Package structure with air-tight cavity and packaging method thereof
By forming an oxide layer on the surface of a semiconductor wafer and performing permanent bonding, combined with dry and wet etching techniques, the size, weight, and cost issues of the packaging structure are solved, achieving a low-roughness hermetic cavity and electromagnetic shielding, which is suitable for high-efficiency packaging of uncooled infrared detectors and radio frequency microsystems.
Patent Information
- Application Number
- CN202510776899.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-11
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-06-11
AI Technical Summary
In the existing technology, the packaging structure of uncooled infrared detectors and radio frequency microsystems has high size, weight and power consumption, high cost and low production efficiency, and the bottom roughness of the hermetic cavity prepared by deep silicon etching technology does not meet the requirements of high transmittance and high uniformity.
By forming an oxide layer on the surface of a semiconductor wafer and performing permanent bonding, combined with dry and wet etching techniques, a low-roughness, hermetic cavity is formed. An electromagnetic shielding layer is introduced during the packaging process to reduce the package volume and increase the package density.
It achieves a miniaturized, low-cost packaging structure, reducing packaging cycle and cost, making it suitable for mass production, and meeting the high transmittance and electromagnetic shielding requirements of uncooled infrared detectors and radio frequency microsystems.
Smart Images

Figure CN120651780B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor packaging technology, and in particular to a packaging structure with an airtight cavity and a packaging method thereof. Background Technology
[0002] In the field of uncooled infrared detectors, uncooled infrared focal plane detectors can operate at room temperature and offer numerous advantages such as fast start-up, low power consumption, small size, light weight, long lifespan, and low cost. Their cost-effectiveness is significantly better than cooled detectors, leading to their application in various fields including security, industry, medical, power, construction, and automotive. In the field of radio frequency microsystems, the development of modern military electronic equipment has placed demands on miniaturization, multifunctionality, and reconfigurability in transceiver and processing subsystems, resulting in increasingly complex micromodule functions. The development of modern military electronic equipment has created further demands for miniaturization, multifunctionality, and reconfigurability in transceiver and processing subsystems, leading to increasingly complex micromodule functions.
[0003] Chip packaging is a crucial step in the integrated circuit chip manufacturing process. For uncooled infrared detectors, the detector chip needs to operate in a high-vacuum environment. Currently, metal or ceramic packages are mainly used, resulting in higher overall size, weight, and power consumption, which cannot meet the miniaturization requirements of the market. Furthermore, the packaging cost is high and the production efficiency is low, making it unsuitable for large-scale, low-cost production. Due to the high transmittance requirements of uncooled infrared detectors, the roughness and hermeticity requirements of the light-emitting surface of the hermetic cavity are extremely stringent. However, the existing deep silicon etching technology produces hermetic cavities with high bottom roughness, for example, greater than 100nm, which does not meet the product requirements of high transmittance and high uniformity for uncooled infrared detectors, such as in the 8μm to 14μm wavelength range.
[0004] In the field of radio frequency microsystems, it is difficult to meet the requirements of circuit complexity and high integration density by integrating chips in three dimensions and setting electromagnetic shielding caps on the outside of the integrated structure. Summary of the Invention
[0005] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a packaging structure with an airtight cavity and a packaging method thereof, to solve the problems in the prior art for packaging structures with airtight cavities, such as uncooled infrared detectors, where the packaging size, weight and power consumption of metal or ceramic shells are relatively high, the packaging cost is high and the production efficiency is low, while the airtight cavity prepared by deep silicon etching technology has high bottom roughness and does not meet product requirements.
[0006] To achieve the above and other related objectives, the present invention provides a packaging method for a packaging structure with an airtight cavity, the packaging method comprising:
[0007] A first semiconductor wafer and a second semiconductor wafer having opposite first and second sides are provided;
[0008] A first oxide layer is formed on a first side surface of the first semiconductor wafer, and a second oxide layer is formed on a first side surface of the second semiconductor wafer; wherein the material of the first oxide layer is an oxide of a semiconductor material based on the first semiconductor wafer, and the material of the second oxide layer is an oxide of a semiconductor material based on the second semiconductor wafer;
[0009] The first oxide layer and the second oxide layer are permanently bonded to achieve permanent bonding between the first semiconductor wafer and the second semiconductor wafer;
[0010] Thin the first semiconductor wafer to the required thickness from the second side surface;
[0011] Dry etching is performed downward from a predetermined area on the second side surface of the first semiconductor wafer to form a first cavity penetrating the first semiconductor wafer;
[0012] The first oxide layer and the second oxide layer exposed in the first cavity are removed by wet etching to form the second cavity;
[0013] A bonding metal pad is formed on the second side of the first semiconductor wafer outside the second cavity;
[0014] A device structure with a bonding metal layer formed on its surface is provided, and the bonding metal layer is bonded to the bonding metal pads to form an airtight cavity between the second cavity and the device structure.
