A method for controlling flatness and shape of GH4169 alloy strip

By optimizing the cold rolling and heat treatment processes of GH4169 alloy strip through a full-process process control method, the problems of strip straightness and shape control were solved, and high-quality GH4169 alloy strip production was achieved, ensuring the forming performance of subsequent sheet metal parts.

CN120662648BActive Publication Date: 2026-11-24AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510909034.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-02
Publication Date
2026-11-24
Estimated Expiration
2045-07-02

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention belongs to the field of high-temperature alloy cold-rolled strip preparation technology. It discloses a method for controlling the straightness and shape of GH4169 alloy strip, comprising the following steps: billet leveling; welding into coils; initial strip rolling to obtain initial strip, detecting the straightness of the initial strip, and performing heat treatment based on the test data of the initial strip's straightness; intermediate rolling to obtain intermediate strip, detecting the straightness of the intermediate strip, and performing heat treatment based on the test data of the intermediate strip's straightness; finished strip rolling to obtain finished strip, detecting the straightness of the finished strip, and performing heat treatment based on the test data of the finished strip's straightness; detecting the straightness of the heat-treated finished strip and performing finished strip straightening accordingly; and finally, stress-relief annealing of the finished strip. This invention employs end-to-end control measures from the original billet to the finished strip, effectively improving and enhancing the straightness and shape of the alloy strip, resulting in high-quality strip products with significant benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-temperature alloy cold-rolled strip preparation and quality control technology, specifically relating to a method for controlling the straightness and shape of GH4169 alloy strip. Background Technology

[0002] GH4169 alloy is a nickel-chromium-iron based precipitation-hardening wrought superalloy. Its microstructure consists of a γ matrix, Composed of phases, carbides, and reinforcing phases γ″ and γ′, GH4169 alloy is widely used in a temperature range of -253 to 650℃, with an instantaneous application temperature reaching 800℃. The alloy exhibits high strength below 650℃ and possesses excellent fatigue resistance, radiation resistance, oxidation resistance, and corrosion resistance, as well as good processing performance, weldability, and long-term structural stability, making it a key material widely used in aerospace, nuclear energy, and petroleum industries. GH4169 alloy metallurgical products mainly include cold-rolled strip, cold-rolled sheet, cold-drawn wire, and forged bars. Cold-rolled strip can be used to manufacture sheet metal parts such as sealing rings, sealing rings, damping rings, mounting edges, elastic elements, and thermal insulation liners for aerospace power units. The straightness and shape of GH4169 alloy strip have a significant impact on the manufacturing and performance of sheet metal parts. GH4169 alloy strip with good straightness and shape can improve the stamping forming performance of parts, which is beneficial for the forming and quality improvement of sheet metal parts.

[0003] For GH4169 alloy strip, the following problems exist: (1) The straightness of the strip is difficult to control and the shape is poor. Due to the ultra-thin strip, the finished product thickness is typically 0.05-0.80 mm, while the strip width is large, usually 200-600 mm, resulting in a very high width-to-thickness ratio, sometimes exceeding 10000. This high width-to-thickness ratio makes it difficult to control the straightness and shape of the strip during cold rolling, leading to significant issues with the product's appearance and quality. This manifests as defects such as wavy bends, wrinkles, edge waviness, center waviness, and warping, all of which negatively impact usability.

[0004] (2) The research on strip straightness and shape control technology is not systematic, resulting in unstable quality. Existing technologies for processing GH4169 alloy strip lack effective methods for controlling its straightness and shape. The traditional method involves tension bending straightening (or simply tension straightening) of the finished strip at the very end of the production process. This single method of improving the straightness of the alloy strip after rolling is not ideal. Actual cold-working production of strip involves a multi-cycle organic combination of cold rolling plastic deformation and heat treatment from the original strip blank to the finished strip. Currently, there is a lack of research on the synergistic control of cold rolling, heat treatment, tension straightening, and other processes that affect the straightness and shape of GH4169 alloy strip. Furthermore, the single tension straightening method used in existing technologies is tension straightening. While it improves the strip's appearance and shape, it increases residual stress. In the stamping process of precision sheet metal parts, the release of residual stress leads to part deformation. Currently, there is a lack of research on the correlation control of stress-relief annealing after tension straightening. Summary of the Invention

[0005] The purpose of this invention is to provide a method for controlling the straightness and shape of GH4169 alloy strip. From the perspective of the entire process, this invention proposes a method to thoroughly and effectively improve the straightness of alloy strip and effectively control the strip shape, so as to solve the current problems in the production of GH4169 alloy strip and ensure its high performance in subsequent use and the manufacturing quality of sheet metal parts.

