A method for preparing nano-copper powder

By controlling the crystal nucleation and growth rate through a two-step reaction using liquid-phase chemical reduction, uniform-sized and oxidation-resistant nano-copper powder was prepared, solving the problems of uneven particle size distribution and high cost in existing technologies, and realizing efficient and low-cost preparation of nano-copper powder.

CN120644677BActive Publication Date: 2026-11-24NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202511053667.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-30
Publication Date
2026-11-24
Estimated Expiration
2045-07-30

AI Technical Summary

Technical Problem

Existing liquid-phase chemical reduction methods are difficult to prepare nano-copper powder with narrow particle size distribution, uniform size and antioxidant capacity, and physical methods are expensive and complex, resulting in high costs.

Method used

A liquid-phase chemical reduction method was used to control the crystal nucleation and growth rate through a two-step reaction. A specific ratio of copper salt, additives and reducing agent was used, combined with slow drop-addition and temperature control, to prepare nano-copper powder with a particle size of 80nm~100nm.

Benefits of technology

This yielded nano-copper powder with uniform particle size and antioxidant capacity, simplifying the process, reducing costs, and improving the performance and purity of the nano-copper powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120644677B_ABST
    Figure CN120644677B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing nano-copper powder, comprising the following steps: 1. Dissolving copper salt in deionized water to obtain a clear blue solution; 2. Preparing an additive and reducing agent A into a solution; 3. Adding the solution to the clear blue solution to obtain a mixed solution B; 4. Adding reducing agent C to mixed solution B to obtain a mixed solution D; 5. Heating mixed solution D to obtain a purplish-red product; 6. Centrifuging, washing, and vacuum drying the purplish-red product to obtain nano-copper powder with a particle size of 80nm~100nm. This invention uses copper salt as raw material and employs a two-step method. First, additives and reducing agent A are added to effectively control the seed crystal nucleation rate. Then, reducing agent C is added to obtain nano-copper powder with small particle size, uniform particle size distribution, good dispersibility, and antioxidant capacity. This method overcomes the current technical limitations of severe agglomeration and difficulty in large-scale preparation of small-particle-size nano-copper powder. The process is simple, easy to operate, and highly reproducible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal nanomaterials technology, and specifically relates to a method for preparing nano-copper powder. Background Technology

[0002] Due to its unique optical, electrical, thermal, magnetic, and chemical properties, nano-copper powder has wide applications in electromagnetic shielding, high-efficiency catalysts, conductive pastes, high-performance alloys, lubricants, and antibacterial applications. In particular, as a novel conductive paste, it features high conductivity and low cost. Currently, methods for preparing nano-copper powder are mainly divided into two categories: physical methods and chemical methods. Physical methods mainly include traditional electrolysis, spherical deposition, vapor deposition, plasma deposition, and exploding wire deposition, etc. These methods involve expensive equipment, complex processes, and high preparation costs. Currently, commercially available nano-copper powder is mainly prepared using physical vapor deposition (PVD), which produces nano-copper powder with high sphericity, but the equipment is expensive and the process is complex, resulting in a high price. Chemical methods mainly include microemulsion methods, solvothermal methods, electrochemical deposition methods, liquid-phase chemical reduction methods, and thermal reduction methods.

[0003] Liquid-phase chemical reduction is currently the most commonly used method for preparing copper nanoparticles in the laboratory. It involves a redox reaction between a copper salt precursor and a reducing agent in an aqueous phase or solvent, reducing copper ions into copper nanoparticles of different morphologies and sizes. While this method can generate a large number of copper nanoparticles in a short time, its rapid nucleation rate makes the growth process difficult to control, often resulting in nanoparticles with large size, wide size distribution, and poor uniformity. Furthermore, smaller-sized copper nanoparticles have a larger specific surface area and higher activity, making them very susceptible to oxidation, which affects their performance. Therefore, although there has been extensive research on liquid-phase reduction methods for preparing copper nanoparticles, obtaining antioxidant copper nanoparticles with narrow particle size distribution, uniform size, and small particle size remains a challenge. Summary of the Invention

[0004] The technical problem to be solved by this invention is to provide a method for preparing nano-copper powder, addressing the shortcomings of the prior art. This method employs a liquid-phase chemical reduction method, effectively controlling the crystal nucleation and growth rate through a two-step reaction, thereby obtaining nano-copper powder with a uniform particle size of 80nm~100nm and a certain degree of antioxidant capacity.