[0015] Optionally, the first semiconductor wafer is a silicon wafer, the second semiconductor wafer is a silicon wafer, the first oxide layer is a silicon oxide layer, and the second oxide layer is a silicon oxide layer.
[0016] Furthermore, the first semiconductor wafer is etched using a Bosch process to form the first cavity; the wet etching solution used to form the second cavity includes hydrofluoric acid.
[0017] Optionally, the bonding metal pads are formed using a vapor deposition process or an electroplating process.
[0018] Optionally, the bonding metal layer and the bonding metal pad are bonded in the form of chip-to-chip bonding, chip-to-wafer bonding, or wafer-to-wafer bonding.
[0019] Optionally, the method of forming the first cavity through the first semiconductor wafer includes:
[0020] A hard mask layer is formed on the second side surface of the first semiconductor wafer;
[0021] A photoresist layer is formed on the surface of the hard mask layer and then patterned.
[0022] After dry etching the hard mask layer based on the patterned photoresist layer, the patterned photoresist layer is removed to obtain the patterned hard mask layer;
[0023] After dry etching the first semiconductor wafer based on the patterned hard mask layer, the patterned hard mask layer is removed to obtain the first cavity.
[0024] Optionally, after forming the second cavity and before forming the bonding metal pad, the method further includes: sequentially forming an insulating dielectric layer and an electromagnetic shielding layer on the bottom wall and side wall of the second cavity and on the second side surface of the first semiconductor wafer.
[0025] Furthermore, the insulating dielectric layer is made of an oxide of semiconductor material based on the first semiconductor wafer, and is formed using a CVD process; the electromagnetic shielding layer is a stack of tantalum material layer and copper material layer, and is formed using a PVD process.
[0026] Optionally, before permanently bonding the first oxide layer to the second oxide layer, a surface CMP grinding step is performed on the bonding surfaces of the first oxide layer and the second oxide layer.
[0027] The present invention also provides a packaging structure with a hermetically tight cavity, wherein the packaging structure comprises, along its thickness direction, the following components in sequence: a device structure, a first semiconductor layer, a first oxide layer, a second oxide layer, a hermetically tight cavity, and a second semiconductor layer; wherein,
[0028] The device structure is bonded to the bonding metal pads on the first semiconductor layer via a bonding metal layer on its surface.
[0029] The first semiconductor layer and the second semiconductor layer are permanently bonded together through the first oxide layer and the second oxide layer;
[0030] The airtight cavity penetrates the first semiconductor layer, the first oxide layer, and the second oxide layer and exposes the surface of the second semiconductor layer, and the airtight cavity is sealed between the device structure and the second semiconductor layer;
[0031] The surface roughness of the second semiconductor layer is less than 5 nm.
[0032] Optionally, the chip disposed on the device structure is an uncooled infrared detector chip.
[0033] Optionally, the chip disposed on the device structure is a radio frequency microsystem chip; the bottom wall and side wall of the hermetic cavity and the surface of the first semiconductor layer are sequentially provided with an insulating dielectric layer and an electromagnetic shielding layer.
[0034] Further, the insulating dielectric layer is a silicon oxide layer with a thickness of 0.3 μm to 0.9 μm; the electromagnetic shielding layer is a stack of a tantalum material layer and a copper material layer, and the thickness of the tantalum material layer is... The thickness of the copper material layer is
[0035] Optionally, the first semiconductor layer is a silicon layer, the second semiconductor layer is a silicon layer, the first oxide layer is a silicon oxide layer, and the second oxide layer is a silicon oxide layer; the thickness of the first semiconductor layer is 100μm to 500μm, the total thickness of the first oxide layer and the second oxide layer is 0.5μm to 3μm, and the diameter of the airtight cavity is not greater than 20mm.
[0036] Optionally, the material of the bonding metal pad includes at least one of tin, lead, aluminum and gold, and the thickness of the bonding metal pad is 2μm to 6μm.
[0037] As described above, the packaging structure and method with an hermetically tight cavity of the present invention, in the process of forming the second cavity, firstly forms oxide layers of corresponding semiconductor materials on the surfaces of the first semiconductor wafer and the second semiconductor wafer, and then permanently bonds the two oxide layers to form an oxide bonding layer. This allows the second cavity to be obtained by dry etching of the first semiconductor wafer combined with wet etching of the oxide bonding layer. Since the oxide of the corresponding semiconductor material has a high etching selectivity compared to dry etching, when the oxide of the semiconductor material is wet-etched to expose the surface of the second semiconductor wafer underneath, the damage to the surface of the second semiconductor wafer is minimal, thereby obtaining a hermetically tight cavity bottom surface with very low roughness. Furthermore, during dry etching of the first semiconductor wafer, the oxide bonding layer acts as an etching barrier, enabling the formation of first cavities of arbitrary diameter and depth, especially for large-diameter and deep first cavities. Moreover, since the oxide layer formed on the semiconductor wafer is based on the semiconductor material of the corresponding semiconductor wafer, the lattice and thermal mismatch between the two is low, reducing the likelihood of cracking and warping. Additionally, the bonding quality of the bonded oxide bonding layer is high. Finally, encapsulating the device structure within a single hermetically sealed cavity formed from semiconductor material results in a small, lightweight finished product that significantly reduces packaging cycle time and cost. Furthermore, the wafer-level packaging process is compatible with existing silicon processes, making it suitable for large-scale production applications. Attached Figure Description
[0038] Figures 1 to 10 and Figures 12 to 16 The diagram shows a cross-sectional view of each step in the packaging method for a packaging structure with an airtight cavity, as described in Embodiment 1 of the present invention.