[0006] To solve this technical problem, the technical solution of the present invention is as follows: A method for controlling the straightness and shape of GH4169 alloy strip, the process flow is as follows: (1) billet flattening → (2) welding into coils → (3) controlled tension rolling → (4) straightness and shape measurement → (5) initial strip controlled tension heat treatment → (6) controlled tension intermediate rolling → (7) straightness and shape measurement → (8) intermediate strip controlled tension heat treatment → (9) controlled tension finished product rolling → (10) straightness and shape measurement → (11) finished strip controlled tension heat treatment → (12) straightness and shape measurement → (13) finished product tension straightening → (14) finished product stress relief annealing.

[0007] The process parameters for step (5) are as follows: when d When the thickness is ≥20mm / m, control the tension of the heat treatment belt to be 20~30KN, the heat treatment temperature to be 1050~1100℃, and the belt speed to be 10~20 m / min. When 5mm / m≤ d When the thickness is <20mm / m, control the tension of the heat treatment belt to be 15~25KN, the heat treatment temperature to be 1000~1050℃, and the belt speed to be 10~20 m / min. when dWhen the tension of the heat treatment belt is less than 5 mm / m, control the tension of the heat treatment belt to be 10-15 KN, the heat treatment temperature to be 950-1000℃, and the belt speed to be 10-20 m / min. in, d The initial horizontal warpage of the strip after billet rolling.

[0008] The process parameters for step (8) are as follows: when d When the thickness is ≥20mm / m, control the tension of the heat treatment belt: 15~25KN, the heat treatment temperature: 1050~1080℃, and the belt speed: 10~25 m / min; When 5mm / m≤ d When the thickness is <20mm / m, control the tension of the heat treatment belt to be 10~20KN, the heat treatment temperature to be 980~1050℃, and the belt speed to be 10~25 m / min. when d When the thickness is <5mm / m, control the tension of the heat treatment belt to be 10-15KN, the heat treatment temperature to be 950-980℃, and the belt speed to be 10-25 m / min. in, d The horizontal warpage of the intermediate strip after intermediate rolling.

[0009] The process parameters for step (11) are as follows: when d When the thickness is ≥20mm / m, control the tension of the heat treatment belt: 10~20KN, the heat treatment temperature: 1050~1070℃, and the belt speed: 10~30 m / min; When 5mm / m≤ d When the thickness is <20mm / m, control the tension of the heat treatment belt: 10~15KN, the heat treatment temperature: 950~1050℃, and the belt speed: 10~30 m / min; when d When the tension of the heat treatment belt is <5mm / m, control the belt tension as follows: 8-12KN, heat treatment temperature: 930-980℃, and belt speed: 10-30 m / min. in, d The horizontal warpage of the finished strip after rolling.

[0010] The process parameters for step (13) are as follows: when d When the diameter is ≥10mm / m, control the tension of the straightening: 5~15KN, and the straightening speed: 1~5 m / min; When 5 mm / m≤ d When the tension is <10mm / m, control the tension: 5~10KN and the tension speed: 5~10 m / min; when d When the thickness is less than 5 mm / m, it is not necessary to straighten the finished strip. in, d The horizontal warpage of the finished strip after heat treatment.

[0011] By comprehensively controlling the tension process parameters in each step, the horizontal warpage of the high-temperature alloy cold-rolled strip produced by this invention reaches a certain level. d <3mm / m.

[0012] The method for controlling the straightness and shape of GH4169 alloy strip of the present invention adopts full-process control measures from raw billet to finished strip, which effectively improves the straightness and shape of alloy strip, and obtains strip products with good quality. It solves the problems of poor straightness, poor shape quality control, poor batch stability, high scrap rate and low pass rate of GH4169 alloy strip in the prior art.

[0013] Preferably, the process parameters for step (6) are: Cold rolling is performed in 5-8 passes, with the deformation per pass controlled at ≤18%, the rolling force per pass at 500-850KN, the inlet tension at 45-70KN, and the outlet tension at 55-80KN.

[0014] Preferably, the process parameters for step (9) are: Cold rolling is performed in 5-9 passes, with the deformation per pass controlled at ≤15%, the rolling force per pass at 600-900KN, the inlet tension at 40-60KN, and the outlet tension at 50-70KN.

[0015] Preferably, the stress-relief annealing of the finished product in step (14) has the following process parameters: stress-relief annealing process temperature: 500~550℃, belt speed: 15~40 m / min, and stress-relief annealing strip tension controlled at 5~8KN.

[0016] Preferably, the process parameters for step (1) are: single pass reduction amount: 0.01~0.1mm, single pass leveling speed: 0.5~10m / min.

[0017] Preferably, the welding process parameters in step (2) are: welding voltage: 10V~20V, welding current: 100A~150A, and plasma gas consumption: 50~150 L / h; the laser welding process parameters are: laser power: 300~800W, welding speed: 5~10 mm / s, and shielding gas: argon is used as the shielding gas, with a flow rate of 10~20 L / min.

