Positive electrode active material, method for producing the same, and battery
By forming a polyanionic coating layer on the surface of the layered oxide core, the problem of structural phase transition of the layered oxide sodium cathode active material under high voltage is solved, thereby improving the high-voltage cycle stability and safety and enhancing battery performance.
Patent Information
- Application Number
- CN202510898287.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-06-30
AI Technical Summary
Layered oxide sodium cathode active materials undergo severe structural phase transitions under high voltage, resulting in insufficient cycle stability and safety, which affects battery performance.
A polyanionic material coating layer is formed on the surface of the layered oxide core, and it is tightly bonded by appropriate sintering treatment to form the first positive electrode active material. The polyanionic material fills the gaps, improving the structural stability and safety.
It improves the high-voltage cycle stability and safety of the positive electrode active material, reduces the rate of increase of the battery's DC internal resistance, and enhances the battery's volumetric energy density and rate performance.
Smart Images

Figure CN120657110B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of sodium-ion batteries, specifically to positive electrode active materials and their preparation methods, and batteries. Background Technology
[0002] In recent years, sodium-ion batteries have seen rapid development in start-stop power supplies, two-wheeled vehicles, and energy storage due to their advantages such as similar working principle to lithium-ion batteries, low raw material cost, and compatibility with existing lithium battery cathode production lines.
[0003] Sodium-ion layered oxides, due to their high theoretical capacity, were among the first sodium-ion battery cathode active materials studied and applied. However, layered oxide materials are prone to structural phase transitions during high-voltage charge-discharge processes, exhibiting poor cycle stability. Furthermore, layered oxides suffer from poor thermal stability and insufficient safety. Therefore, the current use of layered oxides as cathode active materials in sodium-ion batteries still presents numerous challenges that require improvement.
[0004] It should be noted that the above statements are only used to provide background information related to this application and do not necessarily constitute prior art. Summary of the Invention
[0005] In a first aspect, this application proposes a positive electrode active material for sodium secondary batteries, comprising: a first positive electrode active material, the first positive electrode active material comprising a core, the core comprising a layered oxide, a coating layer, the coating layer being located at least on a portion of the surface of the core, the coating layer comprising a polyanionic material; and a second positive electrode active material, the second positive electrode active material comprising the polyanionic material; wherein the peak intensity of the XRD diffraction peak of the positive electrode active material is I within a 2θ diffraction angle of 16.6°±0.5°. (003) The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 15.9°±0.3° is I. (011) The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 41.5°±0.5° is I. (104) 0.5≤I A ≤0.7, 0.02≤I B ≤0.05, where I A =I (003) / (I (003) +I (104) ), I B =I (011) / (I (011) +I (104)Thus, the polyanionic material forms a coating layer on the surface of the layered oxide core, allowing the polyanionic material to bond tightly with the layered oxide to form the first positive electrode active material. At the same time, the polyanionic material also fills the gaps between the first positive electrode active materials. The positive electrode active material has high structural stability and can play a synergistic role over a long period of time. During charge and discharge cycles, the rate of increase of the battery's DC internal resistance (DCR) is significantly reduced, thereby improving the battery's high-voltage cycle stability and safety.
[0006] In some embodiments, the mass ratio of the polyanionic material to the layered oxide in the positive electrode active material is (0.01-1):1; optionally, (0.10-0.45):1. This facilitates the formation of a relatively uniform coating layer of the polyanionic material on the surface of the layered oxide while simultaneously embedding it into the voids surrounding the first positive electrode active material, further improving the structural stability of the positive electrode active material.
[0007] In some embodiments, the Dv50 particle size of the layered oxide is 3 μm-10 μm; optionally, 4 μm-9 μm; further, 5 μm-8 μm; and / or, the Dv50 particle size of the polyanionic material is 0.5 μm-1.0 μm; optionally, 0.6 μm-0.9 μm; further, 0.7 μm-0.8 μm. This is beneficial for increasing the compaction density of the positive electrode active material, thereby improving the volumetric energy density of the battery.
[0008] In some embodiments, the particle size distribution SPAN of the layered oxide is 1.1-1.3; optionally, 1.2-1.4; and / or, the particle size distribution SPAN of the polyanionic material is 3-4; optionally, 3.3-3.7. Thus, by grading particles of different sizes, the compaction density of the positive electrode active material is further improved.
[0009] In some embodiments, the Dv50 particle size of the positive electrode active material is 3μm-10μm; optionally, 5μm-8μm; further, 5μm-7μm. This is beneficial for improving the compaction density of the positive electrode active material.
[0010] In some embodiments, the particle size distribution (SPAN) of the positive electrode active material is 1.5-2.5; optionally, 1.8-2.2. This facilitates a denser packing of the positive electrode active material particles, thereby further improving the volumetric energy density of the sodium-ion battery.
[0011] In some embodiments, the specific surface area of the positive electrode active material is 1 m². 2 / g-7m 2 / g. This can improve the dispersion uniformity of the positive electrode active material in the positive electrode slurry and improve processing performance.
[0012] In some embodiments, the compaction density of the positive electrode active material is 3.1 g / cm³. 3 -3.4g / cm 3 This is beneficial for improving the volumetric energy density of sodium-ion batteries and enhancing their capacity utilization.
[0013] In some embodiments, the layered oxide satisfies the chemical formula: Na a1 (Ni x1 Fe y1 Mn z1 M' n1 O2, wherein 0.90≤a1≤1.10, 0≤x1≤0.5, 0≤y1≤0.5, 0≤z1≤0.5, 0≤n1≤0.3, x1+y1+z1+n1=1, and M' includes at least one of Sn, Ce, La, Co, Ca, Cu, Sr, Y, Ti, V, Mg, B, Cr, Sb, Al, Zn, Zr, Nb, W, and Li. This is beneficial for improving the structural stability and specific capacity of the positive electrode active material.
[0014] In some embodiments, a1:(x1+y1+z1+n1)=(0.90-1.05):1; optionally, (0.95-1.05):1; further, (0.97-1.03):1; and / or, 0<n1≤0.02. This is beneficial for further improving the specific capacity of the positive electrode active material.
[0015] In some embodiments, the polyanionic material satisfies the chemical formula: Na₄Fe 3-x M x (PO4)2(P2O7) / C, where 0≤x≤0.3, and M includes at least one of Mn, Co, Ni, Ti, Cu, and V. This is beneficial for improving the safety of the positive electrode active material.