[0039] Figure 11 Displayed as Figure 12 SEM images of a portion of the area.
[0040] Figure 17 and Figure 18 The diagram shows two examples of the encapsulation structure with an airtight cavity, representing Embodiment 2 of the present invention.
[0041] Component designation explanation
[0042] 10 First Semiconductor Wafers
[0043] 100 First side of the first semiconductor wafer
[0044] 101 The second side of the first semiconductor wafer
[0045] 11 First oxide layer
[0046] 12 Second oxide layer
[0047] 13 First cavity
[0048] 130 hard mask layers
[0049] 131 Photoresist layer
[0050] 14 Second cavity
[0051] 15 Insulating dielectric layer / electromagnetic shielding layer
[0052] 16 Bonded metal pads
[0053] 17 Device Structure
[0054] 170 bonded metal layer
[0055] 18. Airtight cavity
[0056] 19 Second Semiconductor Wafers
[0057] 190 The first side of the second semiconductor wafer
[0058] 191 The second side of the second semiconductor wafer
[0059] 20 Device Structure
[0060] 200 bonded metal layers
[0061] 21 First semiconductor layer
[0062] 210 Bond metal pad
[0063] 22 First oxide layer
[0064] 23 Second oxide layer
[0065] 24. Airtight cavity
[0066] 25 Second semiconductor layer
[0067] 26 Insulating dielectric layer / electromagnetic shielding layer Detailed Implementation
[0068] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0069] In the detailed description of embodiments of the present invention, for ease of explanation, the cross-sectional views illustrating the device structure may be partially enlarged and not to scale. Furthermore, the schematic diagrams are merely examples and should not limit the scope of protection of the present invention. In actual fabrication, the three-dimensional spatial dimensions of length, width, and depth should be included.
[0070] For ease of description, spatial relation terms such as “below,” “under,” “lower than,” “below,” “above,” and “upper” may be used herein to describe the relationship between one element or feature shown in the accompanying drawings and other elements or features. It will be understood that these spatial relation terms are intended to include directions other than those depicted in the drawings for the device in use or operation. Furthermore, when a layer is referred to as being “between” two layers, it can be the only layer between the two layers, or there may be one or more layers in between. The phrase “between” as used herein includes both endpoint values.
[0071] In the context of this application, the structure described above the first feature may include embodiments in which the first and second features are formed in direct contact, or embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.
[0072] Please see Figures 1 to 18It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the illustrations only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0073] Example 1
[0074] This embodiment provides a packaging method with a hermetically sealed cavity packaging structure. This packaging method is suitable for devices that need to operate in a vacuum-sealed environment. The packaging method includes the following steps:
[0075] S1, providing a first semiconductor wafer and a second semiconductor wafer having opposite first and second sides;
[0076] S2, a first oxide layer is formed on a first side surface of the first semiconductor wafer, and a second oxide layer is formed on a first side surface of the second semiconductor wafer; wherein, the material of the first oxide layer is an oxide of a semiconductor material based on the first semiconductor wafer, and the material of the second oxide layer is an oxide of a semiconductor material based on the second semiconductor wafer;
[0077] S3, the first oxide layer and the second oxide layer are permanently bonded to achieve permanent bonding between the first semiconductor wafer and the second semiconductor wafer;
[0078] S4, thin the first semiconductor wafer to the required thickness from the second side surface of the first semiconductor wafer;
[0079] S5, dry etching is performed downward from a predetermined area on the second side surface of the first semiconductor wafer to form a first cavity penetrating the first semiconductor wafer;
[0080] S6, wet etching is used to remove the first oxide layer and the second oxide layer exposed in the first cavity to form a second cavity;
[0081] S7, forming a bonding metal pad on the second side of the first semiconductor wafer outside the second cavity;
[0082] S8, providing a device structure with a bonding metal layer formed on its surface, and bonding the bonding metal layer to the bonding metal pad, so that the second cavity and the device structure are formed into an airtight cavity.