[0018] Preferably, the welding process parameters for step (3) are: cold rolling is performed in 5-7 passes, the deformation amount of each pass is controlled to be ≤20%, the rolling force of each pass is 400-600KN, the inlet tension is 50-80KN, and the outlet tension is 60-90KN.

[0019] Specifically, the steps for controlling the straightness and shape of GH4169 alloy strip are as follows: Step 1: Blank leveling: The original strip blank of a certain thickness is repeatedly rolled and leveled on a multi-roll leveling machine; The thickness of the original strip blank is the incoming material thickness, which is much greater than the thickness of the finished strip. Step 2, Welding into Coils: Several leveled original strip blanks are welded into coils using plasma arc welding or laser welding methods; Step 3, initial rolling: The coiled strip is rolled using a multi-pass, small-deformation-per-pass cumulative deformation tension control method to obtain the initial strip material; Step 4: Straightness and Shape Measurement: A test strip of a certain length is cut from the initial strip material, and the horizontal warpage of the test strip is measured using a laser displacement sensor. d and three-dimensional contours; Step 5, Initial heat treatment of the material: The initial material is subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. Step 6, Intermediate rolling: The intermediate rolling process is carried out by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method to obtain intermediate strip material; Step 7: Flatness and Shape Measurement: A test strip of a certain length is cut from the intermediate process strip, and the horizontal warpage of the test strip is measured using a laser displacement sensor. d and three-dimensional contours; Step 8, intermediate process material heat treatment: The intermediate process material is subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere; Step 9, Finished product rolling: Using a multi-pass, small-deformation-per-pass cumulative deformation control tension method, finished product is precision rolled into a finished strip of a certain thickness; Step 10: Straightness and Shape Measurement: A test strip of a certain length is cut from the finished strip material, and the horizontal warpage of the test strip is measured using a laser displacement sensor. d and three-dimensional contours; Step 11, Heat treatment of finished product strip: The finished product strip is subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere; Step 12, Flatness and Shape Measurement: A test strip of a certain length is cut from the heat-treated finished strip. A laser displacement sensor is used to measure the horizontal warpage of the test strip. d and three-dimensional contours; Step 13, Finished Product Straightening: The finished strip is continuously stretched, bent and straightened on a multi-roller straightening unit; Step Fourteen: Stress-relief annealing of finished product: The finished strip after tension straightening is subjected to stress-relief annealing in a continuous bright heat treatment furnace under a hydrogen protective atmosphere to finally obtain GH4169 alloy strip with good flatness and shape.

[0020] The beneficial effects of this invention are: (1) A variety of process measures are adopted to control the flatness of GH4169 alloy strip throughout the entire process, especially to level the original strip blanks used, so as to control the impact on the flatness and shape of the strip from the source.

[0021] (2) In different cold rolling stages such as billet rolling, intermediate rolling and finished product rolling, different cold rolling process parameters are optimized and different tension rolling methods are adopted with multiple passes and small deformation per pass to control the cumulative deformation. This allows for the generation of smaller strain in the same rolling process, making the rolling force relatively stable, maintaining uniform deformation of the strip during the rolling process, suppressing and reducing uneven deformation and its probability, which is beneficial to improving the flatness of the strip and improving the shape.

[0022] (3) By measuring the horizontal warpage of the initial strip after billet rolling, the intermediate strip after intermediate rolling, the finished strip after finished rolling, and the finished strip after heat treatment, the horizontal warpage and plate shape test values ​​can be obtained. This can effectively guide the optimization and adjustment of processes such as initial strip heat treatment, intermediate strip heat treatment, finished strip heat treatment, and tension leveling, and configure corresponding optimized process parameters to effectively improve the control effect on the flatness and plate shape of alloy strip.

[0023] (4) By stress-relief annealing the finished strip after tension straightening, the residual stress in the finished strip is reduced and released, further controlling the tendency of the finished strip to deform, and achieving high-quality control of the flatness and shape of the alloy finished strip.

[0024] (5) By strictly controlling process parameters and process coordination, a reliable and effective method for full-process control of the straightness and shape of GH4169 alloy strip is provided. The horizontal warpage of GH4169 alloy strip produced by this invention is reduced. d With a thickness of <3mm / m, it has good flatness and shape, which improves the product quality and pass rate of GH4169 alloy strip, reduces production costs, and significantly improves the effect. Detailed Implementation

[0025] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] The features of various aspects of the embodiments of the present invention will now be described in detail. In the following detailed description, numerous specific details are set forth in order to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that the invention can also be practiced without these specific details. The following description of the embodiments is merely intended to provide a better understanding of the invention by illustrating examples. The invention is not limited to any specific setups and methods provided below, but covers all improvements, substitutions, etc., to product structures and methods without departing from the spirit of the invention.

