A humic acid-coated sulfur-doped nano zero-valent iron material, a preparation method therefor, and an application thereof

By coating the surface of nano-zero-valent iron materials with humic acid and sulfur doping, a highly conductive FeS shell and a biocompatible coating are formed, solving the stability and biocompatibility issues of nano-zero-valent iron materials in anaerobic sludge treatment. This achieves efficient organic wastewater treatment and increased methane production, making it suitable for industrial applications.

CN120647008BActive Publication Date: 2026-11-24ANHUI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510951837.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-10
Publication Date
2026-11-24
Estimated Expiration
2045-07-10

AI Technical Summary

Technical Problem

Existing nano-zero-valent iron materials suffer from problems such as easy aggregation, reduced activity, poor biocompatibility, and poor process economy in anaerobic sludge treatment, which affect the treatment effect of organic wastewater.

Method used

By coating the surface of nano-zero-valent iron materials with humic acid and sulfur doping, a highly conductive FeS shell and a natural, non-toxic, and biocompatible outer layer are formed, solving the problems of material stability and biocompatibility, and enhancing electron transfer efficiency and catalytic activity.

Benefits of technology

It significantly enhances the activity of sludge from anaerobic wastewater treatment, improves the removal rate of organic matter and methane production, and achieves high stability and low-cost application of the material, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120647008B_ABST
    Figure CN120647008B_ABST
Patent Text Reader

Abstract

This invention discloses a sulfur-doped nano-zero-valent iron material based on humic acid coating, its preparation method, and its application. The method includes the following steps: (1) dispersing dry nano-zero-valent iron powder in deionized water, adding sodium sulfide solution dropwise under nitrogen protection, stirring, centrifuging, removing the supernatant, washing, and drying to obtain sulfur-doped nano-iron particles; (2) adding the sulfur-doped nano-iron particles to a humic acid solution and dispersing them evenly, stirring under nitrogen protection, then washing and drying to obtain the sulfur-doped nano-zero-valent iron material based on humic acid coating. This invention, by modifying the nano-zero-valent iron material, enhances the activity of anaerobic sludge in wastewater treatment and improves the removal rate of methane production and organic indicators such as COD.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of water pollution control and resource utilization technology, specifically to a sulfur-doped nanomaterial based on humic acid coating, its preparation method, and its application. Background Technology

[0002] With the acceleration of industrialization, the large-scale discharge of organic wastewater poses a serious threat to the aquatic ecological environment. Anaerobic biological treatment technology has been widely used in the field of wastewater treatment, but due to the accumulation of toxic substances and insufficient electron donors, the activity of anaerobic sludge has decreased and the efficiency of organic matter removal has declined. Therefore, how to improve the activity of sludge in the anaerobic treatment of wastewater has become an urgent need.

[0003] In recent years, nano-zero-valent iron (nZVI) has been widely used in organic wastewater treatment and heavy metal remediation due to its strong reducing properties and high reactivity. Adding nZVI to anaerobic wastewater treatment systems can effectively enhance microbial metabolic activity, promote electron transfer, and accelerate the decomposition of organic pollutants. However, exposed nZVI is prone to aggregation, leading to a rapid decrease in activity, and its direct contact with microorganisms can cause toxicity, limiting its application effectiveness. Furthermore, traditional nZVI and its modified products suffer from defects such as easy aggregation and surface oxidation, making them prone to deactivation in anaerobic reaction systems. Sulfur doping often leads to problems such as poor material dispersion, insufficient electron transfer efficiency, and low material utilization.

[0004] In summary, existing technologies still face challenges such as poor material stability, low biocompatibility, and unsatisfactory process economics. There is an urgent need to develop a new modification method to enhance the activity of sludge in anaerobic wastewater treatment. Summary of the Invention

[0005] The purpose of this invention is to provide a sulfur-doped nano-zero-valent iron material based on humic acid coating, its preparation method and application. By modifying the nano-zero-valent iron material, the activity of sludge in anaerobic wastewater treatment is enhanced, and the removal rate of organic indicators such as methane production and COD is improved.