[0016] In a second aspect of this application, a method for preparing the aforementioned positive electrode active material is proposed, comprising: mixing and grinding a sodium source, an iron source, a phosphorus source, and an M' source to obtain an intermediate; mixing the intermediate with a carbon source and performing a first sintering treatment under a nitrogen atmosphere to obtain a polyanionic material; mixing a sodium source, a precursor, and an M' source and performing a second sintering treatment under an oxidizing atmosphere to obtain a layered oxide; and mixing the polyanionic material with the layered oxide material and performing a third sintering treatment under a nitrogen atmosphere, wherein the temperature of the third sintering treatment is less than 500°C, to obtain the positive electrode active material. Thus, by using appropriate sintering treatment, a tight bond between the polyanionic material and the layered oxide can be achieved, resulting in a positive electrode active material with superior high-voltage cycle stability and safety. The process is simple and easy to implement for industrial production.
[0017] In some embodiments, the temperature of the third sintering treatment is 100℃-500℃; optionally, 200℃-400℃; and / or, the time of the third sintering treatment is 3h-10h; optionally, 4h-8h; and / or, the heating rate of the third sintering treatment is 0.5℃ / min-5℃ / min, optionally, 1℃ / min-3℃ / min. This is beneficial for improving the interfacial bonding strength between the polyanionic material and the layered oxide in the positive electrode active material, thereby enhancing the electron conduction and ion diffusion efficiency between particles and improving rate performance.
[0018] In some embodiments, the temperature of the first sintering treatment is 400℃-700℃, and the time is 8h-12h; and / or, the temperature of the second sintering treatment is 900℃-1100℃, and the time is 8h-15h. This facilitates obtaining polyanionic materials and layered oxides that meet the aforementioned particle size requirements.
[0019] In some embodiments, the sodium source includes at least one of sodium carbonate, sodium dihydrogen phosphate, sodium hydroxide, sodium nitrate, and sodium oxide; and / or, the iron source includes at least one of Fe2O3, FeC2O4, FeSO4, FeCl3, and Fe(NO3)3; and / or, the phosphorus source includes at least one of (NH4)2HPO4, H3PO4, and NH4H2PO4; and / or, the M source includes at least one of oxides, carbonates, phosphates, fluorides, chlorides, hydroxides, and silicides of element M; and / or, the carbon source includes at least one of glucose, sucrose, citric acid, and oxalic acid; and / or, the precursor includes (Ni x1 Fe y1 Mn z1 )OOH、(Ni x1 Fe y1 Mn z1 At least one of (OH)2; and / or, the M' source includes at least one of the oxides, carbonates, phosphates, fluorides, chlorides, hydroxides, and silicides of the M' element. Therefore, the raw material sources are wide-ranging, facilitating large-scale application.
[0020] In a third aspect, this application proposes a battery comprising a positive electrode sheet, said positive electrode sheet comprising the aforementioned positive electrode active material, or a positive electrode active material prepared by the aforementioned method. Thus, this battery possesses all the features and advantages of the aforementioned positive electrode active material and its preparation method, which will not be elaborated further here. Attached Figure Description
[0021] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0022] Figure 1 This is a SEM image of the polyanionic material prepared in Example 1 of this application.
[0023] Figure 2 This is an SEM image of the layered oxide prepared in Example 1 of this application.
[0024] Figure 3 This is a SEM image of the positive electrode active material prepared in Example 1 of this application.
[0025] Figure 4 The image shows the XRD pattern of the polyanionic material prepared in Example 1 of this application.
[0026] Figure 5 The image shows the XRD pattern of the layered oxide prepared in Example 1 of this application.
[0027] Figure 6 The image shows the XRD pattern of the positive electrode active material prepared in Example 1 of this application.
[0028] Figure 7 The graph shows the DSC test curve of a half-cell assembled from the polyanionic material, layered oxide and positive electrode active material prepared in Example 1 of this application, charged to 4.15V, and the positive electrode sheet removed. Detailed Implementation
[0029] The embodiments of this application are described in detail below, with examples of these embodiments shown in the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0030] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used in this application is for the purpose of describing particular embodiments only and is not intended to limit this application; unless otherwise stated, the values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this application).
[0031] The terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are open-ended expressions, meaning they include what is specified in this application but do not exclude other aspects.
[0032] In the description of this application, all figures disclosed herein, whether or not the words "approximately" or "about" are used, are approximate values. Each figure may vary by less than 10% or by a difference that is considered reasonable by one of the art, such as 1%, 2%, 3%, 4%, or 5%.
[0033] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0034] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. "First feature" and "second feature" may include one or more of the indicated feature.
[0035] In the description of this application, "A and / or B" can include any of the cases of A alone, B alone, or A and B, where A and B are merely examples and can be any technical feature connected by "and / or" in this application.
[0036] In this application, the order in which the steps are written does not imply a strict execution order and does not limit the implementation process. The specific execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps in this application can be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0037] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0038] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0039] To address the issues of poor high-voltage cycle stability and insufficient safety of layered oxides, related technologies have employed physical mixing of thermally stable and structurally stable polyanionic materials with layered oxides in a specific ratio. While this can improve the cycle performance and safety to some extent, simple physical mixing results in weak interfacial bonding, making it difficult to achieve synergistic structural changes. This leads to particle shedding and electrode damage during long cycles, affecting the battery's cycle stability and rate performance. In this application, while the polyanionic material tightly bonds to the surface of the layered oxide core to form the first positive electrode active material, it also serves as the second positive electrode active material, filling the gaps between the first positive electrode active materials. This results in a tighter bond between the polyanionic material and the layered oxide, better leveraging their synergistic effect and improving the high-voltage cycle stability and safety of the positive electrode active material.