[0027] In the following description, well-known structures and techniques are not shown in order to avoid unnecessarily obscuring the invention.

[0028] Example 1: According to a preferred embodiment of the method for controlling the straightness and shape of GH4169 alloy strip of the present invention, the following steps are included in sequence: The original strip blank with a thickness of 4.0 mm is repeatedly rolled and leveled on a multi-roll leveling machine with a single pass reduction of 0.09 mm and a single pass leveling speed of 3 m / min.

[0029] Several flattened original strip blanks were welded into coils using plasma arc welding. The welding voltage was 20V, the welding current was 150A, and the plasma gas consumption was controlled at 120 L / h.

[0030] The coiled strip was rolled in five passes with small deformation per pass to control the tension. The deformation per pass was controlled at 20%, 15%, 14%, 13%, and 10%, respectively. The rolling force per pass was 600 kN, the inlet tension was 80 kN, and the outlet tension was 90 kN, resulting in an initial strip thickness of 1.8 mm.

[0031] A 1000mm long test strip was cut from an initial strip material with a thickness of 1.8mm, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the initial strip after billet rolling is measured. d It is 22mm / m.

[0032] The initial strip with a thickness of 1.8 mm was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters for controlled tension heat treatment of the initial strip were: controlled tension of the heat treatment strip at 30 kN, heat treatment temperature at 1080 ℃, and conveyor speed at 10 m / min.

[0033] Intermediate process rolling was carried out using a multi-pass, small-deformation-per-pass cumulative deformation control tension method. The intermediate process rolling was carried out in 6 passes, with the deformation amounts controlled at 17.7%, 16%, 15.5%, 15%, 14.2%, and 13% for each pass. The rolling force for each pass was 550 kN, the inlet tension was 70 kN, and the outlet tension was 80 kN, resulting in an intermediate process strip with a thickness of 0.65 mm.

[0034] A 1000mm long test strip was cut from the 0.65mm thick intermediate process strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the intermediate strip after intermediate rolling is measured. d It is 15mm / m.

[0035] The 0.65mm intermediate process strip was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The process parameters for controlled tension heat treatment of the intermediate process strip were as follows: controlled tension of the heat treatment strip: 20KN, heat treatment temperature: 1050℃, and conveyor speed: 15 m / min.

[0036] The finished strip was finished by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method. It was cold rolled in 7 passes, with the deformation controlled at 15%, 12.7%, 12.5%, 9.5%, 8.5%, 7.8%, and 6.3% for each pass. The rolling force for each pass was 650 kN, the inlet tension was 50 kN, and the outlet tension was 65 kN, resulting in a finished strip with a thickness of 0.30 mm.

[0037] A 1000mm long test strip was cut from the 0.30mm thick intermediate process strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the finished strip after rolling is measured. d It is 9mm / m.

[0038] The finished strip with a thickness of 0.30 mm was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters for controlled tension heat treatment of the finished strip were: controlled tension of the heat treatment strip: 15 KN, heat treatment temperature: 980℃, and conveyor speed: 20 m / min.

[0039] A 1000mm long test strip was cut from the heat-treated 0.30mm thick finished strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional contour. In this embodiment, the horizontal warpage of the finished strip after heat treatment is measured. d It is 6.8 mm / m.

[0040] The finished strip with a thickness of 0.30mm is continuously stretched, bent and straightened on a multi-roller stretch straightening unit. The main process parameters for stretch straightening are: tension: 10KN, stretch straightening speed: 8 m / min.

[0041] The 0.30mm thick finished strip after tension straightening was subjected to stress-relief annealing in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters were: stress-relief annealing temperature: 550℃, strip speed: 35 m / min, and tension of the stress-relief annealed strip: 8KN. Finally, GH4169 alloy strip with good flatness and shape was obtained.

[0042] The horizontal warpage of the finished product was determined by random sampling and testing, as shown in Table 1.

[0043] Example 2: According to another preferred embodiment of the method for controlling the straightness and shape of GH4169 alloy strip of the present invention, the following steps are included in sequence: The original strip blank with a thickness of 3.0 mm is repeatedly rolled and leveled on a multi-roll leveling machine with a single pass reduction of 0.07 mm and a single pass leveling speed of 5 m / min.

[0044] Several flattened original strip blanks are welded into a roll using laser welding. The main laser welding process parameters are: laser power: 500W, welding speed: 8mm / s, argon gas is used as the protective gas, and the argon gas flow rate is controlled at 15 L / min.