[0006] In one aspect of the present invention, a method for preparing sulfur-doped zero-valent iron nanomaterials based on humic acid coating is proposed. According to an embodiment of the present invention, the method includes the following steps:

[0007] (1) Disperse dry nano-zero-valent iron powder in deionized water, add sodium sulfide solution dropwise under nitrogen protection, stir, centrifuge, remove supernatant, wash and dry to obtain sulfur-doped nano-iron particles;

[0008] (2) Sulfur-doped nano-iron particles are added to humic acid solution and dispersed evenly. The mixture is stirred under nitrogen protection, then washed and dried to obtain the sulfur-doped nano-zero-valent iron material based on humic acid coating.

[0009] In addition, the method for preparing sulfur-doped zero-valent iron nanomaterials based on humic acid coating according to the above embodiments of the present invention may also have the following additional technical features:

[0010] In some embodiments of the present invention, in step (1), the preparation method of the nano zero-valent iron powder is as follows: under a nitrogen atmosphere, the ferric chloride hexahydrate solution is deoxygenated and then ascorbic acid is added. The reaction process is carried out by stirring in an oil bath. After the reaction is completed, the supernatant is removed by centrifugation, and the nano zero-valent iron powder is obtained after washing and drying.

[0011] In some embodiments of the present invention, the molar ratio of iron to ascorbic acid in the ferric chloride hexahydrate is (0.3-0.5):1; the oil bath temperature is 65-75℃; the stirring speed is 400-500 rpm, and the stirring time is 110-120 min; the washing is performed sequentially with deionized water and anhydrous ethanol. The nano-zero-valent iron powder prepared under the above parameters exhibits better performance and can effectively reduce impurities, thereby optimizing its properties. The centrifugation speed is 8000 rpm, and the centrifugation time is 8-10 min. Under these centrifugation conditions, the nano-zero-valent iron powder obtained is more uniform, facilitating the subsequent preparation of modified materials with better properties.

[0012] In some embodiments of the present invention, in step (1), the molar ratio of S to Fe in the sodium sulfide nonahydrate and ferric chloride hexahydrate is (0.2-0.6):1; the washing is carried out sequentially with deionized water and anhydrous ethanol; the drying temperature is 55-65℃, and the drying time is 6-12h. The above method can ensure the uniform sulfidation degree of the nano-zero valent iron powder and facilitate volatilization and drying while effectively washing the sulfur-doped nano-zero valent iron material.

[0013] In some embodiments of the present invention, in step (2), the concentration of the humic acid solution is 1.0-1.2 g / L; the mass ratio of the sulfur-doped nano-iron particles to the humic acid is (5-6):1; the dropping rate of the sodium sulfide is 0.5-1.0 mL / min; the stirring speed is 300-350 rpm, and the stirring time is 5-6 h; the washing is performed sequentially with deionized water and anhydrous ethanol; the drying temperature is 40-45℃, and the drying time is 6-10 h. The above drying temperature can prevent the humic acid from failing to coat at excessively high temperatures, ensuring that the humic acid layer stably coats the sulfur-doped nano-zero-valent iron material.

[0014] In another aspect of the present invention, the present invention provides a method for preparing sulfur-doped nano-zero-valent iron materials based on humic acid coating to obtain sulfur-doped nano-zero-valent iron materials based on humic acid coating.

[0015] In another aspect of the invention, a method for enhancing the activity of anaerobic sludge is proposed. According to an embodiment of the invention, the sulfur-doped nano-zero-valent iron material based on humic acid coating is added to the anaerobic activated sludge mixture.

[0016] In another aspect of the present invention, the present invention proposes a method for enhancing the activity of anaerobic sludge in organic wastewater. According to an embodiment of the present invention, the method includes the following steps: adding the sulfur-doped nano-zero-valent iron material based on humic acid coating to wastewater containing anaerobic activated sludge for anaerobic biological treatment.