[0083] The packaging method for the hermetically sealed cavity structure in this embodiment first forms oxide layers of corresponding semiconductor materials on the surfaces of a first semiconductor wafer and a second semiconductor wafer during the formation of the second cavity. Then, these two oxide layers are permanently bonded together to form an oxide bonding layer. This allows the second cavity to be obtained by dry etching of the first semiconductor wafer combined with wet etching of the oxide bonding layer. Since the oxide layer of the corresponding semiconductor material has a high etching selectivity compared to dry etching, wet etching of the oxide layer exposes the underlying surface of the second semiconductor wafer with minimal damage, resulting in a hermetically sealed cavity bottom surface with very low roughness. Furthermore... During dry etching of the first semiconductor wafer, the presence of an oxide bonding layer as an etching barrier allows for the formation of first cavities of arbitrary diameter and depth, especially for large-diameter and deep first cavities. Furthermore, since the oxide layer formed on the semiconductor wafer is based on the semiconductor material of the corresponding semiconductor wafer, the lattice mismatch and thermal mismatch between the two are low, making cracking and warping less likely to occur, and the bonding quality of the bonded oxide bonding layer is high. Finally, the device structure is encapsulated in a single hermetically sealed cavity formed of semiconductor material, resulting in a small and lightweight finished product that significantly reduces the packaging cycle and cost. Moreover, the wafer-level packaging process is compatible with existing silicon processes, making it suitable for large-scale production applications.
[0084] The encapsulation method of the encapsulation structure with an airtight cavity in this embodiment will be described in detail below with reference to the specific accompanying drawings.
[0085] like Figure 1 and Figure 2 As shown, step S1 is performed first, providing a first semiconductor wafer 10 and a second semiconductor wafer 19 having opposite first and second sides; as Figure 1 The first semiconductor wafer 10 has a first side 100 and a second side 101 of the first semiconductor wafer, as shown in the figure. Figure 2 The second semiconductor wafer 19 has a first side 190 and a second side 191 of the second semiconductor wafer.
[0086] The first semiconductor wafer 10 and the second semiconductor wafer 19 are made of semiconductor materials, which may be the same or different, but preferably the same semiconductor material. Furthermore, the first semiconductor wafer 10 and the second semiconductor wafer 19 are preferably made of the same group IV elemental or compound material, such as silicon wafers, germanium wafers, silicon carbide wafers, or silicon germanide wafers. In this embodiment, it is preferred that both the first semiconductor wafer 10 and the second semiconductor wafer 19 are silicon wafers. This is because they are easily compatible with existing silicon processes in subsequent wafer-level packaging. Additionally, the silicon wafer has a high etching selectivity with the subsequently formed silicon oxide bonding layer, making it easier to obtain a low-roughness second semiconductor wafer surface during subsequent wet etching of the second cavity.
[0087] The thickness of the first semiconductor wafer 10 and the second semiconductor wafer 19 is generally relatively thick at the beginning, and the thickness will be reduced later according to actual needs.
[0088] like Figure 3 and Figure 4 As shown, step S2 is then performed, in which a first oxide layer 11 is formed on the surface of the first side 100 of the first semiconductor wafer, and a second oxide layer 12 is formed on the surface of the first side 190 of the second semiconductor wafer; wherein, the material of the first oxide layer 11 is an oxide based on the semiconductor material of the first semiconductor wafer 10, for example, when the first semiconductor wafer 10 is a silicon wafer, the first oxide layer is a silicon oxide layer, and the material of the second oxide layer 12 is an oxide based on the semiconductor material of the second semiconductor wafer 19, for example, when the second semiconductor wafer 19 is a silicon wafer, the second oxide layer is a silicon oxide layer.
[0089] The first oxide layer 11 and the second oxide layer 12 can be prepared using existing conventional processes, such as thermo-oxidation process, CVD process, sol-gel process and ALD process, etc., depending on the actual needs.
[0090] In this embodiment, both the first oxide layer 11 and the second oxide layer 12 are preferably silicon oxide layers. Furthermore, the preparation process of the first oxide layer 11 and the second oxide layer 12 is not restricted by the order of their formation, as long as they are formed on the first semiconductor wafer 10 and the second semiconductor wafer 19 respectively.
[0091] The thicknesses of the first oxide layer 11 and the second oxide layer 12 can be the same or different, as long as they can achieve permanent bonding between them. Furthermore, the total thickness of the first oxide layer 11 and the second oxide layer 12 is set according to actual needs. In this embodiment, when the first oxide layer 11 and the second oxide layer 12 are selected as silicon oxide layers, their total thickness is generally selected to be 0.5 μm to 3 μm. Further, to improve the bonding quality of the subsequent permanent bonding, the bonding surfaces of the first oxide layer 11 and the second oxide layer 12 can be CMP-polished after deposition and before bonding to improve surface smoothness.
[0092] like Figure 5 and Figure 6 As shown, step S3 is then performed to permanently bond the first oxide layer 11 and the second oxide layer 12 to achieve permanent bonding between the first semiconductor wafer 10 and the second semiconductor wafer 19.
[0093] As an example, when the first oxide layer 11 and the second oxide layer 12 are selected as silicon oxide layers, during the permanent bonding process, the hydroxyl groups (-OH) and silicon-oxygen bonds (Si-O) on the surface of silicon oxide interact through van der Waals forces and hydrogen bonds to form stable chemical bonds. Under appropriate temperature and pressure conditions, these chemical bonds are further strengthened, and finally permanent bonding is achieved.