[0045] A multi-pass, small-deformation-per-pass cumulative deformation control tension method was adopted to perform initial rolling on the coiled strip, followed by cold rolling in 6 passes. The deformation amounts for each pass were controlled at 16.6%, 14%, 13.3%, 11.7%, 11.6%, and 10.5%, respectively. The rolling force for each pass was 500 kN, the inlet tension was 70 kN, and the outlet tension was 80 kN, resulting in an initial strip thickness of 1.3 mm.

[0046] A 1000mm long test strip was cut from an initial strip material with a thickness of 1.3mm, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the initial strip after billet rolling is measured. d It is 19.2 mm / m.

[0047] The initial strip with a thickness of 1.3 mm was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters for controlled tension heat treatment of the initial strip were: controlled tension of the heat treatment strip at 25 KN, heat treatment temperature at 1050℃, and conveyor speed at 15 m / min.

[0048] Intermediate process rolling is carried out by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method. The cold rolling is carried out in 7 passes, and the deformation amounts of each pass are controlled at 15.0%, 14.3%, 13.6%, 13.3%, 11.7%, 10.5%, and 9%, respectively. The rolling force of each pass is 700KN, the inlet tension is 60KN, and the outlet tension is 75KN, to obtain an intermediate process strip with a thickness of 0.5mm.

[0049] A 1000mm long test strip was cut from the 0.5mm thick intermediate process strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the intermediate strip after intermediate rolling is measured. d It is 12mm / m.

[0050] The 0.5mm intermediate process strip was subjected to tension-controlled heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The process parameters for tension-controlled heat treatment of the intermediate process strip were as follows: tension of the heat treatment strip: 15KN, heat treatment temperature: 1000℃, and conveyor speed: 20 m / min.

[0051] The finished strip was finished by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method. The cold rolling was carried out in 8 passes, with the deformation controlled at 14%, 13.9%, 13.5%, 12.5%, 12%, 10.7%, 10%, and 9% for each pass. The rolling force for each pass was 680 kN, the inlet tension was 46 kN, and the outlet tension was 60 kN, resulting in a finished strip with a thickness of 0.18 mm.

[0052] A 1000mm long test strip was cut from the 0.18mm thick intermediate process strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the finished strip after rolling is measured. d It is 6.2 mm / m.

[0053] The finished strip with a thickness of 0.18 mm was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters for controlled tension heat treatment of the finished strip were: controlled tension of the heat treatment strip: 13 KN, heat treatment temperature: 960℃, and conveyor speed: 26 m / min.

[0054] A 1000mm long test strip was cut from the heat-treated 0.18mm thick finished strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional contour. In this embodiment, the horizontal warpage of the finished strip after heat treatment is measured. d It is 5.5 mm / m.

[0055] The finished strip with a thickness of 0.18mm is continuously stretched, bent and straightened on a multi-roller straightening unit. The main process parameters for straightening are: straightening tension: 8KN, straightening speed: 10 m / min.

[0056] The 0.18mm thick finished strip after tension straightening was subjected to stress-relief annealing in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters were: stress-relief annealing temperature: 500℃, strip speed: 40 m / min, and tension of the stress-relief annealed strip: 6KN. Finally, GH4169 alloy strip with good flatness and shape was obtained.

[0057] The horizontal warpage of the finished product was determined by random sampling and testing, as shown in Table 1.

[0058] Example 3: According to another preferred embodiment of the method for controlling the straightness and shape of GH4169 alloy strip of the present invention, the following steps are included in sequence: The original strip blank with a thickness of 2.0 mm is repeatedly rolled and leveled on a multi-roll leveling machine with a single pass reduction of 0.05 mm and a single pass leveling speed of 7 m / min.

[0059] Several leveled original strip blanks were welded into coils using plasma arc welding. The welding voltage was 15V, the welding current was 120A, and the plasma gas consumption was controlled at 100 L / h.

[0060] A multi-pass, small-deformation-per-pass cumulative deformation control tension method was adopted to perform initial rolling on the coiled strip, followed by cold rolling in 5 passes with controlled deformation amounts of 20%, 19%, 16.6%, 14.3%, and 12.5% ​​for each pass. The rolling force for each pass was 450 kN, the inlet tension was 55 kN, and the outlet tension was 68 kN, resulting in an initial strip thickness of 0.8 mm.

[0061] A 1000mm long test strip was cut from an initial strip with a thickness of 0.8mm. A laser displacement sensor was used to measure the horizontal warpage δ and the three-dimensional profile of the test strip. In this embodiment, the measured horizontal warpage δ of the initial strip after billet rolling was 21.6mm / m.

[0062] The initial strip with a thickness of 0.8 mm was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters for controlled tension heat treatment of the initial strip were: controlled tension of the heat treatment strip at 22 KN, heat treatment temperature at 1060℃, and conveyor speed at 12 m / min.