[0017] In addition, the method for enhancing the activity of anaerobic sludge in organic wastewater according to the above embodiments of the present invention may also have the following additional technical features:

[0018] In some embodiments of the present invention, the concentration of the anaerobic digestion sludge is 4–6 g / L; the dosage of the sulfur-doped nano-zero-valent iron material based on humic acid coating is 0.3–0.6 g / L. The above-mentioned dosage of sulfur-doped nano-zero-valent iron material based on humic acid coating can provide exogenous electrons and enrich the ability of functional microorganisms, thereby improving treatment efficiency.

[0019] In some embodiments of the present invention, the temperature of the anaerobic biological treatment is 34-36°C.

[0020] Compared with the prior art, the beneficial effects of the present invention are:

[0021] 1. This invention fundamentally enhances the performance of nano-iron cores by introducing a sulfidation reagent. Sulfur doping forms a highly conductive FeS shell around the core, fundamentally improving its properties. This FeS shell replaces the traditional easily formed insulating oxide passivation layer, effectively and rapidly transferring electrons generated by the core to the material surface, thus facilitating their transfer to contaminants. Simultaneously, the microcouple effect formed by FeS and the iron core accelerates electron release, both significantly enhancing the material's electron donor reduction capability. Furthermore, the surface of this sulfide iron core itself serves as an excellent catalytic active site, efficiently activating peroxides to generate strong oxidizing free radicals or promoting hydrogen evolution reactions, thereby endowing the material with superior catalytic reactivity.

[0022] 2. This preparation method addresses material instability through a step-by-step construction of a synergistic structure. First, a FeS shell with enhanced conductivity and corrosion resistance is generated outside the nZVI core via a sulfidation reaction, initially improving electron transfer efficiency and oxidation resistance. Next, HA coating utilizes electrostatic repulsion and steric hindrance to fundamentally solve the particle agglomeration problem. Simultaneously, HA acts as a physical barrier, completely preventing oxidative deactivation. Its unique quinone structure also serves as an electron shuttle, synergistically working with the FeS shell to efficiently transfer electrons to pollutants, achieving a balance between stability and high efficiency.

[0023] 3. This invention solves the problem of microbial toxicity through HA coating. This invention coats the highly active S-nZVI core with a natural, non-toxic "biocompatible outer layer." The HA coating not only physically isolates the nanoparticles from direct contact with microbial cells, preventing physical damage, but also effectively complexes and buffers potentially leaked iron ions, eliminating chemical toxicity. This transforms the material from one that inhibits microorganisms into a biocompatible material that can be safely integrated into biological systems such as anaerobic digestion.

[0024] 4. The method of this invention significantly improves both wastewater COD removal rate and anaerobic digestion methane yield. Experimental data show that the material of this invention significantly enhances sludge activity, and the modified S-nZVI has excellent reducing ability, synergistically promoting microbial metabolism, effectively promoting organic matter decomposition and methane production. The overall methane yield is higher than that of traditional anaerobic reaction systems, and the reaction endpoint is more stable.

[0025] 5. The entire process of this invention is carried out under mild aqueous phase conditions. The HA used is a natural organic compound, which is environmentally friendly and non-toxic. Furthermore, the doping elements such as iron and sulfur used are widely available, making the preparation process simple and convenient to operate. The entire process is mild, requiring no high-temperature or high-pressure conditions, significantly reducing operating energy consumption. This enables the preparation of high-performance, highly stable materials at low cost and with environmental friendliness, making them suitable for large-scale industrial production and application. Attached Figure Description

[0026] Figure 1 This is a comparison chart of total methane production and yield when the materials prepared in Examples 1-3 and Comparative Examples 1-5 are used to enhance the activity of anaerobic sludge in Application Example 1 of the present invention;

[0027] Figure 2 This is a comparison diagram showing the methanogenesis during anaerobic digestion when the materials prepared in Examples 1-3 and Comparative Examples 1-5 are used to enhance the activity of anaerobic sludge in Application Example 1 of the present invention.

[0028] Figure 3 This is a comparison chart showing the remaining SCOD when the materials prepared in Examples 1-3 and Comparative Examples 1-5 are used to enhance the activity of anaerobic sludge in Application Example 1 of the present invention.