[0094] like Figure 6 As shown, step S4 is then performed, thinning the first semiconductor wafer 101 from the second side surface 101 to the required thickness. The thickness of the first semiconductor wafer 10 after thinning is part of the depth of the subsequently formed hermetic cavity; therefore, the thickness of the first semiconductor wafer 10 after thinning is set according to the depth requirements of the hermetic cavity. The thinning process is implemented using existing conventional thinning techniques, such as first using coarse grinding to thin and then combining it with fine grinding to smooth it. However, it is not limited to this; other suitable thinning techniques can be used.
[0095] As an example, the thickness H of the first semiconductor wafer 10 after thinning (e.g.) Figure 10 (As shown) is 100μm~500μm.
[0096] like Figure 10 As shown, step S5 is then performed, where dry etching is performed downwards from a predetermined area on the second side 101 surface of the first semiconductor wafer 10 to form a first cavity 13 penetrating the first semiconductor wafer 10. The diameter of the first cavity 13 can be set according to actual needs. Based on the packaging method of this embodiment, the diameter D of the first cavity 13 can be up to 20mm.
[0097] During the dry etching process in this step, since the first oxide layer 11 is located below the first semiconductor wafer 10, the first oxide layer 11 can serve as an etching barrier layer in the dry etching process. There is no need to consider the damage to the surface of the first oxide layer 11 during the dry etching process. Therefore, it is easy to obtain a first cavity 13 with a large diameter range and good verticality.
[0098] As an example, when the first semiconductor wafer 10 in this embodiment is selected as a silicon wafer, the first semiconductor wafer 10 can be etched using the Bosch process.
[0099] As a specific example, a method for forming the first cavity 13 penetrating the first semiconductor wafer 10 includes:
[0100] like Figure 7 As shown, in step S51, a hard mask layer 130, such as a silicon oxide hard mask layer, is formed on the surface of the second side 101 of the first semiconductor crystal 10.
[0101] like Figure 7 and Figure 8 As shown, in step S52, a photoresist layer 131 is formed on the surface of the hard mask layer 130 and patterned to form a patterned photoresist layer 131.
[0102] like Figure 9 As shown, in step S53, the hard mask layer 130 is dry-etched based on the patterned photoresist layer 131 and then the patterned photoresist layer 131 is removed to obtain the patterned hard mask layer 130.
[0103] like Figure 9 and Figure 10 As shown, after dry etching the first semiconductor wafer 10 based on the patterned hard mask layer 130, the patterned hard mask layer 130 is removed to obtain the first cavity 13.
[0104] like Figure 12 As shown, step S6 is then performed, where wet etching is used to remove the first oxide layer 11 and the second oxide layer 12 exposed in the first cavity 13, forming the second cavity 14. Based on the high etching selectivity of wet etching, the surface roughness of the exposed second semiconductor wafer 19 can be effectively reduced.
[0105] like Figure 11The image shows a SEM image of the surface of the second semiconductor wafer 19 exposed in the second cavity 14 when both the first semiconductor wafer 11 and the second semiconductor wafer 19 are silicon wafers. Point A in the image represents the exposed surface of the second semiconductor wafer 19, with a surface roughness of less than 5 nm. In optimal conditions, the surface roughness can reach less than 1 nm, which fully meets the surface roughness requirements for the hermetic cavity of an uncooled infrared detector. Furthermore, when the first oxide layer 11 and the second oxide layer 12 are silicon oxide layers, hydrofluoric acid is generally chosen as the wet etching solution. Hydrofluoric acid has a very high selectivity for etching silicon oxide to silicon, typically ranging from 100:1 to 1000:1, thus allowing for the removal of the silicon oxide layer with minimal damage.
[0106] As another specific example, the packaging method of this embodiment can be applied to the packaging of uncooled infrared detector chips. For uncooled infrared detector chips, the bottom roughness of the hermetic cavity is the main factor affecting the light transmittance. The packaging method of this embodiment can effectively reduce the bottom roughness of the hermetic cavity (i.e., the second cavity 14). As shown above, for silicon wafers and silicon oxide layers, the bottom roughness of the formed second cavity 14 is less than 5nm, the depth of the first cavity 13 can reach 100μm to 500μm, and the transmittance of infrared wavelengths from 8μm to 14μm can reach more than 90%.