[0040] In a first aspect, this application proposes a positive electrode active material for sodium secondary batteries, comprising: a first positive electrode active material, the first positive electrode active material comprising a core, the core comprising a layered oxide, a coating layer, the coating layer being located at least on a portion of the surface of the core, the coating layer comprising a polyanionic material; and a second positive electrode active material, the second positive electrode active material comprising the polyanionic material; wherein the peak intensity of the XRD diffraction peak of the positive electrode active material is I within a 2θ diffraction angle of 16.6°±0.5°. (003) The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 15.9°±0.3° is I. (011)The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 41.5°±0.5° is I. (104) 0.5≤I A ≤0.7, 0.02≤I B ≤0.05, where I A =I (003) / (I (003) +I (104) ), I B =I (011) / (I (011) +I (104) Thus, the polyanionic material forms a coating layer on the surface of the layered oxide core, allowing the polyanionic material to tightly bond with the layered oxide to form the first positive electrode active material. The electron conduction and ion diffusion efficiency between the polyanionic material and the layered oxide inside the first positive electrode active material is greatly improved. At the same time, the polyanionic material also fills the gaps between the first positive electrode active materials. The positive electrode active material has high structural stability and can play a synergistic role over a long period of time. During charge and discharge cycles, the rate of increase of the battery's DC internal resistance is greatly reduced, thereby improving the battery's high-voltage cycle stability, rate performance, and safety.
[0041] In this application, I A The physical meaning of I is: the relative proportion of the characteristic peak intensity of layered oxides in the total characteristic intensity of the positive electrode active material, directly reflecting the proportion of layered structure in the positive electrode active material. B The physical meaning represented is: the relative proportion of the characteristic peak intensity of polyanionic materials in the total characteristic intensity of the positive electrode active material, directly reflecting the proportion of polyanionic materials in the positive electrode active material. Specifically, the (003) crystal plane reflects the interlayer Na... + The long-range ordered stacking of the transition metal (TM) layer is a characteristic peak of the layered structure. The higher the intensity of this peak, the greater the proportion of the typical layered phase in the cathode active material. The (011) crystal plane represents a plane with a specific orientation in the sodium iron phosphate pyrophosphate crystal and is a characteristic peak of the polyanionic material. The (104) peak represents the local structural order within the transition metal layer, and its intensity is related to both the layered and non-layered phases. When the cathode active material undergoes a transformation from a layered phase to a non-layered phase, the (104) peak may be enhanced due to the diffraction contribution of the new phase, or it may be broadened or split due to lattice distortion. Among these factors, the mass ratio of the polyanionic material to the layered oxide affects the coating and mixing ratio. When the amorphous polyanionic material coats the surface of the layered oxide, the peak intensity of the (003) crystal plane diffraction peak in the corresponding c-axis direction will decrease. With more uniform surface coating, the peak intensity of the (003) crystal plane of the cathode active material will further decrease.
[0042] As an example, I AIt can be 0.5, 0.55, 0.6, 0.65, or 0.7, etc.; I B It can be 0.02, 0.03, 0.04, or 0.05, etc.
[0043] When the positive electrode active material I A and I B When the above conditions are met, the ratio of polyanionic material to layered oxide in the positive electrode active material remains constant, which can simultaneously achieve a uniform polyanionic material coating layer on the surface of the layered oxide core, and the polyanionic material as the second positive electrode active material effectively fills the gaps between the first positive electrode active materials, resulting in higher structural stability and safety of the positive electrode active material.
[0044] In some embodiments, the polyanionic material only partially covers the surface of the layered oxide core, while the remaining polyanionic material is independently distributed in the voids surrounding the first positive electrode active material particles.
[0045] In some embodiments, the mass ratio of the polyanionic material to the layered oxide in the positive electrode active material is (0.01-1):1, for example, it can be 0.01:1, 0.05:1, 0.1:1, 0.3:1, 0.5:1, 0.8:1 or 1:1, etc.; optionally, (0.10-0.45):1.
[0046] The (011) peak of the positive electrode active material corresponds to the characteristic peak of the polyanionic material, and its peak intensity can reflect the content of the polyanionic material. When the mass ratio is within the above range, it is beneficial to make the polyanionic material uniformly coated on the surface of the layered oxide and embedded in the gaps between the layered oxide particles, thereby improving the high-voltage cycle stability and safety of the positive electrode active material.
[0047] In this application, the polyanionic material and the layered oxide are dry-blended at a low mixing temperature. Therefore, after heat treatment, the polyanionic material only partially covers the surface of the layered oxide core, and the gaps between the layered oxides are also filled with polyanionic material. Within the aforementioned mass ratio range, the polyanionic material can achieve both partial coating of the layered oxides and gap-filling effect between them.
[0048] In some embodiments, the Dv50 particle size of the layered oxide is 3μm-10μm, for example, it can be 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm or 10μm, etc.; optionally, 4μm-9μm; further, 5μm-8μm.
[0049] In some embodiments, the Dv50 particle size of the polyanionic material is 0.5 μm-1.0 μm, for example, it can be 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, or 1 μm; optionally, 0.6 μm-0.9 μm; further, 0.7 μm-0.8 μm. This is beneficial for increasing the compaction density of the positive electrode active material, thereby improving the volumetric energy density of the battery.
[0050] In some embodiments, the particle size distribution SPAN of the layered oxide is 1.1-1.3, for example, 1.1, 1.2, or 1.3; optionally, 1.2-1.4; and / or, the particle size distribution SPAN of the polyanionic material is 3-4, for example, 3, 3.2, 3.4, 3.6, 3.8, or 4; optionally, 3.3-3.7. When the particle size distribution meets the above requirements, the compaction density of the positive electrode active material is further improved by grading particles of different sizes.
[0051] In some embodiments, the Dv50 particle size of the positive electrode active material is 3μm-10μm, for example, it can be 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm or 10μm, etc.; optionally, 5μm-8μm; further, 5μm-7μm. This is beneficial to improving the compaction density of the positive electrode active material.
[0052] In some embodiments, the particle size distribution (SPAN) of the positive electrode active material is 1.5-2.5, for example, it can be 1.5, 1.7, 1.9, 2.1, 2.3 or 2.5, etc.; optionally, it is 1.8-2.2. This facilitates a denser packing of the positive electrode active material particles, thereby further improving the volumetric energy density of the sodium-ion battery.
[0053] Dv50 particle size, also known as median particle size, means that 50% of the volume of particles are smaller than or equal to this value. It can be measured using a Malvern Mastersizer 3000 laser particle size analyzer.
[0054] Particle size distribution (SPAN) is a key parameter describing the dispersion of particle size distribution. A smaller SPAN value indicates a more concentrated particle size distribution, while a larger SPAN value indicates a wider particle size distribution. The specific test for SPAN can be performed using particle size data obtained from a Malvern Mastersizer 3000 laser particle size analyzer. The SPAN value is calculated as follows: SPAN = (D... 90 -D 10 ) / D 50 .
