Brazing method for packaging enclosure and packaging enclosure thereof
By forming a continuous nickel layer through chemical nickel plating and electroplating, combined with T-shaped nested welding and multi-stage heating brazing, the problems of high manufacturing cost and low yield of large-size packaging shells are solved, achieving high reliability and low cost in packaging shell manufacturing.
Patent Information
- Application Number
- CN202511068626.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-31
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-07-31
AI Technical Summary
Existing technologies have high manufacturing costs and low yield rates for large-size packaging shells, and the local gold plating process is complex, making it difficult to effectively reduce costs.
A continuous and uniform nickel layer is formed on the chassis using a combination of chemical nickel plating and electroplating. Combined with a T-shaped nested welding structure and a multi-stage heating brazing method, Au80Sn20 eutectic alloy solder is used for welding, which simplifies the gold plating process and improves welding strength and airtightness.
It significantly shortens the preparation process, reduces raw material costs, improves yield, and achieves high reliability and good airtightness, making it suitable for mass production.
Smart Images

Figure CN120662902B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal packaging shell technology, and in particular to a brazing method for packaging shells and the packaging shell thereof. Background Technology
[0002] Eutectic Au80Sn20 solder alloy (melting point 280℃) has been used in semiconductor and microelectronic packaging for many years. Eutectic gold-tin eutectic alloy solder possesses many superior properties, including a low melting point yet high strength, ensuring high reliability of the solder joint; good resistance to thermal fatigue, preventing fatigue fracture due to temperature cycling, allowing use under harsh climate conditions; good oxidation resistance; excellent wetting and flow properties; and high thermal conductivity. Due to its excellent physical properties, gold-tin alloy has gradually become one of the best soldering materials for optoelectronic device packaging.
[0003] Currently, to achieve good weld joint results with gold-tin alloy solder, in addition to reasonable brazing process settings, the temperature is generally set at 310~350℃, and the holding time is 5~10 minutes. There are certain requirements for the plating layer on the surface of the packaged shell to be welded, that is, the surfaces of the two objects to be welded must be gold-plated. This method is invented by making full use of the brazing principle of gold-tin alloy solder. When the solder temperature reaches the eutectic point of 280℃, the solder melts and fully wets and flows on the gold-plated surface. At the same time, the gold plating layer on the surface of the component to be welded will quickly integrate into the gold-tin solder, followed by a reaction with the nickel layer to form an intermetallic compound (IMC layer) between gold, tin and nickel. This alloy layer is the key to ensuring the weld strength and sealing reliability. The gold plating on the surface of the shell welding part is to avoid the nickel plating surface from being oxidized, which would affect the wetting, spreading and reaction of the gold-tin solder at the weld joint, and ultimately affect the weld strength and sealing performance of the joint. Furthermore, the thickness of the gold layer on the casing is generally between 0.5μm and 1.5μm, which will significantly increase the manufacturing cost for large-sized packaging shells used in optoelectronic devices, typically with a length greater than 100mm and a width greater than 80mm.
[0004] To address the market demand for increasingly lower packaging costs, a popular approach is to shift from full gold plating of large-size metal chassis to partial gold plating, specifically plating only the soldered areas. While partial gold plating reduces the cost of gold used in chassis manufacturing, it imposes higher operational and control requirements on the plating process. It necessitates applying adhesive or using custom fixtures to shield the plating, increasing the number of steps, complexity, and time required. Furthermore, the complex plating process inevitably reduces the yield rate of the chassis, and the overall average cost of the plating process remains above 100 yuan. Therefore, the cost reduction for large-size optoelectronic chassis using partial gold plating and gold-tin soldering is limited. Summary of the Invention
[0005] The purpose of this invention is to provide a brazing method for a packaging shell and a packaging shell thereof, so as to solve the problems in the prior art. It can significantly shorten the shell preparation process, reduce raw material costs, improve yield, and has broad application prospects.
[0006] This invention provides a brazing method for a packaged housing, comprising the following steps: The components, including the chassis and connectors, are sandblasted. The parts are chemically nickel-plated and then electroplated with nickel in sequence; The chassis and connecting parts are assembled using a T-shaped nested welding structure to obtain the chassis assembly; The chassis assembly is subjected to multi-stage heating brazing in a vacuum environment to produce the encapsulated shell.