[0029] Figure 4 This is a comparison chart showing the accumulation of VFAs during anaerobic digestion when the materials prepared in Examples 1-3 and Comparative Examples 1-5 are used to enhance the activity of anaerobic sludge in Application Example 1 of the present invention.

[0030] Figure 5 This is a comparison chart showing the pH changes during anaerobic digestion when the materials prepared in Examples 1-3 and Comparative Examples 1-5 are used to enhance the activity of anaerobic sludge in Application Example 1 of the present invention.

[0031] Figure 6 This is a comparison chart showing the COD removal rate when the materials prepared in Examples 1 and 4-13 enhance the activity of anaerobic sludge and when the materials in Examples 2-4 enhance the activity of anaerobic sludge. Detailed Implementation

[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0033] Example 1

[0034] A method for preparing sulfur-doped zero-valent iron nanomaterials based on humic acid coating includes the following steps:

[0035] S1. Preparation of nZVI

[0036] 100 mL of 0.1 mol / L ferric chloride hexahydrate solution was added to a three-necked flask, and nitrogen gas with a purity of 99.9% was passed through for 30 min to completely remove oxygen. 0.2 mol / L ascorbic acid solution was added dropwise at 1 mL / min using a constant pressure dropping funnel for 1 h. The mixture was stirred in an oil bath at 70 °C and 500 rpm for 2 h. After the reaction was completed, the supernatant was removed by centrifugation at 8000 rpm for 10 min. The supernatant was washed sequentially with deionized water and 95% anhydrous ethanol under the same centrifugation conditions. The mixture was then vacuum dried at 60 °C for 6 h to obtain nano-iron particles, denoted as nZVI.

[0037] S2, nZVI vulcanization modification

[0038] Dry nZVI powder was ultrasonically dispersed in 100 mL of deionized water. Under a nitrogen atmosphere with a purity of 99.9%, sodium sulfide heptahydrate solution was slowly added dropwise at a rate of 1 mL / min according to the target sulfur-iron ratio S:Fe = 0.4 (molar ratio). The mixture was stirred at room temperature for 2 h. After centrifugation at 8000 rpm for 10 min, the supernatant was removed, and the mixture was washed successively with deionized water and 95% anhydrous ethanol. After vacuum drying at 60 °C for 6 h, sulfur-doped iron nanoparticles were obtained, denoted as S-nZVI.

[0039] S3, humic acid modification

[0040] 0.2 g of HA powder was dissolved in 200 mL of deionized water and magnetically stirred for 2 h. The pH was adjusted to 7.0 using 1 mol / L NaOH solution, and the mixture was ultrasonically dispersed for 30 min before filtration. 0.2 g of the above S-nZVI powder was added to 200 mL of the HA solution and ultrasonically dispersed for 10 min. The mixture was then magnetically stirred at 300 rpm for 6 h under a nitrogen atmosphere with a purity of 99.9% to ensure complete HA adsorption. The mixture was then washed successively with deionized water and 95% anhydrous ethanol, and vacuum dried at 40 °C for 6 h to obtain HA-S-nZVI, named HS2-0.4.

[0041] Example 2

[0042] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating differs from Example 1 only in that: in step S2, sodium sulfate heptahydrate and ferric chloride hexahydrate are in a molar ratio of S:Fe=0.2:1; the final sulfur-doped nano-zero-valent iron material based on humic acid coating is named HS2-0.2.

[0043] Example 3

[0044] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating differs from Example 1 only in that: in step S2, sodium sulfate heptahydrate and ferric chloride hexahydrate are in a molar ratio of S:Fe=0.6:1; the final sulfur-doped nano-zero-valent iron material based on humic acid coating is named HS2-0.6.

[0045] Example 4

[0046] A method for preparing sulfur-doped zero-valent iron nanomaterials based on humic acid coating differs from Example 1 only in that: in step S1, a 0.2 mol / L ascorbic acid solution is added dropwise to the mixture through a constant pressure funnel at a dropping rate of 2 mL / min for 42 min.

[0047] Example 5

[0048] A method for preparing sulfur-doped zero-valent iron nanomaterials based on humic acid coating differs from Example 1 only in that: in step S1, a 0.4 mol / L ascorbic acid solution is added dropwise to the mixture through a constant pressure funnel at a dropping rate of 4 mL / min for 16 min.