[0107] As another specific example, the packaging method of this embodiment can also be applied to the packaging of radio frequency (RF) microsystem chips. RF microsystem chips generally require electromagnetic shielding. Typically, this is achieved by placing an electromagnetic shielding cap on the external structure of the package after packaging the RF microsystem chip. However, this results in a large overall structure volume, limited selection of electromagnetic shielding materials, and unfavorable packaging density. In this embodiment, the electromagnetic shielding function of the RF microsystem chip can be achieved using the airtight cavity formed by the second cavity. This is achieved by sequentially forming an insulating dielectric layer / electromagnetic shielding layer 15 (e.g., ...) on the bottom and side walls of the second cavity 14 and the second side surface of the first semiconductor wafer 10. Figure 13As shown in the diagram, since the electromagnetic shielding layer can be formed directly during the packaging process, it is essentially embedded within the package, effectively reducing the package volume and complexity, and facilitating package density. Furthermore, since the electromagnetic shielding layer can be prepared using conventional deposition processes, the choice of electromagnetic shielding material can be diversified. Finally, due to the low roughness at the bottom of the second cavity 14, the continuity of the insulating dielectric layer / electromagnetic shielding layer 15 formed thereon is good, meaning the electromagnetic shielding layer has strong adhesion, improving the reliability of the electromagnetic shielding layer 15. Preferably, the insulating dielectric layer in the insulating dielectric layer / electromagnetic shielding layer 15 is an oxide of a semiconductor material based on the first semiconductor wafer, and is formed using a CVD process, with a thickness typically selected to be 0.3 μm to 0.9 μm. The electromagnetic shielding layer is a stack of a tantalum material layer and a copper material layer, and is formed using a PVD process, with a thickness typically selected as follows: the thickness of the tantalum material layer is... The thickness of the copper material layer is
[0108] like Figure 14 and Figure 15 As shown, where Figure 14 The illustration shows the case where the bottom and side walls of the second cavity 14 and the second side surface of the first semiconductor wafer 10 are formed with an insulating dielectric layer / electromagnetic shielding layer 15. Figure 15 The diagram shows the case where the bottom wall and side wall of the second cavity 14 and the second side surface of the first semiconductor wafer 10 are not formed with an insulating dielectric layer / electromagnetic shielding layer 15. Then, step S7 is performed to form a bonding metal pad 16 on the second side of the first semiconductor wafer 10 outside the second cavity 14.
[0109] As an example, the bonding metal pad 16 is formed using a vapor deposition process, but it is not limited to this; other suitable processes are also possible, such as electroplating. Specifically, the vapor deposition process includes: first forming a photoresist layer on the surface of the resulting structure; then patterning the photoresist layer to form a patterned photoresist layer; next, vapor-depositing a bonding metal pad layer on one side of the patterned photoresist layer; and finally removing the patterned photoresist layer and the vapor-deposited bonding metal pad layer thereon, leaving the bonding metal pad layer on the first semiconductor wafer 10 as the bonding metal pad 16. The material of the bonding metal pad 16 can be selected as at least one of tin, lead, aluminum, and gold, but it is not limited to this; other suitable pad materials are also possible, and its thickness is selected to be 2μm to 6μm.
[0110] like Figure 16As shown, the final step, S8, involves providing a device structure 17 with a bonding metal layer 170 formed on its surface, and bonding the bonding metal layer 170 to the bonding metal pad 16, thereby forming an airtight cavity 18 between the second cavity 14 and the device structure 17. It should be noted here that... Figure 16 This illustration is based on the example where the bottom and side walls of the second cavity 14 and the second side surface of the first semiconductor wafer 10 do not have an insulating dielectric layer / electromagnetic shielding layer 15. In this case, if a chip is disposed on the device structure 17 within the airtight cavity 18, the chip is suitable to be an uncooled infrared detector chip; when the chip disposed on the device structure 17 is a radio frequency microsystem chip, such as... Figure 14 As shown, an insulating dielectric layer / electromagnetic shielding layer 15 will be formed on the bottom wall and side wall of the second cavity 14 and the second side surface of the first semiconductor wafer 10, as mentioned above, and will not be repeated here.
[0111] As an example, the bonding metal layer 170 and the bonding metal pad 16 in this step can be bonded in the form of chip-to-chip bonding, chip-to-wafer bonding, or wafer-to-wafer bonding. Specifically: when the bonding form is chip-to-chip bonding, the device structure 17 is provided in chip form, and the resulting structure is also cut into chip form after step S7, thereby achieving chip-to-chip bonding in the bonding process of this step; when the bonding form is chip-to-wafer bonding, the device structure 17 is provided in chip form, thereby achieving chip-to-wafer bonding in the bonding process of this step; when the bonding form is wafer-to-wafer bonding, the device structure 17 is provided in wafer form, thereby achieving wafer-to-wafer bonding in the bonding process of this step.
[0112] The material of the bonding metal layer 170 can be any material suitable for metal bonding, such as titanium, platinum, gold, etc., depending on the actual needs.
[0113] Example 2
[0114] This embodiment provides a packaging structure with an airtight cavity. This packaging structure can be obtained by the packaging method described in Embodiment 1. The beneficial effects it achieves can be found in the description of Embodiment 1, and will not be repeated below. Figure 17 and Figure 18 As shown, the packaging structure, along its thickness direction, sequentially includes: a device structure 20, a first semiconductor layer 21, a first oxide layer 22, a second oxide layer 23, a hermetically tight cavity 24, and a second semiconductor layer 25; wherein,
[0115] The device structure 20 is bonded to the bonding metal pad 210 on the first semiconductor layer 21 via a bonding metal layer 200 on its surface.