[0007] In this invention, electroless nickel plating serves as the base layer, first forming a continuous and uniform nickel layer on the chassis, providing a complete conductive substrate for subsequent electroplating. Subsequent electroplating can then be uniformly thickened on this basis, avoiding localized plating defects and ensuring overall coating consistency of the outer casing. In contrast, existing technologies only electroless or electroplating nickel onto the chassis, and then sequentially plating nickel and gold layers at the weld joints between the chassis and connectors. During the gold plating process, specialized tools are required for masking, and due to the special shape of the weld holes, the gold plating process is extremely cumbersome. This invention simplifies this step, not only reducing the process difficulty but also decreasing the manufacturing cost of gold plating at the weld joints.
[0008] Traditional brazing methods for packaged housings, in order to ensure airtightness, can only be performed at the welding points of the chassis or on the gold layer of the entire chassis-solder-connector. This invention, by changing the nickel plating method, controlling the thickness of the nickel layer, and performing brazing in a vacuum environment with multi-stage heating, can achieve brazing at the interface between the gold layer of the connector, the solder, and the nickel layer of the chassis, or the interface between the nickel layer of the connector, the solder, and the nickel layer of the chassis. The resulting packaged housing meets the sealing test requirements of Method 1014 of GJB548B-2005 "Test Methods and Procedures for Microelectronic Devices", achieving good airtightness and saving the gold plating process and cost. The manufacturing method of this invention has low process cost and high yield in actual production.
[0009] In the brazing method for the encapsulation shell described above, preferably, the components are obtained by machining from raw materials. The raw materials can be materials conventionally used in the art, such as Kovar alloy or iron-nickel alloy. The machining method is not particularly limited; any conventional machining method in the art is acceptable, including but not limited to milling, stamping, wire cutting, and MIMU machining. It is understood that machining can be performed according to the design dimensions, with the machining accuracy controlled within ±0.02mm.
[0010] In the brazing method for the encapsulation shell described above, preferably, the sandblasting treatment method involves using 200-1000 mesh silicon carbide cutting abrasive at a concentration of 0.5~1.0 kg / cm². 2 The parts are polished under impact, and the roughness is controlled at 0.6~0.8μm.
[0011] In the brazing method for the encapsulation shell described above, preferably, the electroless nickel plating uses a nickel-phosphorus alloy plating solution, wherein the content of each component in each liter of the nickel-phosphorus alloy plating solution is: 240g nickel sulfate, 45g nickel chloride, 3-8g phosphorous acid, and the balance of deionized water; the phosphorus content of the plating layer ranges from 8-12%; the temperature is 85-95℃; the pH value is 4.4-4.8; and the thickness of the nickel layer of the electroless nickel plating is 2.54-5.08μm.
[0012] In the brazing method for the encapsulation shell described above, preferably, the nickel plating uses a nickel sulfamate plating solution, and the content of each component in each liter of the nickel sulfamate plating solution is: 300-450g of nickel sulfamate, 5-15g of nickel chloride, 25-50g of boric acid, 0.1-1.0g of sodium dodecyl sulfonate, with deionized water as the balance, the temperature is 44-54℃, the pH value is 4-5, and the nickel layer thickness of the electroplated nickel is 2.54~5.08μm.
[0013] The purpose of using nickel aminosulfonate in this invention is to reduce the stress of the coating, which helps to alleviate the welding stress between parts made of different materials; the coating surface is dense, not easy to oxidize, and has good wettability and weldability.
[0014] The brazing method for the encapsulation shell described above, wherein preferably, the T-shaped nested welding structure assembly method specifically comprises: opening welding holes on the chassis before sandblasting; cutting a stepped groove on the side of the connector connected to the chassis; the stepped groove being adapted to the size of the welding hole; placing solder on the groove surface of the connector; positioning it to the corresponding welding hole using a graphite mold; and after assembly, the single-sided gap allowance is 0.02~0.05mm.
[0015] Traditional packaging shells have through holes in the chassis for welding to the connectors. However, this invention uses a T-shaped nested welding structure with a larger contact area and better welding effect. It takes into account the difference in thermal expansion coefficients between different materials and ensures the maximum capillary action capability of the gap after assembly. The graphite mold positioning is a conventional process in this field. Its purpose is to position the chassis with the fiber optic tail tube and feedthrough connector respectively, which will not be elaborated here.