[0063] Intermediate process rolling is carried out by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method. The intermediate process rolling is carried out in 6 passes, and the deformation amounts of each pass are controlled at 15.5%, 14.2%, 12.5%, 10%, 9%, 8%, and 7%, respectively. The rolling force of each pass is 620KN, the inlet tension is 50KN, and the outlet tension is 65KN, to obtain an intermediate process strip with a thickness of 0.35mm.

[0064] A 1000mm long test strip was cut from the 0.35mm thick intermediate process strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the intermediate strip after intermediate rolling is measured. d It is 4.8 mm / m.

[0065] The 0.35mm intermediate process strip was subjected to tension-controlled heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The process parameters for tension-controlled heat treatment of the intermediate process strip were as follows: tension of the heat treatment strip: 12KN, heat treatment temperature: 950℃, and conveyor speed: 25m / min.

[0066] The finished strip was finished by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method. The cold rolling was carried out in 9 passes, with the deformation controlled at 14.6%, 14.2%, 14.0%, 13.3%, 13%, 12.5%, 12%, 11.1%, and 7.6% for each pass. The rolling force for each pass was 750 kN, the inlet tension was 55 kN, and the outlet tension was 65 kN, resulting in a finished strip with a thickness of 0.1 mm.

[0067] A 1000mm long test strip was cut from the 0.1mm thick intermediate process strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional profile. In this embodiment, the horizontal warpage of the finished strip after rolling is measured. d It is 4.6 mm / m.

[0068] The finished strip with a thickness of 0.1 mm was subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters for controlled tension heat treatment of the finished strip were: controlled tension of the heat treatment strip: 8 KN, heat treatment temperature: 930℃, and conveyor speed: 28 m / min.

[0069] A 1000mm long test strip was cut from the heat-treated 0.1mm thick finished strip, and the horizontal warpage of the test strip was measured using a laser displacement sensor. d and three-dimensional contour. In this embodiment, the horizontal warpage of the finished strip after heat treatment is measured. d It is 3.5 mm / m.

[0070] The 0.1mm thick finished strip after heat treatment was subjected to stress-relief annealing in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. The main process parameters were: stress-relief annealing temperature: 530℃, strip speed: 30 m / min, and tension of the stress-relief annealed strip: 5KN. Finally, GH4169 alloy strip with good flatness and shape was obtained.

[0071] After random sampling and final inspection, the horizontal warpage of the finished product is shown in Table 1.

[0072] Comparative Example 1: The methods, processes, instruments, and equipment used to control the straightness and shape of 0.30mm thick finished strips of GH1469 alloy in this comparative example are the same as in Example 1. The difference is: In this comparative example, the horizontal warpage of the initial strip after billet rolling was measured. d The horizontal warpage of the intermediate strip after intermediate rolling is 22 mm / m. d The horizontal warpage of the finished strip after rolling is 18 mm / m. d The measured horizontal warpage of the finished strip after heat treatment is 11.5 mm / m. d It is 7.9 mm / m.

[0073] The process parameters used for the initial tension-controlled heat treatment of the strip in this comparative example are shown in Table 2.

[0074] The results of the horizontal warpage test of the finished product after random sampling and final inspection are shown in Table 1.

[0075] Comparative Example 2: The methods, processes, instruments, and equipment used to control the straightness and shape of 0.18mm thick GH1469 alloy finished strips in this comparative example are the same as in Example 2. The difference is: In this comparative example, the horizontal warpage of the initial strip after billet rolling was measured. d The measured horizontal warpage of the intermediate strip after intermediate rolling is 19.2 mm / m. d The measured horizontal warpage of the finished strip after rolling is 13.6 mm / m. d The measured horizontal warpage of the finished strip after heat treatment is 7.5 mm / m. dIt is 6.7 mm / m.

[0076] The process parameters used in the intermediate tension heat treatment of the material in this comparative example are shown in Table 2.

[0077] The results of the horizontal warpage test of the finished product after random sampling and final inspection are shown in Table 1.

[0078] Comparative Example 3: The methods, processes, instruments, and equipment used to control the straightness and shape of 0.1mm thick finished strips of GH1469 alloy in this comparative example are the same as in Example 3. The difference is: In this comparative example, the measured horizontal warpage δ of the initial strip after billet rolling was 21.6 mm / m, and the measured horizontal warpage of the strip during the intermediate rolling process was... d The measured horizontal warpage of the finished strip after rolling is 7.95 mm / m. d The measured horizontal warpage of the finished strip after heat treatment is 6.78 mm / m. d It is 5.82 mm / m.

[0079] The process parameters used in this comparative example, including the initial tension-controlled heat treatment of the strip, the intermediate tension-controlled heat treatment of the strip, the finished strip tension-controlled heat treatment, and the finished strip straightening, are shown in Table 2.