[0049] Example 6

[0050] A method for preparing sulfur-doped nano-zero-valent iron materials based on humic acid coating, which differs from Example 1 only in that: in step S1, the oil bath temperature is 65°C, the stirring speed is 320 rpm, and the stirring time is 48 min.

[0051] Example 7

[0052] A method for preparing sulfur-doped nano-zero-valent iron materials based on humic acid coating, which differs from Example 1 only in that: in step S1, the oil bath temperature is 75°C, the stirring speed is 420 rpm, and the stirring time is 75 min.

[0053] Example 8

[0054] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating, which differs from Example 1 only in that: in step S2, the oil bath temperature is 30°C, the stirring speed is 320 rpm, and the stirring time is 48 min.

[0055] Example 9

[0056] A method for preparing sulfur-doped nano-zero-valent iron materials based on humic acid coating, which differs from Example 1 only in that: in step S2, the oil bath temperature is 55°C, the stirring speed is 220 rpm, and the stirring time is 98 min.

[0057] Example 10

[0058] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating, which differs from Example 1 only in that: in step S1, the vacuum drying method is to place the washed material in a vacuum drying oven at a temperature of 45°C and dry it for 12 hours.

[0059] Example 11

[0060] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating differs from Example 1 only in that: in step S1, the vacuum drying method involves placing the washed material in a vacuum drying oven at 65°C for 3 hours.

[0061] Example 12

[0062] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating differs from Example 1 only in that: in step S2, the vacuum drying method involves placing the washed material in a vacuum drying oven at 45°C for 12 hours.

[0063] Example 13

[0064] A method for preparing sulfur-doped nano-zero-valent iron material based on humic acid coating differs from Example 1 only in that: in step S3, the vacuum drying method involves placing the washed material in a vacuum drying oven at 45°C for 10 hours.

[0065] Comparative Example 1

[0066] A nano-iron particle, whose preparation method is exactly the same as step S1 in Example 1, is denoted as nZVI.

[0067] Comparative Example 2

[0068] A sulfur-doped iron nanoparticle, whose preparation method is exactly the same as steps S1 and S2 in Example 1, is denoted as S-nZVI.

[0069] Comparative Example 3

[0070] A method for preparing sulfur-doped iron nanoparticles differs from that in Example 1 in that a one-step synthesis of S-nZVI is employed. The specific method is as follows: 100 mL of 0.1 mol / L ferric chloride hexahydrate solution is added to a three-necked flask under a nitrogen atmosphere with a purity of 99.9%. The flask is magnetically stirred at 500 rpm, and 0.02 mol / L sodium sulfide heptahydrate solution is slowly added dropwise at a rate of 1 mL / min for 45 min. Then, 0.2 mol / L ascorbic acid solution is added dropwise at a rate of 1 mL / min. The oil bath temperature is maintained at 50 ± 1 °C, and stirring is continued for 1 h. The solution gradually changes from brownish-red to a black suspension. The suspension is then centrifuged at 8000 rpm for 10 min, the supernatant is discarded, and the suspension is washed three times with 10 mL of 95% anhydrous ethanol to remove unreacted substances. The suspension is then vacuum dried at 60 °C for 6 h to obtain black S-nZVI powder, which is then coated with HA and named HSI-0.4.

[0071] Comparative Example 4

[0072] A method for preparing sulfur-doped iron nanoparticles differs from Comparative Example 3 only in that: ferric chloride hexahydrate and sodium sulfate heptahydrate are prepared in a molar ratio of S:Fe = 0.2:1, and named HS1-0.2.

[0073] Comparative Example 5

[0074] A method for preparing sulfur-doped iron nanoparticles differs from Comparative Example 3 only in that: ferric chloride hexahydrate and sodium sulfate heptahydrate are prepared in a molar ratio of S:Fe = 0.6:1, and named HS1-0.6.