[0016] The brazing method for the encapsulation shell described above, preferably, involves the following multi-stage heating brazing method: When the vacuum degree is <1.0×10 -3 Under the condition of Pa, the temperature is first raised from room temperature to 200-250℃ at a heating rate of 5-15℃ / min, and held for 30-60min to fully clean the brazing surfaces of the chassis components. The temperature is increased to 250-270℃ at a rate of 2-5℃ / min, and then held for 5-10 minutes to fully preheat the chassis assembly. Rapidly heat the material to 380-400℃ at a heating rate of 30-50℃ / min, hold it at that temperature for 1-3 minutes, then rapidly cool it down to 260-280℃ at a cooling rate of 30-50℃ / min, and finally cool it down to room temperature at a cooling rate of 5-15℃ / min to complete the brazing.
[0017] The gold-tin solder used in this invention is typically set at 310-350°C and held for 5-10 minutes during the traditional brazing of the package casing. However, in this invention, the temperature is rapidly increased to 400°C to enhance the instantaneous overheating and improve the wettability of the solder on the nickel layer surface. The shortened holding time and rapid cooling are to ensure that the molten solder solidifies quickly, avoiding excessive metallurgical reaction between the solder and the plating layer under high temperature conditions, thus preventing a reduction in welding strength and sealing reliability.
[0018] The present invention also provides a packaging shell, which is manufactured by the above-described brazing method.
[0019] In the encapsulation housing described above, preferably, the connector includes an optical fiber tailpipe and a feedthrough connector, and corresponding welding holes are respectively formed on the chassis. The design method for the diameter of the welding holes is as follows: The welding holes at the fiber optic tail tube are arranged according to diameter Make an opening, where D represents the diameter of the fiber optic tail tube; The welding holes at the feedthrough connector are arranged according to length ,width Make an opening, where L represents the cross-sectional length of the feedthrough connector and W represents the cross-sectional width of the feedthrough connector.
[0020] The design of this welding hole not only meets the requirement of the assembly gap margin, but also allows the solder to fully adhere to the surface of the fiber optic tail tube or feedthrough connector after melting and wetting and flowing. Under capillary action, the solder fully flows and fills along the mating gap direction.
[0021] In the encapsulation housing described above, preferably, the nickel layer surfaces of the fiber optic tail tube and the feedthrough connector can also be plated with a gold layer. When the fiber optic tail tube and the feedthrough connector are plated with a gold layer, the thickness of the nickel layer is 2.54μm~8.9μm and the thickness of the gold layer is 0.5μm~1.5μm.
[0022] This invention can achieve airtightness of the connection between the nickel layer, solder and nickel layer. However, in some cases, at the request of the client, the surface of the connector needs to be plated with a gold layer. Therefore, the connector in this invention can also be plated with a gold layer after the nickel layer is plated. When a gold layer needs to be plated again, the thickness of the nickel layer can be relatively thin.
[0023] Compared with existing technologies, this invention achieves the replacement of the traditional gold-solder-gold interface with a nickel-solder-nickel interface, achieving the same welding strength and sealing reliability requirements for the welded joint. The high-reliability packaging shell prepared using this invention significantly shortens the overall manufacturing process, and components can be plated with only a nickel layer, which saves gold plating, significantly improves the plating yield, reduces the overall manufacturing cost, and has good potential for widespread application. Attached Figure Description
[0024] Figure 1 This is a flowchart of a brazing method for a package housing provided by an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of the encapsulation shell of a brazing method for an encapsulation shell provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of the connection of an optical fiber tail tube according to a brazing method for a packaged shell provided in an embodiment of the present invention. Figure 4 This is a schematic diagram of the connection of a feedthrough connector according to a brazing method for a packaged housing provided in an embodiment of the present invention; Figure 5 This is a temperature curve diagram in step S4 of the brazing method for a packaged housing according to the present invention.
[0025] Explanation of reference numerals in the attached figures: 1. Chassis; 2. Fiber optic tail tube; 3. Feeder connector; 4. Welding hole; 40. Recess; 5. Groove; 6. Solder. Detailed Implementation
[0026] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0027] Example 1 See Figure 2 As shown, the structure of the encapsulation shell obtained in this embodiment includes components such as a chassis 1, an optical fiber tail tube 2, and a feedthrough connector 3. The chassis 1 has welding holes 4 for connecting and assembling the optical fiber tail tube 2 and the feedthrough connector 3. It should be noted that the encapsulation shell structure shown in this embodiment is only a specific example; other conventional encapsulation shells in the art are also applicable.
[0028] Any range described in this invention includes the endpoint, any value between the endpoints, and any subrange consisting of the endpoint or any value between the endpoints.