[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing nano-copper powder, characterized in that the method includes the following steps: Step 1: Dissolve the copper salt in deionized water and stir until homogeneous to obtain a clear blue solution; Step 2: Prepare a solution by mixing the additive and reducing agent A; Step 3: Add the solution prepared from additive and reducing agent A in step 2 to the clear blue solution obtained in step 1 to obtain mixed solution B; Step 4: Add reducing agent C to the mixed solution B obtained in step 3 and stir until homogeneous to obtain mixed solution D; Step 5: Place the mixed solution D obtained in Step 4 into a reaction vessel, and then react it in an oven at 90℃~120℃ for 1h~5h to obtain a purple-red product; Step 6: Wash the purplish-red product obtained in Step 5 with deionized water and anhydrous ethanol in sequence, and then dry it under vacuum to obtain nano-copper powder with a particle size of 80nm~100nm.

[0006] The method for preparing nano-copper powder described above is characterized in that the copper salt in step one is copper nitrate trihydrate, copper sulfate pentahydrate, copper chloride dihydrate, or copper acetate monohydrate. This invention, by controlling the type of copper salt, achieves high solubility, facilitating subsequent preparation.

[0007] The above-mentioned method for preparing nano-copper powder is characterized in that the mass ratio of copper salt to deionized water in step one is 1:6~10. This invention obtains copper nanoparticles with controllable particle size by reasonably and effectively controlling the copper salt concentration. Too high a concentration is detrimental to particle size control, while too low a solution concentration is unfavorable for industrial production.

[0008] The above-mentioned method for preparing nano-copper powder is characterized in that the additive in step two is one or more of sodium alginate, L-methionine, betaine, and glycine. This invention ensures that the reducing agent A can coordinate or cross-link with copper ions by controlling the additive, effectively controlling the concentration of copper ions in the solution, which is beneficial for controlling the particle size of the nano-copper powder. Simultaneously, this additive also helps the product to obtain a near-spherical morphology.

[0009] The method for preparing nano-copper powder described above is characterized in that the reducing agent A in step two is one or more of maltose, fructose, and galactose. This invention, by controlling the composition of the reducing agent A, ensures that copper seed crystals are obtained first, providing nuclei for subsequent copper crystal growth.

[0010] The above-mentioned method for preparing nano-copper powder is characterized in that, in step two, the mass ratio of the additive to the reducing agent A is 1:100~150, and the molar ratio of the reducing agent A to the copper salt is 2~3:1; the concentration of the reducing agent A in the solution prepared by the additive and the reducing agent A is 1M. This invention effectively controls the amount of reducing agent used and the reaction rate by controlling the ratio of the additive, the reducing agent A, and the copper salt, thereby obtaining nano-copper powder with the desired particle size.

[0011] The method for preparing nano-copper powder described above is characterized in that the reducing agent C in step four is hydroxylamine hydrochloride, benzoic acid, or hyaluronic acid. This invention achieves a sufficient reduction reaction by controlling the composition of the reducing agent C.

[0012] The method for preparing nano-copper powder described above is characterized in that the molar ratio of reducing agent C to copper salt in step four is 1~1.5:1, and the reducing agent C is added dropwise. This invention ensures the full progress of the reduction reaction by controlling the molar ratio of reducing agent C to copper salt. Furthermore, by adding reducing agent C dropwise, the concentration of the reducing agent in the reaction system is effectively controlled, allowing the reaction to occur slowly and avoiding the problem of uneven particle size distribution caused by an excessively high concentration of reducing agent in the system at one time, which would lead to uncontrollable product particle size.

[0013] The method for preparing nano-copper powder described above is characterized in that the heating rate of the oven to 90℃~120℃ in step five is no greater than 5℃ / min. This invention controls the heating rate to meet the required reaction temperature and achieves a slow temperature rise in the system, thus controlling the nucleation reaction at a certain rate and ensuring the uniformity of the product particle size.

[0014] The method for preparing nano-copper powder described above is characterized in that the vacuum drying temperature in step six is ​​50℃~80℃. This invention ensures the nano-copper powder is fully dried and avoids oxidation by controlling the vacuum drying temperature.

[0015] Compared with the prior art, the present invention has the following advantages: 1. This invention proposes to use a liquid-phase chemical reduction method to effectively control the crystal nucleation and growth rate through a two-step reaction, thereby obtaining nano-copper powder with a particle size of 80nm~100nm, uniform size, and certain antioxidant capacity.

[0016] 2. This invention employs a two-step control method. First, copper ions react simultaneously with the additive and reducing agent A. On one hand, since reducing agent A is a weak reducing agent, it can effectively control the crystal nucleation rate when reacting with copper ions, preventing rapid nucleation and anisotropic growth, and ensuring that the obtained copper crystal nuclei are of uniform size. On the other hand, copper ions can form a bonding coordination with the carboxyl groups in the additive, which can effectively reduce the oxidation of the generated copper seed crystals by dissolved oxygen in the solution or air. At the same time, due to the steric hindrance effect, it can also prevent the occurrence of seed crystal agglomeration. Therefore, the obtained nucleated seed crystals are controllable in size and uniform in size, providing a good nucleation basis for subsequent crystal growth. Subsequently, a certain amount of strong reducing agent is added dropwise, and the copper crystal nuclei are gradually regrown by slow dropwise addition, finally obtaining nano-copper powder with a particle size of 80nm~100nm, uniform size, and antioxidant capacity.