[0075] Application Example 1

[0076] A method for enhancing the activity of anaerobic sludge in organic wastewater includes the following steps:

[0077] (1) Preparation of anaerobic activated sludge mixed liquor

[0078] The anaerobic activated sludge mixed liquor comprises anaerobic activated sludge and organic wastewater. In this application example, the organic wastewater is artificially synthesized from the following raw materials: sucrose (C... 12 H 22 O 11 (NH4)6Mo6O provides the carbon source, ammonium chloride (NH4Cl) provides the nitrogen source, and potassium dihydrogen phosphate (KH2PO4) provides the phosphorus source, with a C:N:P ratio of 200:5:1 (mass ratio). Trace elements include the following raw materials: (NH4)6Mo6O 24 ·4H2O 1.5mg / L, H3BO40.5mg / L, NiCl2·6H2O 0.5mg / L, AlCl3 0.25mg / L, MnCl2·4H2O 0.5mg / L, COCl2·6H2O 0.5mg / L, MgCl2·6H2O 10mg / L, FeCl2 2.5mg / L, ZnCl2 0.5mg / L, CaCl2 5mg / L, CuCl2·5H2O 0.5mg / L, NaCl 1.0mg / L, EDTA 2.5mg / L.

[0079] The preparation method of anaerobic activated sludge is as follows: The sludge used as inoculum in the glass reactor was taken from the internal circulation anaerobic reactor of a wastewater treatment plant in Hefei. The sludge had a moisture content of 88.95%, a total suspended solids concentration of 191.44 g / L, and a volatile solids concentration of 265.32 g / L. Before inoculation, the anaerobic sludge was acclimated and cultured for one week in a 5L laboratory UASB reactor with an influent of 3000 mg / L COD at a C:N:P ratio of 200:5:1 (mass ratio) for 48 hours to maintain its activity.

[0080] (2) Add 400 mL of anaerobic activated sludge mixture to a 500 mL glass reactor. The concentration of anaerobic digested sludge is 5 g / L, and the sludge load F / M is 0.93 kg COD / (kg VSS). Then add the materials prepared in Examples 1-3 and Comparative Examples 1-5 to the mixture at a dosage of 0.5 g / L. Adjust the pH to 8.0 with NaHCO3. After nitrogen stripping for 30 min, place the mixture in a shaker. Adjust the shaker speed to 200 rpm and the temperature to 35 °C for anaerobic biological treatment.

[0081] A blank control group was set up, which differed from Application Example 1 in that the optimized HA-S-nZVI was not added. Then the following tests were performed:

[0082] (1) Total methane production and yield

[0083] The gas produced in the glass reactor was collected using a Bekman aluminum foil gas collection bag. A 1 mL syringe was used to extract the gas for gas chromatography composition analysis, primarily detecting the CH4 content. The gas volume was determined using the water displacement method. The methane yield was calculated by dividing the actual methane production by the theoretical methane production.

[0084] like Figure 1 As shown, the addition of materials can effectively improve the methane yield during the anaerobic digestion of wastewater. The HS2-0.4, HS2-0.2, and HS1-0.4 obtained in Examples 1, 2, and 3, respectively, showed increases of 11.89%, 9.41%, and 7.34% compared to the blank control group. Figure 2 As shown, except for the blank control group, the cumulative methane production in each group gradually increased. The irreversible acid accumulation in the blank control group affected COD degradation and methane production, indicating that the addition of nZVI material facilitated the anaerobic digestion of organic wastewater. Comparisons of Comparative Examples 1 and 2-5 show that sulfur doping further promoted methane production. Furthermore, the HS2-0.4, HS2-0.2, and HS1-0.4 obtained in Examples 1, 2, and 3, respectively, showed increases of 18.21%, 9.56%, and 4.72% compared to the nZVI group in Comparative Example 1. Therefore, in the sludge anaerobic metabolism system, the two-step synthesis method with an S / Fe molar ratio of 0.4, i.e., the preparation of HA-S-nZVI in Example 1, demonstrates absolute advantages in promoting anaerobic digestion of organic wastewater, alleviating acid inhibition, and increasing methane production yield and efficiency.