[0080] The results of the horizontal warpage test of the finished product after random sampling and final inspection are shown in Table 1.

[0081] Table 1

[0082] Table 2

[0083] As can be seen from Table 1, the horizontal warpage of the GH4169 alloy strip in Examples 1-3 d All values ​​are very low. Lower horizontal warpage indicates better strip straightness, while higher horizontal warpage indicates worse strip straightness. Strip horizontal warpage in each embodiment. d <3mm / m, with a very low horizontal warpage value, meaning that the GH4169 alloy strip produced by this invention has good straightness and shape.

[0084] As can be seen from Table 2, the initial tension control heat treatment process parameters used in Comparative Example 1 are different from the process parameters required by this invention. Combined with Table 1, it can be seen that the horizontal warpage of the GH4169 strip in Comparative Example 1 is higher than that of the strip of the same thickness in Example 1, indicating that the flatness and shape quality of the strip in Comparative Example 1 are worse.

[0085] As can be seen from Table 2, the intermediate process parameters for tension-controlled heat treatment of the strip used in Comparative Example 2 are different from the process parameters required by this invention. Combined with Table 1, it can be seen that the horizontal warpage of the GH4169 strip in Comparative Example 2 is higher than that of the strip of the same thickness in Example 2, indicating that the flatness and shape quality of the strip in Comparative Example 2 are worse.

[0086] As can be seen from Table 2, the initial strip tension control heat treatment, intermediate strip tension control heat treatment, finished strip tension control heat treatment, and finished strip straightening process parameters used in Comparative Example 3 are all different from the process parameters required by this invention. Combined with Table 1, it can be seen that the GH4169 strip in Comparative Example 3 has the highest horizontal warpage, indicating that the straightness and shape quality of the strip in Comparative Example 3 are the worst.

[0087] The technical solution of this invention involves many parameters, and it is necessary to comprehensively consider the synergistic effect between various parameters. Only through a large number of experiments, especially the synergistic control of the process parameters in steps five, eight, eleven, and thirteen, can the beneficial effects and significant progress of this invention be obtained.

[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should be covered within the protection scope of the present invention.

Claims

1. A method for controlling the straightness and shape of GH4169 alloy strip, characterized in that, The process flow is as follows: (1) billet leveling → (2) welding and coiling → (3) controlled tension rolling → (4) flatness and shape measurement → (5) initial strip controlled tension heat treatment → (6) controlled tension intermediate rolling → (7) flatness and shape measurement → (8) intermediate strip controlled tension heat treatment → (9) controlled tension finished product rolling → (10) flatness and shape measurement → (11) finished product strip controlled tension heat treatment → (12) flatness and shape measurement → (13) finished product tension leveling → (14) finished product stress relief annealing; The process parameters for step (5) are as follows: when δ When the thickness is ≥20mm / m, control the tension of the heat treatment belt to be 20~30KN, the heat treatment temperature to be 1050~1100℃, and the belt speed to be 10~20 m / min. When 5mm / m≤ δ When the thickness is <20mm / m, control the tension of the heat treatment belt: 15~25KN, the heat treatment temperature: 1000~1050℃, and the belt speed: 10~20 m / min; when δ When the thickness is <5mm / m, control the tension of the heat treatment belt to be 10-15KN, the heat treatment temperature to be 950-1000℃, and the belt speed to be 10-20 m / min. in, δ The horizontal warpage of the initial strip after billet rolling; The process parameters for step (8) are as follows: when δ When the thickness is ≥20mm / m, control the tension of the heat treatment belt: 15~25KN, the heat treatment temperature: 1050~1080℃, and the belt speed: 10~25 m / min; When 5mm / m≤ δ When the thickness is <20mm / m, control the tension of the heat treatment belt: 10~20KN, the heat treatment temperature: 980~1050℃, and the belt speed: 10~25 m / min; when δ When the tension of the heat treatment belt is <5mm / m, control the belt tension at 10-15KN, the heat treatment temperature at 950-980℃, and the belt speed at 10-25 m / min. in, δ The horizontal warpage of the intermediate strip after intermediate rolling; The process parameters for step (11) are as follows: when δ When the thickness is ≥20mm / m, control the tension of the heat treatment belt: 10~20KN, the heat treatment temperature: 1050~1070℃, and the belt speed: 10~30 m / min; When 5mm / m≤ δ When the thickness is <20mm / m, control the tension of the heat treatment belt: 10~15KN, the heat treatment temperature: 950~1050℃, and the belt speed: 10~30 m / min; when δ When the tension of the heat treatment belt is <5mm / m, control the belt tension as follows: 8-12KN, heat treatment temperature: 930-980℃, and belt speed: 10-30 m / min. in, δ The horizontal warpage of the finished strip after rolling; The process parameters for step (13) are as follows: when δ When the diameter is ≥10mm / m, control the tension of the straightening: 5~15KN, and the straightening speed: 1~5 m / min; When 5 mm / m≤ δ When the tension is <10mm / m, control the tension: 5~10KN and the tension speed: 5~10 m / min; when δ When the thickness is less than 5 mm / m, it is not necessary to straighten the finished strip. in, δ The horizontal warpage of the finished strip after heat treatment.

