic polymers.
47. The method for preparing the porous negative electrode material as described in claim 46, characterized in that, The post-processing includes carbonization.
48. The method for preparing the porous negative electrode material as described in claim 47, characterized in that, The carbonization process is carried out at a temperature of 800℃-1600℃.
49. The method for preparing the porous negative electrode material as described in claim 47, characterized in that, The carbonization process takes 2-15 hours.
50. The method for preparing the porous negative electrode material according to any one of claims 19 to 24, characterized in that, The pyrolysis granulation temperature is 600℃-1600℃; and / or The pyrolysis granulation time is 0.5h-6h.
51. The method for preparing the porous negative electrode material as described in claim 50, characterized in that, The pyrolysis granulation temperature is 800℃-1200℃; and / or The pyrolysis granulation time is 2h-5h.
52. A negative electrode sheet, characterized in that, include: Negative electrode current collector; and A negative electrode active material layer is located on at least one side of the negative electrode current collector, and the negative electrode active material layer comprises the porous negative electrode material according to any one of claims 1 to 18 or the porous negative electrode material prepared by the preparation method according to any one of claims 19 to 51.
53. The negative electrode sheet as described in claim 52, characterized in that, The compaction density of the negative electrode sheet is 1.4 g / cm³. 3 -1.65g / cm 3 .
54. The negative electrode sheet as described in any one of claims 52 to 53, characterized in that, The negative electrode active material layer also includes a conductive agent, a dispersant, and a binder.
55. The negative electrode sheet as described in claim 54, characterized in that, The conductive agent includes one or more of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene, and carbon nanotubes.
56. The negative electrode sheet as described in claim 54, characterized in that, The dispersant includes one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, sodium dodecyl sulfate, methylpentanol, cellulose derivatives, polyacrylamide, and polyvinylpyrrolidone.
57. The negative electrode sheet as described in claim 54, characterized in that, The adhesive includes one or more of polyimide resin, acrylic resin, polyvinylidene fluoride, polyvinyl alcohol, sodium carboxymethyl cellulose, and styrene-butadiene rubber.
58. The negative electrode sheet as described in claim 54, characterized in that, The porous anode material accounts for 95.5%-97% of the mass of the anode active material layer.
59. The negative electrode sheet as described in claim 54, characterized in that, The conductive agent accounts for 0.8%-1.2% of the mass of the negative electrode active material layer.
60. The negative electrode sheet as described in claim 54, characterized in that, The dispersant accounts for 0.5%-1% of the mass of the negative electrode active material layer.
61. The negative electrode sheet as described in claim 54, characterized in that, The binder accounts for 1.2%-1.8% of the mass of the negative electrode active material layer.
62. A secondary battery, characterized in that, Includes the negative electrode sheet as described in any one of claims 52 to 61.
63. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 62.
Citation Information
Patent Citations
Negative active material for rechargeable lithium battery, method of preparing the same, and rechargeable lithium battery including the same
KR1020130015967A
Negative active material, lithium secondary battery including the material, and method of manufacturing the material
US20180097229A1