[0017] 3. This invention addresses the current challenges of preparing narrow-particle-size copper powder, resulting in poor uniformity of particle size distribution, high activity, and susceptibility to oxidation of the obtained small-sized copper powder. It employs a two-step reduction control method to avoid the use of long-chain surfactants such as PVP and CTAB, reducing residual organic matter on the surface of the nano-copper and effectively improving its optical, thermal, electrical, and magnetic properties. This method overcomes the current technical limitations of severe agglomeration and difficulty in large-scale preparation of small-particle-size nano-copper powder. The process is simple, easy to operate, and highly reproducible, representing a novel method for preparing small-particle-size, narrow-distribution, and oxidation-resistant nano-copper powder materials.

[0018] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0019] Figure 1 This is a high-magnification SEM image of the nano-copper powder prepared in Example 1 of this invention.

[0020] Figure 2 This is a low-magnification SEM image of the nano-copper powder prepared in Example 1 of this invention.

[0021] Figure 3 This is a SEM image of the nano-copper powder prepared in Example 2 of the present invention.

[0022] Figure 4 This is a SEM image of the nano-copper powder prepared in Example 3 of the present invention. Detailed Implementation

[0023] Example 1 This embodiment includes the following steps: Step 1: Dissolve 100g of copper nitrate trihydrate in 600mL of deionized water and stir well to obtain a clear blue solution; Step 2: Take 0.85 mol of maltose, add 850 mL of deionized water, stir until completely dissolved, then add 3 g of L-methionine to prepare a solution. Step 3: Add the solution prepared in Step 2 to the clear blue solution obtained in Step 1 to obtain a brown mixed solution B; Step 4: Add 0.41 mol of hydroxylamine hydrochloride to the mixed solution B obtained in Step 3 to obtain mixed solution D; Step 5: Place the mixed solution D obtained in Step 4 into a reaction vessel, and then heat it to 90°C in an oven at a heating rate of 5°C / min for 1 hour to obtain a purple-red product. Step 6: Wash the purplish-red product obtained in Step 5 with deionized water and anhydrous ethanol three times in sequence, and dry it in a vacuum drying oven at 50°C for 10 hours to obtain nano-copper powder with a particle size of 100nm.

[0024] Figure 1 This is a high-magnification SEM image of the nano-copper powder prepared in this embodiment. Figure 2 This is a low-magnification SEM image of the nano-copper powder prepared in this embodiment. Figure 1 and Figure 2 As can be seen from the above, the nano-copper powder prepared in this embodiment is nanoparticles with a particle size distribution of about 100nm. The particles are uniform in size, clean in surface, and no obvious coatings were found. In addition to the particle morphology, no other morphological or impurity products were found in the nano-copper powder prepared in this embodiment, indicating that the obtained nano-copper powder has high purity.

[0025] Example 2 This embodiment includes the following steps: Step 1: Dissolve 100g of copper acetate monohydrate in 1L of deionized water and stir well to obtain a clear blue solution; Step 2: Take 1.5 mol of fructose, add 1.5 L of deionized water, stir until completely dissolved, then add 1.8 g of sodium alginate to prepare a solution. Step 3: Add the solution prepared in Step 2 to the clear blue solution obtained in Step 1 to obtain a brown mixed solution B; Step 4: Add 0.75 mol of hyaluronic acid to the mixed solution B obtained in Step 3 to obtain mixed solution D; Step 5: Place the mixed solution D obtained in Step 4 into a reaction vessel, and then heat it to 120°C in an oven at a heating rate of 5°C / min for 5 hours to obtain a purple-red product. Step 6: Wash the purplish-red product obtained in Step 5 with deionized water and anhydrous ethanol three times in sequence, and dry it in a vacuum drying oven at 50°C for 10 hours to obtain nano-copper powder with a particle size of 80nm.

[0026] Figure 3 This is a SEM image of the nano-copper powder prepared in this embodiment. Figure 3 As can be seen from the above, the nano-copper powder prepared in this embodiment has a granular structure with a particle size of about 80 nm. The particle size distribution is uniform and the size is consistent. In addition to copper nanoparticles, no other morphological or impurity products appeared in the nano-copper powder prepared in this embodiment, indicating that the obtained nano-copper powder has high purity.