[0029] In this embodiment, welding holes 4 are opened on the machined chassis 1. The cross-section of the welding holes 4 is stepped, with one side communicating with the interior of the chassis 1 and the other side forming a recess 40 on the surface of the chassis 1. Stepped grooves 5 are cut on the surfaces where the fiber optic tail tube 2 and the feedthrough connector 3 are connected to the chassis 1. The fiber optic tail tube 2 and the feedthrough connector 3 are connected to the chassis 1 through the welding holes 4. The bottom wall of the groove 5 abuts against the recess 40 on the surface of the chassis 1. During brazing, solder 6 is first placed on the contact surface between the fiber optic tail tube 2 and the feedthrough connector 3. The solder 6 is made of Au80Sn20 eutectic alloy and is positioned to the corresponding welding holes 4 by a graphite mold. After assembly, the single-sided gap margin is 0.02~0.05mm.
[0030] In this embodiment, the design method for the diameter of the welding hole 4 is as follows: Welding hole 4 at fiber optic tail tube 2 according to diameter Make an opening, where D represents the diameter of the fiber optic tail tube 2; The welding hole 4 at feedthrough connector 3 is arranged according to length ,width Make an opening, where L represents the cross-sectional length of feedthrough connector 3 and W represents the cross-sectional width of feedthrough connector 3.
[0031] The soldering method for the package housing is as follows: Use 200-1000 mesh silicon carbide cutting abrasive at a concentration of 0.5~1.0 kg / cm². 2 The parts are polished under impact, and the roughness is controlled at 0.6~0.8μm; The parts are sequentially electroless nickel plated and then electroplated with nickel, wherein: The electroless nickel plating uses a nickel-phosphorus alloy plating solution. The content of each component in each liter of the nickel-phosphorus alloy plating solution is as follows: 240g of nickel sulfate, 45g of nickel chloride, 5g of phosphorous acid, and the balance of deionized water. The phosphorus content of the plating layer is 10%, the temperature is 90℃, the pH value is 4.6, and the thickness of the nickel layer in the electroless nickel plating is 3.81μm. The nickel plating process uses a nickel sulfamate plating solution. The components in each liter of the nickel sulfamate plating solution are: 375g nickel sulfamate, 10g nickel chloride, 40g boric acid, 1g sodium dodecyl sulfonate, and the balance being deionized water. The temperature is 49℃, the pH value is 4.5, and the nickel layer thickness is 3.81μm. After this step, the overall thickness of the nickel plating layer is 7.62μm. The assembled chassis assembly was placed in a vacuum brazing furnace at a vacuum degree of 5.0 × 10⁻⁶. -4 Under the condition of Pa, the temperature is increased from room temperature to 225℃ at a heating rate of 10℃ / min and held for 45min to fully clean all brazing surfaces of the chassis assembly; the temperature is increased to 270℃ at a heating rate of 35℃ / min and held for 10min to fully preheat the chassis assembly; the temperature is rapidly increased to 400℃ at a heating rate of 35℃ / min and held for 2min; the temperature is then rapidly decreased to 265℃ at a cooling rate of 45℃ / min; and finally, the temperature is cooled to room temperature at a cooling rate of 15℃ / min to complete the brazing.
[0032] Figure 5 The temperature curves for the multi-stage heating brazing process in this embodiment are shown below. T1 represents the temperature rising to 225°C, t1 represents the holding time for 45 minutes, T2 represents the temperature rising to 270°C, t2 represents the holding time for 10 minutes, T3 represents the rapid temperature rising to 400°C, t3 represents the holding time for 2 minutes, and after t3, the temperature rapidly decreases to 265°C and finally decreases to room temperature.
[0033] Example 2 The difference from Example 1 is that the fiber optic tail tube 2 and the feedthrough connector 3 are plated with a nickel layer and then a gold layer, with the nickel layer having a thickness of 3.78 μm and the gold layer having a thickness of 0.8 μm.