[0055] When the Dv50 particle size and particle size distribution SPAN of polyanionic materials, layered oxides and positive electrode active materials meet the above conditions, the positive electrode active materials have high compaction density and specific capacity.
[0056] In some embodiments, the specific surface area of the positive electrode active material is 1 m². 2 / g-7m 2 / g, for example, can be 1m 2 / g、2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g or 7m 2 / g etc.
[0057] Specific surface area refers to the total surface area per unit mass of positive electrode active material. It can be measured using the Tristar II3020 specific surface area analyzer from Micromertics, Inc.
[0058] A specific surface area within the above range can improve the dispersion uniformity of the positive electrode active material in the positive electrode slurry, reduce the amount of dispersant and binder, and improve the processing performance of the positive electrode active material.
[0059] In some embodiments, the compaction density of the positive electrode active material is 3.1 g / cm³. 3 -3.4g / cm 3 For example, it can be 3.1 g / cm³. 3 3.2g / cm 3 3.3g / cm 3 Or 3.4g / cm 3 wait.
[0060] Compacted density refers to the mass per unit volume of the electrode coating after rolling. It is measured using the weighing-thickness method. Specifically, the compacted density is calculated by measuring the mass, area, and thickness of the electrode sheet.
[0061] Compaction density within the above range is beneficial for improving the volumetric energy density of the battery and enhancing its capacity utilization during charge-discharge cycles.
[0062] In some embodiments, the layered oxide satisfies the chemical formula: Na a1 (Ni x1 Fe y1 Mn z1 M' n1O2, wherein 0.90≤a1≤1.10, 0≤x1≤0.5, 0≤y1≤0.5, 0≤z1≤0.5, 0≤n1≤0.3, x1+y1+z1+n1=1, and M' includes at least one of Sn, Ce, La, Co, Ca, Cu, Sr, Y, Ti, V, Mg, B, Cr, Sb, Al, Zn, Zr, Nb, W, and Li. This is beneficial for improving the structural stability and specific capacity of the positive electrode active material.
[0063] As an example, a1 can be 0.90, 0.95, 1, 1.05 or 1.10, etc.; x1 can be 0, 0.1, 0.2, 0.3, 0.4 or 0.5, etc.; y1 can be 0, 0.1, 0.2, 0.3, 0.4 or 0.5, etc.; z1 can be 0, 0.1, 0.2, 0.3, 0.4 or 0.5, etc.; and n1 can be 0, 0.1, 0.2 or 0.3, etc.
[0064] In some embodiments, a1:(x1+y1+z1+n1)=(0.90-1.05):1, for example, can be 0.90:1, 0.93:1, 0.95:1, 0.98:1, 1:1, 1.03:1 or 1.05:1, etc.; optionally, (0.95-1.05):1; further, (0.97-1.03):1; and / or, 0<n1≤0.02. This is beneficial for further improving the specific capacity of the positive electrode active material.
[0065] In some embodiments, the polyanionic material satisfies the chemical formula: Na₄Fe 3-x M x (PO4)2(P2O7) / C, where 0≤x≤0.3, for example, can be 0, 0.1, 0.2 or 0.3, etc., and M includes at least one of Mn, Co, Ni, Ti, Cu, and V. This is beneficial to improving the safety of the positive electrode active material.
[0066] It should be noted that " / C" indicates that at least a portion of the surface of the polyanionic material has a carbon coating layer. This is beneficial for improving the electronic conductivity of the polyanionic material.
[0067] In a second aspect of this application, a method for preparing the aforementioned positive electrode active material is provided, comprising:
[0068] S1: Sodium source, iron source, phosphorus source, and M source are mixed and ground to obtain an intermediate. The intermediate is then mixed with a carbon source and subjected to a first sintering treatment under a nitrogen atmosphere to obtain a polyanionic material.
[0069] In this step, there are no particular restrictions on the specific method of mixing the sodium source, iron source, phosphorus source, and M source; for example, a mixer can be used. It can be understood that in this step, the addition of the M source can be flexibly chosen as needed.
[0070] In some embodiments, the sodium source includes at least one selected from sodium carbonate, sodium dihydrogen phosphate, sodium hydroxide, sodium nitrate, and sodium oxide; the iron source includes at least one selected from Fe₂O₃, FeC₂O₄, FeSO₄, FeCl₃, and Fe(NO₃)₃; the phosphorus source includes at least one selected from (NH₄)₂HPO₄, H₃PO₄, and NH₄H₂PO₄; the M source includes at least one selected from oxides, carbonates, phosphates, fluorides, chlorides, hydroxides, and silicides of element M; and the carbon source includes at least one selected from glucose, sucrose, citric acid, and oxalic acid. Therefore, the raw materials are widely available, facilitating large-scale application.
[0071] Specifically, the M source may include at least one of Mn(CH3COO)2, MnO2, MnSO4, Co(OH)2, Co(NO3)2, CoO, CoCl2, NiCl2, NiO, NiSO4, TiO2, TiCl4, CuO, CuSO4, V2O5, and NH4VO3.
[0072] In some embodiments, the temperature of the first sintering treatment is 400℃-700℃ (e.g., 400℃, 500℃, 600℃, or 700℃), and the time is 8h-12h (e.g., 8h, 9h, 10h, 11h, or 12h). This is beneficial for controlling the particle size of the polyanionic material and improving its crystallinity and structural stability.
[0073] In some embodiments, after the first sintering treatment, the material can be naturally cooled, then pulverized and sieved to obtain submicron-sized polyanionic materials.
[0074] S2: The sodium source, precursor, and M' source are mixed and subjected to a second sintering treatment under an oxidizing atmosphere to obtain a layered oxide.
[0075] In this step, there are no particular restrictions on the specific method of mixing the sodium source, precursor, and M' source; for example, a mixer can be used. It is understood that in this step, the addition of the M' source can be flexibly chosen as needed.
[0076] In some embodiments, the precursor includes (Ni x1 Fe y1 Mn z1 )OOH、(Ni x1 Fe y1 Mn z1 At least one of (OH)2.
[0077] In some embodiments, the M' source includes at least one of the following: oxides, carbonates, phosphates, fluorides, chlorides, hydroxides, and silicides of the M' element. Therefore, the raw material sources are widely available, facilitating large-scale deployment.