[0027] Example 3 This embodiment includes the following steps: Step 1: Dissolve 200g of copper sulfate pentahydrate in 1.6L of deionized water and stir well to obtain a clear blue solution; Step 2: Take 2 mol of glucose, add 2 L of deionized water to it, stir until completely dissolved, then add 2 g of L-methionine and 1 g of glycine to prepare a solution. Step 3: Add the solution prepared in Step 2 to the clear blue solution obtained in Step 1 to obtain a brown mixed solution B; Step 4: Add 1 mol of hydroxylamine hydrochloride to the mixed solution B obtained in Step 3 to obtain mixed solution D; Step 5: Place the mixed solution D obtained in Step 4 into a reaction vessel, and then heat it to 100°C in an oven at a heating rate of 5°C / min for 3 hours to obtain a purple-red product. Step 6: Wash the purplish-red product obtained in Step 5 with deionized water and anhydrous ethanol four times in sequence, and dry it in a vacuum drying oven at 80°C for 8 hours to obtain nano-copper powder with a particle size of 100nm.

[0028] Figure 4 This is a SEM image of the nano-copper powder prepared in this embodiment. Figure 4 As can be seen from the above, the nano-copper powder prepared in this embodiment has a granular structure with a particle size of about 100 nm. The particle size distribution is uniform and the size is consistent. In addition to copper nanoparticles, no other morphological or impurity products appeared in the nano-copper powder prepared in this embodiment, indicating that the obtained nano-copper powder has high purity.

[0029] Example 4 This embodiment includes the following steps: Step 1: Dissolve 100g of copper chloride dihydrate in 1L of deionized water and stir well to obtain a clear blue solution; Step 2: Take 1 mol of fructose and 0.5 mol of glucose, add 1.5 L of deionized water, stir until completely dissolved, then add 2.25 g of sodium alginate to prepare a solution. Step 3: Add the solution prepared in Step 2 to the clear blue solution obtained in Step 1 to obtain a brown mixed solution B; Step 4: Add 0.7 mol of hyaluronic acid to the mixed solution B obtained in Step 3 to obtain mixed solution D; Step 5: Place the mixed solution D obtained in Step 4 into a reaction vessel, and then heat it to 110°C in an oven at a heating rate of 5°C / min for 5 hours to obtain a purple-red product. Step 6: Wash the purplish-red product obtained in Step 5 with deionized water and anhydrous ethanol three times in sequence, and dry it in a vacuum drying oven at 50°C for 10 hours to obtain nano-copper powder with a particle size of 90nm.

[0030] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing nano-copper powder, characterized in that, The method includes the following steps: Step 1: Dissolve the copper salt in deionized water and stir until homogeneous to obtain a clear blue solution; the copper salt is copper nitrate trihydrate, copper sulfate pentahydrate, copper chloride dihydrate, or copper acetate monohydrate. Step 2: Prepare a solution by mixing the additive and reducing agent A; the additive is one or more of sodium alginate, L-methionine and glycine; the reducing agent A is one or more of maltose, fructose and galactose. Step 3: Add the solution prepared from additive and reducing agent A in step 2 to the clear blue solution obtained in step 1 to obtain mixed solution B; Step 4: Add reducing agent C to the mixed solution B obtained in Step 3 and stir until homogeneous to obtain mixed solution D; the reducing agent C is hydroxylamine hydrochloride or hyaluronic acid; the reducing agent C is added dropwise. Step 5: Place the mixed solution D obtained in Step 4 into a reaction vessel, and then react it in an oven at 90℃~120℃ for 1h~5h to obtain a purple-red product; Step 6: Wash the purplish-red product obtained in Step 5 with deionized water and anhydrous ethanol in sequence, and then dry it under vacuum to obtain nano-copper powder with a particle size of 80nm~100nm.

2. The method for preparing nano-copper powder according to claim 1, characterized in that, The mass ratio of copper salt to deionized water in step one is 1:6~10.

3. The method for preparing nano-copper powder according to claim 1, characterized in that, In step two, the mass ratio of the additive to the reducing agent A is 1:100~150, and the molar ratio of the reducing agent A to the copper salt is 2~3:1; the concentration of the reducing agent A in the solution prepared by the additive and the reducing agent A is 1M.

4. The method for preparing nano-copper powder according to claim 1, characterized in that, The molar ratio of reducing agent C to copper salt in step four is 1~1.5:

1.

5. The method for preparing nano-copper powder according to claim 1, characterized in that, In step five, the heating rate of the oven to 90℃~120℃ shall not exceed 5℃ / min.

6. The method for preparing nano-copper powder according to claim 1, characterized in that, The vacuum drying temperature in step six is ​​50℃~80℃.

Citation Information

Patent Citations

  • Silver powder and method for manufacturing same

    CN113165075A

  • Method for preparing homogeneous spherical copper granule by seeding growth

    CN1522815A

  • Method for producing copper powder and copper powder

    JP2010144234A

  • Nano-metal 3D printing ink and application thereof

    WO2022262801A1