[0116] The first semiconductor layer 21 and the second semiconductor layer 25 are permanently bonded together through the first oxide layer 22 and the second oxide layer 23;
[0117] The airtight cavity 24 penetrates the first semiconductor layer 21, the first oxide layer 22 and the second oxide layer 23 and exposes the surface of the second semiconductor layer 25, and the airtight cavity 24 is sealed between the device structure 20 and the second semiconductor layer 25.
[0118] The surface roughness of the second semiconductor layer 25 is less than 5 nm, which mainly refers to the surface facing the hermetic cavity 24.
[0119] like Figure 17 As shown, as a specific example, if a chip is provided on the device structure 17 inside the airtight cavity 18, the chip provided on the device structure 20 is an uncooled infrared detector chip.
[0120] like Figure 18 As shown, as another specific example, if a chip is disposed on the device structure 17 within the hermetically sealed cavity 18, and the chip disposed on the device structure 20 is a radio frequency microsystem chip, then an insulating dielectric layer / electromagnetic shielding layer 26 is sequentially disposed on the bottom wall and side walls of the hermetically sealed cavity 24 and on the surface of the first semiconductor layer 21. Preferably, the insulating dielectric layer in the insulating dielectric layer / electromagnetic shielding layer 26 is a silicon oxide layer with a thickness of 0.3 μm to 0.9 μm; the electromagnetic shielding layer is a stack of a tantalum material layer and a copper material layer, and the thickness of the tantalum material layer is... The thickness of the copper material layer is
[0121] The first semiconductor layer 21 and the second semiconductor layer 25 are made of semiconductor materials, which may be the same or different, but preferably the same semiconductor material. Furthermore, the first semiconductor layer 21 and the second semiconductor layer 25 are preferably made of the same Group IV elemental or compound material, such as silicon, germanium, silicon carbide, or silicon germanide. In this embodiment, the first semiconductor layer 21 and the second semiconductor layer 25 are preferably both silicon layers, the first oxide layer 22 is a silicon oxide layer, the second oxide layer 23 is a silicon oxide layer, the thickness of the first semiconductor layer 21 is 100μm to 500μm, the total thickness of the first oxide layer 22 and the second oxide layer 23 is 0.5μm to 3μm, and the diameter of the hermetic cavity 24 is no greater than 20mm.
[0122] As an example, the bonding metal pad 210 is made of at least one of tin, lead, aluminum, and gold, and the thickness of the bonding metal pad 210 is 2 μm to 6 μm. The bonding metal layer 170 is made of at least one of titanium, platinum, and gold.
[0123] In summary, this invention provides a packaging structure and method with an hermetically tight cavity. In forming the second cavity, oxide layers of corresponding semiconductor materials are first formed on the surfaces of a first semiconductor wafer and a second semiconductor wafer. These two oxide layers are then permanently bonded together to form an oxide bonding layer. This allows the second cavity to be obtained by dry etching of the first semiconductor wafer combined with wet etching of the oxide bonding layer. Since the oxide layer of the corresponding semiconductor material has a high etching selectivity compared to dry etching, wet etching of the oxide layer exposes the underlying surface of the second semiconductor wafer with minimal damage to the second semiconductor wafer surface. This results in a hermetically tight cavity bottom surface with very low roughness. Furthermore, during dry etching of the first semiconductor wafer, the oxide bonding layer acts as an etching barrier, enabling the formation of first cavities of arbitrary diameter and depth, especially for large-diameter, deep first cavities. Moreover, since the oxide layer formed on the semiconductor wafer is based on the semiconductor material of the corresponding semiconductor wafer, the lattice and thermal mismatch between the two is low, reducing the likelihood of cracking and warping. Additionally, the bonding quality of the bonded oxide bonding layer is high. Finally, encapsulating the device structure within a single hermetically sealed cavity formed of semiconductor material results in a small, lightweight finished product that significantly reduces packaging cycle time and cost. Furthermore, the wafer-level packaging process is compatible with existing silicon processes, making it suitable for large-scale production applications. Therefore, this invention effectively overcomes the various shortcomings of existing technologies and possesses high industrial applicability.
[0124] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A packaging method for a packaging structure with an airtight cavity, characterized in that, The encapsulation method includes: Provides a first semiconductor wafer and a second semiconductor wafer having opposite first and second sides; A first oxide layer is formed on a first side surface of the first semiconductor wafer, and a second oxide layer is formed on a first side surface of the second semiconductor wafer; wherein the material of the first oxide layer is an oxide of a semiconductor material based on the first semiconductor wafer, and the material of the second oxide layer is an oxide of a semiconductor material based on the second semiconductor wafer; The first oxide layer and the second oxide layer are permanently bonded to achieve permanent bonding between the first semiconductor wafer and the second semiconductor wafer; Thinning the first semiconductor wafer to the required thickness from the second side surface; Dry etching is performed downward from a predetermined area on the second side surface of the first semiconductor wafer to form a first cavity penetrating the first semiconductor wafer; The first oxide layer and the second oxide layer exposed in the first cavity are removed by wet etching to form a second cavity, wherein the surface roughness of the second semiconductor wafer exposed in the second cavity is less than 1 nm; then, an insulating dielectric layer and an electromagnetic shielding layer are sequentially formed on the bottom wall and side wall of the second cavity and on the second side surface of the first semiconductor wafer. A bonding metal pad is formed on the second side of the first semiconductor wafer outside the second cavity; A device structure with a bonding metal layer formed on its surface is provided, and the bonding metal layer is bonded to the bonding metal pads to form an airtight cavity between the second cavity and the device structure.