[0078] Specifically, the source M' may include at least one of CaO, CaCO3, Ca3(PO4)2, CaF2, CaCl2, Ca(OH)2, CaSi2, CuO, CuSO4, Sr(OH)2, SrCO3, Sn(OH)4, Y2O3, La2O3, Ce2O3, CeO2, Li2CO3, LiOH, Co(OH)2, V2O5, Cr2O3, ZrO, Zr(HPO4)2, ZrSi2, Al2O3, AlPO4, AlCl3, ZnO, TiO2, MgO, MgCO3, Mg2Si, Mg3(PO4)2, MgF2, MgCl2, Nb2O5, WO3, B2O3, Sb2O5, and Sb2O3.
[0079] In some embodiments, the temperature of the second sintering treatment is 900℃-1100℃ (e.g., 900℃, 950℃, 1000℃, 1050℃, or 1100℃), and the time is 8h-15h (e.g., 8h, 9h, 10h, 11h, 12h, 13h, 14h, or 15h). This is beneficial for improving the crystallinity of the layered oxides and controlling the particle size.
[0080] In some embodiments, the second sintering process may also involve natural cooling followed by pulverization and sieving to obtain micron-sized layered oxides.
[0081] S3: The polyanionic material and the layered oxide material are mixed and then subjected to a third sintering treatment under a nitrogen atmosphere. The temperature of the third sintering treatment is less than 500°C, so as to obtain the positive electrode active material.
[0082] Specifically, polyanionic materials and layered oxides can be weighed and mixed evenly according to the mass ratio to obtain a blended material. The blended material is then subjected to a third sintering treatment under a nitrogen atmosphere. After sintering, the material is naturally cooled, and then crushed and sieved to obtain the positive electrode active material.
[0083] In some embodiments, the temperature of the third sintering treatment is 100℃-500℃, for example, it can be 100℃, 200℃, 300℃, 400℃ or 500℃; optionally, it is 200℃-400℃.
[0084] In some embodiments, the time for the third sintering treatment is 3h-10h, for example, it can be 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h, etc.; optionally, 4h-8h.
[0085] In some embodiments, the heating rate of the third sintering process is 0.5℃ / min-5℃ / min, for example, it can be 0.5℃ / min, 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min or 5℃ / min, etc.; optionally, it is 1℃ / min-3℃ / min.
[0086] The lower temperature of the third sintering process is beneficial for obtaining a cathode active material in which amorphous polyanionic material is partially coated on the surface of layered oxides. The uniformity of the surface coating is related to the temperature of the third sintering process. When the temperature of the third sintering process is within the above range, the peak intensity of the diffraction peaks of specific crystal planes in the cathode active material is controllable, which can meet the requirements of I... A I B The aforementioned limitations apply. This improves the interfacial bonding strength between the polyanionic material and the layered oxide in the positive electrode active material, significantly enhances the electron conduction and ion diffusion efficiency between particles, improves rate performance, significantly reduces the increase in DC internal resistance (DCR) during cycling, and improves high-voltage cycling performance.
[0087] In some embodiments, the layered oxide and the polyanionic material each independently comprise single-crystal particles.
[0088] In some embodiments, the crystalline phase of the layered oxide includes the O3 phase.
[0089] Compared to simple single-crystal layered oxides, this application, by controlling the mass ratio of polyanionic material to layered oxides and selecting a suitable sintering process, obtains a cathode active material with high voltage cycling stability and high safety. After sintering, the two particle interfaces in the cathode active material are more tightly bonded, significantly improving the electron conduction and ion diffusion efficiency between particles, thus improving rate performance and reducing DCR growth during cycling, resulting in improved high-voltage cycling performance. Simultaneously, the uniform composite of a suitable amount of thermally stable polyanionic material around the layered oxides contributes to the high safety of the cathode active material. Furthermore, the process is simple and easily scalable for industrial production.
[0090] In a third aspect, this application proposes a battery comprising a positive electrode sheet, said positive electrode sheet comprising the aforementioned positive electrode active material, or a positive electrode active material prepared by the aforementioned method. Thus, this battery possesses all the features and advantages of the aforementioned positive electrode active material and its preparation method, which will not be elaborated further here.
[0091] It is understood that there are no particular restrictions on the specific type of battery; it can be a primary battery or a secondary battery. The shape of the sodium-ion battery can be cylindrical, square, or any other shape. According to the outer packaging, sodium-ion batteries can be hard-shell batteries, soft-pack batteries, etc.
[0092] Taking sodium-ion batteries as an example, a typical sodium-ion battery includes a positive electrode, a negative electrode, an electrolyte, and a separator. The positive and negative electrodes and the separator are fabricated into electrode assemblies using winding or stacking processes. The electrode assemblies and electrolyte are housed in an outer package. During the charging and discharging process of a sodium-ion battery, sodium ions repeatedly insert and extract between the positive and negative electrodes. The electrolyte acts as a conductor of ions between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing active sodium ions to pass through.
[0093] In some embodiments, the positive electrode sheet may include a positive current collector and a positive active material layer disposed on at least one side surface of the positive current collector. The positive active material layer includes a positive active material, a conductive agent, and a binder. The positive current collector may include a metal foil, for example, aluminum foil. The positive active material may be the positive active material of the first aspect of this application or the positive active material prepared by the method described in the second aspect of this application. The conductive agent may include acetylene black, single-walled carbon nanotubes, and conventional materials in the art. The binder may be polyvinylidene fluoride (PVDF) and conventional materials in the art.
[0094] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a layer of negative electrode active material disposed on at least one side surface of the negative electrode current collector. The negative electrode active material layer may include a negative electrode active material, a thickener, a conductive agent, and a binder. The negative electrode current collector may be a metal foil, for example, copper foil. The negative electrode active material may include artificial graphite, natural graphite, silicon-carbon based composite materials, sodium metal sheets, and other commonly used negative electrode active materials in the art. The thickener may be sodium carboxymethyl cellulose (CMC-Na) and other conventional materials in the art. The conductive agent may be acetylene black and other conventional materials in the art. The binder may be styrene-butadiene rubber and other conventional materials in the art.
[0095] In some embodiments, the separator may be a separator known in the art that can be used in sodium-ion batteries and is stable to the electrolyte used, such as a polyethylene separator, a polypropylene separator, a polyethylene / polypropylene composite separator, etc.
[0096] The following specific embodiments illustrate the solution of this application. It should be noted that these embodiments are for illustrative purposes only and should not be considered as limiting the scope of this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0097] Example 1
[0098] S1: Sodium carbonate, ferric oxalate, ammonium dihydrogen phosphate, and manganese oxalate are mixed evenly in a molar ratio of Na, Fe, P, and Mn of 4:2.7:4:0.3 to obtain the first mixture.