2. The control method according to claim 1, characterized in that, The process parameters for step (6) are as follows: Cold rolling is performed in 5-8 passes, with the deformation per pass controlled at ≤18%, the rolling force per pass at 500-850KN, the inlet tension at 45-70KN, and the outlet tension at 55-80KN.

3. The control method according to claim 1, characterized in that, The process parameters for step (9) are as follows: Cold rolling is performed in 5-9 passes, with the deformation per pass controlled at ≤15%, the rolling force per pass at 600-900KN, the inlet tension at 40-60KN, and the outlet tension at 50-70KN.

4. The control method according to claim 1, characterized in that, The stress-relief annealing of the finished product in step (14) has the following process parameters: stress-relief annealing process temperature: 500~550℃, belt speed: 15~40 m / min, and stress-relief annealing strip tension: 5~8KN.

5. The control method according to claim 1, characterized in that, The process parameters for step (1) are: single pass reduction amount: 0.01~0.1mm, single pass leveling speed: 0.5~10m / min.

6. The control method according to claim 1, characterized in that, Step (2) Welding is performed using plasma arc welding or laser welding; The plasma arc welding process parameters are: welding voltage: 10V~20V, welding current: 100A~150A, and plasma gas consumption: 50~150 L / h. The laser welding process parameters are as follows: laser power: 300-800W, welding speed: 5-10 mm / s, shielding gas: argon is used as the shielding gas, and the flow rate is controlled at 10-20 L / min.

7. The control method according to claim 1, characterized in that, Step (3) The controlled tension billet rolling process parameters are as follows: cold rolling is carried out in 5-7 passes, the deformation amount of each pass is controlled to be ≤20%, the rolling force of each pass is 400-600KN, the inlet tension is 50-80KN, and the outlet tension is 60-90KN.

8. The control method according to claim 1, characterized in that, The method steps are as follows: Step 1: Blank leveling: The original strip blank in single sheet form is repeatedly rolled and leveled on a multi-roll leveling machine; Step 2, Welding into Coils: Several leveled original strip blanks are welded into coils using plasma arc welding or laser welding methods; Step 3, initial rolling: The coiled strip is rolled using a multi-pass, small-deformation-per-pass cumulative deformation tension control method to obtain the initial strip material; Step 4: Flatness and Shape Measurement: Cut a test strip from the initial strip material and use a laser displacement sensor to measure the horizontal warpage of the test strip. δ and three-dimensional contours; Step 5, Initial heat treatment of the material: The initial material is subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere. Step 6, Intermediate rolling: The intermediate rolling process is carried out by using a multi-pass, small-deformation-per-pass cumulative deformation control tension method to obtain intermediate strip material; Step 7: Flatness and Shape Measurement: Cut a test strip from the intermediate process strip and use a laser displacement sensor to measure the horizontal warpage of the test strip. δ and three-dimensional contours; Step 8, intermediate process material heat treatment: The intermediate process material is subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under a hydrogen protective atmosphere; Step 9, Finished product rolling: The finished product is rolled into finished strip by using a multi-pass, small-deformation-per-pass cumulative deformation tension control method; Step 10: Flatness and Shape Measurement: Cut a test strip from the finished strip and use a laser displacement sensor to measure the horizontal warpage of the test strip. δ and three-dimensional contours; Step 11, Heat treatment of finished product strip: The finished product strip is subjected to controlled tension heat treatment in a continuous bright heat treatment furnace under hydrogen protective atmosphere; Step 12, Flatness and Shape Measurement: Cut a test strip from the heat-treated finished strip and measure the horizontal warpage of the test strip using a laser displacement sensor. δ and three-dimensional contours; Step 13, Finished Product Straightening: The finished strip is continuously stretched, bent and straightened on a multi-roller straightening unit; Step Fourteen: Stress-relief annealing of finished product: The finished strip after tension straightening is subjected to stress-relief annealing in a continuous bright heat treatment furnace under a hydrogen protective atmosphere to finally obtain GH4169 alloy strip with good flatness and shape.

Citation Information

Patent Citations

  • Preparation method of wrought superalloy wide and thin strip

    CN113414551A

  • Method for the production of rolled strip with high strip shape accuracy and flatness

    DE3401894A1