2. The packaging method for the packaging structure with an airtight cavity according to claim 1, characterized in that: The first semiconductor wafer is a silicon wafer, the second semiconductor wafer is a silicon wafer, the first oxide layer is a silicon oxide layer, and the second oxide layer is a silicon oxide layer.
3. The packaging method for the packaging structure with an airtight cavity according to claim 2, characterized in that: The first semiconductor wafer is etched using the Bosch process to form the first cavity; The wet etching solution used to form the second cavity includes hydrofluoric acid.
4. The packaging method for the packaging structure with an airtight cavity according to claim 1, characterized in that: The bonding metal pads are formed using a vapor deposition process or an electroplating process.
5. The packaging method for the packaging structure with an airtight cavity according to claim 1, characterized in that: The bonding metal layer and the bonding metal pad are bonded in the form of chip-to-chip bonding, chip-to-wafer bonding, or wafer-to-wafer bonding.
6. The packaging method for the packaging structure with an airtight cavity according to claim 1, characterized in that, The method of forming the first cavity penetrating the first semiconductor wafer includes: A hard mask layer is formed on the second side surface of the first semiconductor wafer; A photoresist layer is formed on the surface of the hard mask layer and then patterned. After dry etching the hard mask layer based on the patterned photoresist layer, the patterned photoresist layer is removed to obtain the patterned hard mask layer; After dry etching the first semiconductor wafer based on the patterned hard mask layer, the patterned hard mask layer is removed to obtain the first cavity.
7. The packaging method for the packaging structure with an airtight cavity according to claim 1, characterized in that: The insulating dielectric layer is made of an oxide of semiconductor material based on the first semiconductor wafer and is formed using a CVD process; the electromagnetic shielding layer is a stack of tantalum material layer and copper material layer and is formed using a PVD process.
8. The packaging method for the packaging structure with an airtight cavity according to claim 1, characterized in that: Before permanently bonding the first oxide layer to the second oxide layer, a surface CMP grinding step is performed on the bonding surfaces of the first oxide layer and the second oxide layer.
9. A packaging structure with an airtight cavity, characterized in that, The packaging structure, along its thickness direction, sequentially comprises: a device structure, a first semiconductor layer, a first oxide layer, a second oxide layer, an hermetically sealed cavity, and a second semiconductor layer; wherein, The device structure is bonded to the bonding metal pads on the first semiconductor layer via a bonding metal layer on its surface; wherein, the chip disposed on the device structure is a radio frequency microsystem chip; the bottom wall and side wall of the hermetic cavity and the surface of the first semiconductor layer are sequentially provided with an insulating dielectric layer and an electromagnetic shielding layer. The first semiconductor layer and the second semiconductor layer are permanently bonded together through the first oxide layer and the second oxide layer; The airtight cavity penetrates the first semiconductor layer, the first oxide layer, and the second oxide layer and exposes the surface of the second semiconductor layer, and the airtight cavity is sealed between the device structure and the second semiconductor layer; The surface roughness of the second semiconductor layer is less than 1 nm.
10. The packaging structure with an airtight cavity according to claim 9, characterized in that: The insulating dielectric layer is a silicon oxide layer with a thickness of 0.3 μm to 0.9 μm; the electromagnetic shielding layer is a stack of tantalum material layer and copper material layer, with the tantalum material layer having a thickness of 200 Å to 0.14 μm and the copper material layer having a thickness of 800 Å to 2 μm.
11. The packaging structure with an airtight cavity according to claim 9, characterized in that: The first semiconductor layer is a silicon layer, the second semiconductor layer is a silicon layer, the first oxide layer is a silicon oxide layer, and the second oxide layer is a silicon oxide layer; the thickness of the first semiconductor layer is 100μm~500μm, the total thickness of the first oxide layer and the second oxide layer is 0.5μm~3μm, and the diameter of the airtight cavity is no greater than 20mm.
12. The packaging structure with an airtight cavity according to claim 9, characterized in that: The bonding metal pad is made of at least one of tin, lead, aluminum and gold, and the thickness of the bonding metal pad is 2μm to 6μm.
Citation Information
Patent Citations
Wafer level packaging method and packaging structure
CN110875199A
Wafer level packaging method of non-refrigeration detector, non-refrigeration detector and preparation method of non-refrigeration detector