[0099] S2: Place the first mixture from S1 into the grinding chamber of a sand mill, and add an appropriate amount of deionized water as the grinding medium. The solid-liquid ratio is controlled at 1:3 (mass ratio). Set the grinding speed of the sand mill to 2000 r / min, and grind for 2 hours to obtain a slurry with a suitable particle size. Then, spray dry the slurry to obtain an intermediate, and mix it with an appropriate amount of glucose to obtain a second mixture.
[0100] S3: The second mixture of S2 is heated to 600℃ in a nitrogen atmosphere at a heating rate of 1.5℃ / min and held for 9 hours. The calcined material is then naturally cooled, pulverized, and sieved to obtain a single-crystal polyanionic material with Dv50 = 0.7 micrometers and a particle size distribution SPAN of 3.5.
[0101] S4: Nickel sulfate, ferric sulfate, and manganese sulfate were dissolved in a nickel, iron, and manganese molar ratio of 1:1:1 to obtain a 2 mol / L mixed salt solution; sodium hydroxide was dissolved to prepare a 10 mol / L precipitant solution; and ammonia was dissolved to prepare an 8 mol / L complexing agent solution. 100 L of the mixed salt solution, precipitant solution, and complexing agent solution were fed into a reactor in a parallel flow. Under a nitrogen atmosphere and continuous control of the precipitate crystallization growth via an overflow device, the average particle size grew to 3.5 μm. The precursor slurry was filtered, washed, and the filter cake was dried at 120°C and sieved to obtain the precursor with a particle size distribution (SPAN) of 1.3.
[0102] S5: The multi-component precursor described in S4 is mixed with Na2CO3, calcium oxide, and strontium hydroxide in a molar ratio of Na / (Ni+Fe+Mn+Ca+Sr) = 1.01:1, where Na / Ca / Sr = 1.01:0.01:0.01. The mixture is heated to 600°C at a rate of 6°C / min in an oxidizing atmosphere, and then to 1000°C at a rate of 1.5°C / min. The mixture is held at this temperature for 12 hours. After cooling, crushing, and sieving, a single-crystal layered oxide with a Dv50 of 6.5 micrometers and a particle size distribution SPAN of 1.3 is obtained.
[0103] S6: The single-crystal polyanionic material described in S3 and the single-crystal layered oxide described in S5 are uniformly mixed at a mass ratio of 0.25:1. The mixture is heated to 300°C at a heating rate of 3°C / min in a nitrogen atmosphere and held at that temperature for 6 hours. After calcination, the material is allowed to cool naturally, then pulverized and sieved to obtain a positive electrode active material with Dv50 = 5.3 micrometers and a particle size distribution SPAN of 1.9.
[0104] The differences between the other embodiments and comparative examples and embodiment 1 are shown in Table 1. In comparative example 2, only layered oxide is used as the positive electrode active material, and in comparative example 7, polyanionic material and layered oxide are physically mixed and used as the positive electrode active material.
[0105]
[0106]
[0107]
[0108]
[0109]
[0110]
[0111] I. Testing methods and results for powders:
[0112] (1) Morphological test
[0113] This application tested scanning electron microscope (SEM) images of the monocrystalline polyanionic material, monocrystalline layered oxide, and positive electrode active material prepared in the above embodiments and comparative examples, and exemplarily provides SEM images of the monocrystalline polyanionic material, monocrystalline layered oxide, and positive electrode active material prepared in Example 1. The results are as follows: Figure 1-3 As shown. From Figure 1 It can be seen that the morphology of the single-crystal polyanionic material is submicron small particles with a wide particle size distribution; from Figure 2It can be seen that the morphology of the single-crystal layered oxide consists of micron-sized particles with smooth surfaces and a wide particle size distribution; from Figure 3 It can be seen that a small portion of the monocrystalline polyanionic material in the positive electrode active material covers the surface of the monocrystalline layered oxide, while most of the monocrystalline polyanionic material is independently distributed in the gaps around its particles, playing a gap-filling role and helping to improve the compaction density of the positive electrode active material.
[0114] (2) Physical property testing
[0115] This application tested the XRD patterns of the monocrystalline polyanionic material, monocrystalline layered oxide material, and positive electrode active material in the above embodiments and comparative examples, and exemplarily provides the XRD spectra of the monocrystalline polyanionic material, monocrystalline layered oxide, and positive electrode active material prepared in Example 1. The results are as follows: Figures 4-6 As shown, from Figure 4 It can be seen that the phase of the single-crystal polyanionic material is Na4Fe. 2.7 Mn 0.3 (PO4)2(P2O7) / C; from Figure 5 It can be seen that the phase of the single-crystal layered oxide in this application is O3-type layered oxide (Na). 1.01 Ni 0.327 Fe 0.327 Mn 0.327 Ca 0.01 Sr 0.01 O2), Figure 6 It can be seen that the phase of the positive electrode active material in this application is a composite phase of sodium electropolymerized anion material and O3-type layered oxide material (Na4Fe). 2.7 Mn 0.3 (PO4)2(P2O7) / C@Na 1.01 Ni 0.327 Fe 0.327 Mn 0.327 Ca 0.01 Sr 0.01 O2).
[0116] II. Electrochemical Performance Tests and Results of the Battery
[0117] 1. Battery manufacturing method:
[0118] The positive electrode active material, acetylene black, and polyvinylidene fluoride (PVDF) were thoroughly mixed with an appropriate amount of N-methylpyrrolidone (NMP) at a mass ratio of 95:3:2 to form a uniform slurry. This slurry was coated onto aluminum foil and dried at 120°C for 12 hours. Then, it was stamped under a pressure of 100 MPa to form a positive electrode sheet with a diameter of 12 mm and a thickness of 120 μm. The loading of the positive electrode active material was 15 mg / cm³. 2 .
[0119] 2. Battery Assembly: In an Ar gas glove box with both water and oxygen content less than 5 ppm, assemble the positive electrode, separator, negative electrode, and electrolyte into a 2025 coin cell and let it stand for 6 hours. The negative electrode uses a 17 mm diameter, 1 mm thick sodium metal sheet; the separator uses a 25 μm thick Celgard 2325 porous membrane; the electrolyte uses a 1 mol / L NaPF6 solution with equal volumes of ethylene carbonate (EC) and diethyl carbonate (DEC) as solvents.