[0085] (2) Remaining SCOD status

[0086] Take the water sample after the reaction in the glass reactor, filter it with a 0.45um aqueous filter membrane, add it to the COD digestion tube, shake it evenly, and then place it in the COD digester at 165℃ for 15 minutes. After digestion is completed, let it stand and cool to about 60℃, shake it evenly again, and let it stand until it is completely cooled before testing it in the COD detector.

[0087] like Figure 3 As shown, in the first 72 hours after the reaction started, the residual COD of each group was below 1500 mg / L, with the residual COD of HS2-0.4 being lower than that of the other groups, below 800 mg / L. During the 200-hour run, the residual COD of Comparative Examples 1-5 and Examples 1-3 was less than 200 mg / L.

[0088] (3) VFAs accumulation status

[0089] Water samples from the glass reactor were filtered through a 0.45 μm aqueous filter membrane and then acidified with 3.3% formic acid. Detection was performed using an imported gas chromatograph equipped with a flame ionization detector and a 30 m × 0.25 mn × 0.25 μm DB-FFAP column. The column oven was initially set at 100℃ for 3 min, then increased by 20℃ / min for 4 min, and finally held at 180℃ for 3 min. The injector and detector temperatures were 220℃ and 230℃, respectively. Nitrogen was used as the carrier gas at a flow rate of 5 mL / min. The acidified sample was placed in an autosampler for analysis, and standard solutions of various acids corresponding to VFAs were prepared to calculate the VFA concentration in the effluent.

[0090] In the anaerobic digestion process of wastewater, during the 200-hour operation, the blank control group showed significant and irreversible acid accumulation, which also significantly inhibited COD degradation and methane production, thus preventing the anaerobic digestion process from proceeding smoothly. However, the addition of materials in Comparative Examples 1-5 and Examples 1-3 effectively alleviated acid inhibition. Figure 4 As shown, after anaerobic digestion, the VFAs in the material group all reached below 30 mg / L.

[0091] (4) pH changes

[0092] A pH meter was used to test the water sample in the glass reactor.

[0093] In the anaerobic digestion process of wastewater, during the 200-hour operation, the blank control group showed significant and irreversible acidification, which prevented the anaerobic digestion process from proceeding smoothly. However, in Comparative Examples 1-5 and Examples 1-3, the reaction proceeded normally after the addition of materials. Figure 5As shown, the pH value of the blank group water sample remained below 6.5, while the pH value of the material group fluctuated within the normal range of 7.0-7.5.

[0094] (5) COD removal rate

[0095] The COD removal content is obtained by subtracting the remaining SCOD value from the initial COD value, and then dividing it by the initial COD value to calculate the COD removal rate.

[0096] like Figure 6 As shown, in the first 72 hours after the reaction started, the COD removal rate of each group was above 50%, with the COD removal rate of HS2-0.4 being higher than that of the other groups, reaching 78.16%. During the 200-hour operation, the COD removal rate of Comparative Examples 1-5 and Examples 1-3 was all greater than 90%.

[0097] Application Example 2

[0098] A method for enhancing the activity of anaerobic sludge, which differs from Application Example 1 only in that: the dosage of HA-S-nZVI prepared in Example 1 is 0.4 g / L, the concentration of anaerobic digested sludge is 4 g / L, and the sludge loading F / M is 0.74 kg COD / (kg VSS).

[0099] Application Example 3

[0100] A method for enhancing the activity of anaerobic sludge, which differs from Application Example 1 only in that: the dosage of HA-S-nZVI prepared in Example 1 is 0.6 g / L, the concentration of anaerobic digested sludge is 6 g / L, and the sludge loading F / M is 1.11 kg COD / (kg VSS).

[0101] Application Example 4

[0102] A method for enhancing the activity of anaerobic sludge, which differs from Application Example 1 only in that the shaking speed is 160 rpm and the temperature is 38°C.