[0120] 3. Electrical performance testing methods
[0121] Electrochemical tests were conducted on the coin cells at 25°C using the Xinwei Battery Testing System, and the charge / discharge current density at 0.1C was 140 mA / g.
[0122] The positive electrode active materials prepared in the aforementioned examples and comparative examples were assembled into coin cells, and their electrical performance was tested. The test methods are as follows, and the results are shown in Table 3.
[0123] (1) Test method for specific capacity of 0.1C first charge and discharge at 2.0V-4.15V.
[0124] The prepared coin cells were subjected to charge-discharge tests at 25°C, 2.0V-4.15V, and 0.1C to evaluate the 0.1C initial charge-discharge specific capacity of the material.
[0125] (2) Average voltage test method for positive electrode active materials
[0126] The prepared coin cells were subjected to charge-discharge tests at 25℃, 2.0V-4.15V, and 0.1C to evaluate the material's initial discharge specific energy and discharge specific capacity at 0.1C. The average voltage was calculated as: discharge specific energy / discharge specific capacity.
[0127] (3) Ratio Performance Testing Method
[0128] The prepared coin cells were cycled twice at 25°C, 2.0V-4.15V, and 0.1C, and then cycled once each at 0.2C, 0.33C, 0.5C, and 1C. The rate performance of the positive electrode active material was evaluated by the ratio of the initial discharge specific capacity at 0.1C to the discharge specific capacity at 1C. The initial discharge specific capacity at 0.1C was the discharge specific capacity of the coin cell in the first cycle, and the discharge specific capacity at 1C was the discharge specific capacity of the coin cell in the sixth cycle.
[0129] (4) Cyclic performance testing method
[0130] The prepared coin cells were cycled twice at 25°C, 2.0V-4.15V, and 0.1C, and then cycled for 80 cycles at 1C to evaluate the capacity retention of the material.
[0131] (5) Volumetric energy density test method
[0132] The volumetric energy density can be obtained by multiplying the 0.1C discharge specific capacity, average voltage and corresponding compaction density obtained by the above methods (1) and (2).
[0133] (6) HPPC DCR Test Method
[0134] Test procedure: First, the button cell battery was charged at a constant current and constant voltage of 0.3C to 4.15V, with a cutoff current of 0.05C, and left to rest for 10 minutes. Then, it was discharged at a constant current to a cutoff voltage of 2.0V, and left to rest for 10 minutes. Next, it was charged at a constant current and constant voltage of 0.3C to 4.15V, with a cutoff current of 0.05C, and left to rest for 10 minutes. Then, it was discharged at a constant current of 0.3C to 90% SOC, left to rest for 10 minutes, discharged at 3C for 18 seconds, left to rest for 10 minutes, charged at 3C for 10 seconds, and left to rest for 10 minutes. The DCR at this SOC was calculated according to the HPPC test method. Next, it was discharged at a constant current of 0.3C to 80% SOC, left to rest for 10 minutes, discharged at 3C for 18 seconds, left to rest for 10 minutes, charged at 3C for 10 seconds, and left to rest for 10 minutes. The DCR at this SOC was calculated according to the HPPC test method. Then, the DCR values at different SOCs (90% to 10% SOC) were calculated in this way.
[0135] The button cell was then cycled twice at 2.0-4.15V and 0.1C, and then 80 times at 1C.
[0136] Repeat the HPPC DCR test on this cycled coin cell to calculate the DCR value at different SOCs after the cycle. Then, calculate the DCR growth rate of the battery using the discharge DCR values at 60% SOC before and after the cycle ((DCR growth rate = (DCR value at 60% SOC before the cycle - DCR value at 60% SOC after the cycle) / DCR value at 60% SOC before the cycle)).
[0137] Table 3
[0138]
[0139]
[0140] As shown in Table 3, through comparison of the examples and comparative examples, it can be seen that the heat treatment process of the positive electrode active material is related to the coating condition and interstitial filling effect of the single-crystal polyanionic material and the single-crystal layered oxide, thus affecting I.A and I B The value of is not satisfied with I. A and I B The limited positive electrode active material exhibits a higher initial DCR and a faster DCR increase after cycling during charge and discharge, but worse rate and cycle performance.
[0141] When the types of doping elements in single-crystal polyanionic materials and single-crystal layered oxides are within the preferred range, composite cathodes with different doping elements can exhibit comparable improved performance after heat treatment at the same doping amount.
[0142] Compared to simple monocrystalline layered oxides, the positive electrode active material obtained by mixing monocrystalline polyanionic materials with monocrystalline layered oxides in a certain proportion and then performing a heat treatment process has improved DCR, rate performance and cycle performance.
[0143] Compared to simple physical mixing, the positive electrode active material prepared by the heat treatment process in this application has improved DCR, rate performance and cycle performance.
[0144] The single-crystal morphology of monocrystalline polyanionic materials and monocrystalline layered oxides is characterized by a wide distribution of particle size. When the particle size distribution (SPAN) of monocrystalline polyanionic materials and monocrystalline layered oxides is within the aforementioned range, and the mass ratio is also within the aforementioned range, the positive electrode active material has a higher compaction density, and the battery has a higher volumetric energy density.
[0145] In this embodiment, the polyanionic material, layered oxide, and positive electrode active material from Example 1 were assembled into half-cells, charged to 4.15V, and the positive electrode was removed for DSC testing. The test result curve is shown below. Figure 7 As shown. By Figure 7 It can be seen that the heat release of the positive electrode active material (Example 1) is significantly lower than that of the single-crystal layered oxide, and the heat release peak is shifted to the later stage, which shows that the safety of the positive electrode active material is greatly improved compared with that of the simple single-crystal layered oxide.
[0146] In Comparative Example 7, the amount of polyanionic material used was too small, which could only achieve a very small amount of coating on the surface of the layered oxide, resulting in poor cycle performance and rate performance of the positive electrode active material.