[0103] The materials prepared in Examples 1 and 4-13 were enhanced to increase the activity of anaerobic sludge according to the method in Application Example 1. Then, the above groups and Application Examples 2-3 were subjected to performance tests, including COD removal rate and methane production. The test results are shown in the table below:

[0104] Group Example 1 Example 4 Example 5 Example 6 Example 7 Example 8 Example 9 COD removal rate % 97.07 96.24 96.03 96.59 96.35 96.86 97.01 Methane production (mL) 306.9 298.6 295.5 300.2 296.7 302.4 305.7 Group Example 10 Example 11 Example 12 Example 13 Application Example 2 Application Example 3 Application Example 4 COD removal rate % 96.66 95.24 96.68 96.74 96.09 96.32 96.75 Methane production (mL) 301.1 291.1 301.7 302.3 295.6 298.3 299.3

[0105] As shown in the table above, under the anaerobic treatment of organic wastewater with excessively low or high ascorbic acid dosing parameters, stirring parameters, drying temperature and centrifugation parameters within the scope of this application, the COD removal effect and methane generation efficiency are not significantly different from those in Example 1. Therefore, from an economic point of view, Example 1 is the optimal solution.

[0106] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the structure of the present invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.

Claims

1. A method for enhancing the activity of anaerobic sludge in organic wastewater, characterized by, Includes the following steps: Sulfur-doped nano-zero-valent iron materials coated with humic acid were added to wastewater containing anaerobic activated sludge for anaerobic biological treatment. The method for preparing sulfur-doped zero-valent iron nanomaterials based on humic acid coating includes the following steps: (1) Disperse dry nano-zero-valent iron powder in deionized water, add sodium sulfide solution dropwise under nitrogen protection, stir, centrifuge, remove supernatant, wash and dry to obtain sulfur-doped nano-iron particles; (2) Sulfur-doped nano-iron particles are added to humic acid solution and dispersed evenly. The mixture is stirred under nitrogen protection, then washed and dried to obtain the sulfur-doped nano-zero-valent iron material based on humic acid coating.

2. The method for enhancing the activity of anaerobic sludge in organic wastewater according to claim 1, characterized in that: In step (1), the preparation method of the nano zero-valent iron powder is as follows: under a nitrogen atmosphere, the ferric chloride hexahydrate solution is deoxygenated and then ascorbic acid is added. The reaction process is carried out by stirring in an oil bath. After the reaction is completed, the supernatant is removed by centrifugation, and the nano zero-valent iron powder is obtained after washing and drying.

3. The method for enhancing the activity of anaerobic sludge in organic wastewater according to claim 2, characterized in that: The molar ratio of iron to ascorbic acid in the ferric chloride hexahydrate is (0.3-0.5):1; the temperature of the oil bath is 65-75℃; the stirring speed is 400-500 rpm and the stirring time is 110-120 min; the washing is carried out sequentially with deionized water and anhydrous ethanol.

4. The method for enhancing the activity of anaerobic sludge in organic wastewater according to claim 2, characterized in that: In step (1), the molar ratio of S to Fe in sodium sulfide nonahydrate and ferric chloride hexahydrate is (0.2-0.6):1; the washing is carried out sequentially with deionized water and anhydrous ethanol; the drying temperature is 55-65℃ and the drying time is 6-12h.

5. The method for enhancing the activity of anaerobic sludge in organic wastewater according to claim 1, characterized in that: In step (2), the concentration of the humic acid solution is 1.0-1.2 g / L; the stirring speed is 300-350 rpm and the stirring time is 5-6 h; the washing is carried out sequentially with deionized water and anhydrous ethanol; the drying temperature is 40-45℃ and the drying time is 6-10 h; in step (1), the dropping rate of sodium sulfide is 0.5-1.0 mL / min.

6. The method for enhancing the activity of anaerobic sludge in organic wastewater according to claim 1, characterized in that: The concentration of the anaerobic activated sludge is 4–6 g / L; the dosage of the sulfur-doped nano-zero-valent iron material based on humic acid coating is 0.3–0.6 g / L.

7. The method for enhancing the activity of anaerobic sludge in organic wastewater according to claim 1, characterized in that: The temperature for the anaerobic biological treatment is 34-36℃.

Citation Information

Patent Citations

  • Method for rapidly starting dye-organic wastewater anaerobic co-metabolism system based on S-nZVI

    CN119390239A