[0147] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A positive electrode active material for sodium secondary batteries, characterized in that, include: A first positive electrode active material, comprising a core, the core comprising an O3-type layered oxide, and a coating layer, the coating layer being located at least on a portion of the surface of the core, the coating layer comprising a polyanionic material; The second positive electrode active material includes the polyanionic material, wherein the polyanionic material has the chemical formula: Na₄Fe₂O₃. 3-x M x (PO4)2(P2O7) / C, where 0≤x≤0.3, and M includes at least one of Mn, Co, Ni, Ti, Cu, and V; The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 16.6°±0.5° is I. (003) The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 15.9°±0.3° is I. (011) The peak intensity of the XRD diffraction peak of the positive electrode active material within a 2θ diffraction angle of 41.5°±0.5° is I. (104) , 0.5≤I A ≤0.7, 0.02≤I B ≤0.05, wherein I A =I (003) / (I (003) +I (104) ), I B =I (011) / (I (011) +I (104) ); The O3-type layered oxide satisfies the following chemical formula: Na a1 (Ni x1 Fe y1 Mn z1 M' n1 O2, wherein 0.90≤a1≤1.10, 0≤x1≤0.5, 0≤y1≤0.5, 0≤z1≤0.5, 0≤n1≤0.3, x1+y1+z1+n1=1, and M' includes at least one of Sn, Ce, La, Co, Ca, Cu, Sr, Y, Ti, V, Mg, B, Cr, Sb, Al, Zn, Zr, Nb, W, and Li.
2. The positive electrode active material according to claim 1, characterized in that, The mass ratio of the polyanionic material to the O3-type layered oxide in the positive electrode active material is (0.01-1):
1.
3. The positive electrode active material according to claim 2, characterized in that, The mass ratio of the polyanionic material to the O3-type layered oxide in the positive electrode active material is (0.10-0.45):
1.
4. The positive electrode active material according to claim 1, characterized in that, The Dv50 particle size of the O3-type layered oxide is 3μm-10μm; and / or, The Dv50 particle size of the polyanionic material is 0.5μm-1.0μm.
5. The positive electrode active material according to claim 4, characterized in that, The Dv50 particle size of the O3-type layered oxide is 4μm-9μm; and / or, The Dv50 particle size of the polyanionic material is 0.6μm-0.9μm.
6. The positive electrode active material according to claim 5, characterized in that, The Dv50 particle size of the O3-type layered oxide is 5μm-8μm; and / or The Dv50 particle size of the polyanionic material is 0.7μm-0.8μm.
7. The positive electrode active material according to claim 4, characterized in that, The particle size distribution (SPAN) of the O3-type layered oxide is 1.1-1.3; and / or, The particle size distribution SPAN of the polyanionic material is 3-4.
8. The positive electrode active material according to claim 7, characterized in that, The particle size distribution (SPAN) of the O3-type layered oxide is 1.2-1.4; and / or, The particle size distribution (SPAN) of the polyanionic material is 3.3-3.
7.
9. The positive electrode active material according to any one of claims 1-8, characterized in that, The Dv50 particle size of the positive electrode active material is 3μm-10μm.
10. The positive electrode active material according to claim 9, characterized in that, The positive electrode active material has a Dv50 particle size of 5μm-8μm.
11. The positive electrode active material according to claim 10, characterized in that, The positive electrode active material has a Dv50 particle size of 5μm-7μm.
12. The positive electrode active material according to claim 9, wherein the particle size distribution (SPAN) of the positive electrode active material is 1.5-2.5; and / or, The specific surface area of the positive electrode active material is 1 m². 2 / g -7 m 2 / g; and / or, The compaction density of the positive electrode active material is 3.1 g / cm³. 3 -3.4g / cm 3 .
13. The positive electrode active material according to claim 12, wherein the particle size distribution SPAN of the positive electrode active material is 1.8-2.
2.
14. The positive electrode active material according to claim 1, characterized in that, a1:(x1+y1+z1+n1)=(0.90-1.05):1; and / or, 0<n1≤0.02。 15. The positive electrode active material according to claim 14, characterized in that, a1:(x1+y1+z1+n1)=(0.95-1.05):
1.
16. The positive electrode active material according to claim 15, characterized in that, a1:(x1+y1+z1+n1)=(0.97-1.03):
1.
17. A method for preparing the positive electrode active material according to any one of claims 1-16, characterized in that, Sodium source, iron source, phosphorus source and M source are mixed and ground to obtain an intermediate. The intermediate is mixed with carbon source and subjected to a first sintering treatment in nitrogen atmosphere to obtain polyanionic material. The sodium source, precursor, and M' source were mixed and subjected to a second sintering treatment under an oxidizing atmosphere to obtain O3-type layered oxides. The polyanionic material is mixed with the O3-type layered oxide and then subjected to a third sintering treatment under a nitrogen atmosphere. The temperature of the third sintering treatment is less than 500°C to obtain the positive electrode active material.
18. The method according to claim 17, characterized in that, The temperature of the third sintering treatment is 100℃-500℃; and / or, The third sintering treatment takes 3-10 hours; and / or, The heating rate of the third sintering process is 0.5℃ / min to 5℃ / min.
19. The method according to claim 18, characterized in that, The temperature of the third sintering treatment is 200℃-400℃; and / or, The third sintering treatment takes 4-8 hours; and / or, The heating rate of the third sintering treatment is 1℃ / min-3℃ / min.
20. The method according to any one of claims 17-19, characterized in that, The temperature of the first sintering treatment is 400℃ 700℃ for 8-12 hours; and / or, the second sintering treatment is performed at 900℃. 1100℃, for 8-15 hours.
21. The method according to claim 20, characterized in that, The sodium source includes at least one selected from sodium carbonate, sodium dihydrogen phosphate, sodium hydroxide, sodium nitrate, and sodium oxide; and / or, The iron source includes Fe2O3 and FeC2O 4、 At least one of FeSO4, FeCl3, and Fe(NO3)3; and / or, The phosphorus source includes at least one of (NH4)2HPO4, H3PO4, and NH4H2PO4; and / or, The M source includes at least one of the following: oxides, carbonates, phosphates, fluorides, chlorides, hydroxides, and silicides of element M; and / or, The carbon source includes at least one selected from glucose, sucrose, citric acid, and oxalic acid; and / or, The M' source includes at least one of the following: oxides, carbonates, phosphates, fluorides, chlorides, hydroxides, and silicides of the M' element.
22. A battery, characterized in that, include: The positive electrode sheet comprises the positive active material according to any one of claims 1-16, or the positive active material prepared by the method according to any one of claims 17-21.
Citation Information
Patent Citations
Mixed type sodium ion battery positive electrode material and preparation method thereof
CN116014119A
Sodium-ion battery positive electrode material, preparation method thereof, sodium-ion battery positive electrode and sodium-ion battery
CN117080379A