[0034] Example 3 The difference from Example 1 is as follows: The content of each component in each liter of nickel-phosphorus alloy plating solution for electroless nickel plating is as follows: 240g nickel sulfate, 45g nickel chloride, 3g phosphorous acid, and the balance of deionized water. The phosphorus content of the plating layer is within the range of 10%, the temperature is 85℃, the pH value is 4.5, and the thickness of the nickel layer in electroless nickel plating is 2.54μm. The composition of each component in the nickel sulfamate plating solution per liter is as follows: 300g nickel sulfamate, 5g nickel chloride, 30g boric acid, 0.5g sodium dodecyl sulfonate, and the balance of deionized water. The temperature is 46℃, the pH value is 4, the nickel layer thickness of the electroplated nickel is 2.54μm, and the overall nickel layer thickness is 5.08μm. The assembled chassis assembly was placed in a vacuum brazing furnace at a vacuum degree of 6.0 × 10⁻⁶. -4 Under the conditions of Pa, the temperature is first increased from room temperature to 200℃ at a heating rate of 5℃ / min, and held for 45min to thoroughly clean all brazing surfaces of the chassis assembly. The temperature is then increased to 250℃ at a heating rate of 3℃ / min and held for 6min to fully preheat the chassis assembly. The temperature is then rapidly increased to 380℃ at a heating rate of 30℃ / min and held for 1min. The temperature is then rapidly decreased to 260℃ at a cooling rate of 30℃ / min and finally cooled to room temperature at a cooling rate of 5℃ / min to complete the brazing.
[0035] Example 4 The difference from Example 1 is as follows: The content of each component in each liter of nickel-phosphorus alloy plating solution for electroless nickel plating is as follows: 240g nickel sulfate, 45g nickel chloride, 5g phosphorous acid, and the balance of deionized water. The phosphorus content of the plating layer is 8%, the temperature is 88℃, the pH value is 4.4, and the thickness of the nickel layer in electroless nickel plating is 3.52μm. The composition of each component in the nickel sulfamate plating solution per liter is as follows: nickel sulfamate 410g, nickel chloride 12g, boric acid 38g, sodium dodecyl sulfonate 0.1g, deionized water balance, temperature 44℃, pH value 5, nickel layer thickness of the electroplated nickel is 3.04μm, and the overall nickel layer thickness is 6.56μm. The assembled chassis assembly was placed in a vacuum brazing furnace at a vacuum degree of 3.0 × 10⁻⁶. -4 Under the condition of Pa, the temperature is first increased from room temperature to 220℃ at a heating rate of 10℃ / min, and held for 30min to fully clean all brazing surfaces of the chassis assembly. The temperature is then increased to 255℃ at a heating rate of 2℃ / min, and held for 5min to fully clean the chassis assembly. The temperature is then rapidly increased to 385℃ at a heating rate of 35℃ / min, and held for 2min. The temperature is then rapidly decreased to 270℃ at a cooling rate of 35℃ / min, and finally cooled to room temperature at a cooling rate of 12℃ / min to complete the brazing.
[0036] Example 5 The difference from Example 1 is as follows: The content of each component in each liter of nickel-phosphorus alloy plating solution for electroless nickel plating is as follows: 240g nickel sulfate, 45g nickel chloride, 8g phosphorous acid, and the balance of deionized water. The phosphorus content of the plating layer is 12%, the temperature is 95℃, the pH value is 4.8, and the thickness of the nickel layer in electroless nickel plating is 5.08μm. The composition of each component in the nickel sulfamate plating solution per liter is as follows: nickel sulfamate 450g, nickel chloride 15g, boric acid 50g, sodium dodecyl sulfonate 1.0g, deionized water balance, temperature 54℃, pH value 5, nickel layer thickness of the electroplated nickel is 4.88μm, and the overall nickel layer thickness is 9.96μm. The assembled chassis assembly was placed in a vacuum brazing furnace at a vacuum degree of 8.0 × 10⁻⁶. -4 Under the condition of Pa, the temperature is first increased from room temperature to 250℃ at a heating rate of 15℃ / min and held for 60min to thoroughly clean all brazing surfaces of the chassis assembly. The temperature is then increased to 270℃ at a heating rate of 5℃ / min and held for 10min to fully preheat the chassis assembly. The temperature is then rapidly increased to 400℃ at a heating rate of 50℃ / min and held for 3min. The temperature is then rapidly decreased to 280℃ at a cooling rate of 50℃ / min and finally cooled to room temperature at a cooling rate of 15℃ / min to complete the brazing.
[0037] Through testing, the packaging shells obtained in Examples 1-4 all met the sealing test requirements of Method 1014 of GJB548B-2005 "Test Methods and Procedures for Microelectronic Devices". Example 1 will be used as an example below, along with comparative examples, for illustration.
[0038] Comparative Example This comparative example uses a commonly used local gold plating method in the prior art, employing the same implementation method as Example 1, except that: the chassis 1 is only subjected to either chemical nickel plating or electroplating nickel plating, with a nickel layer thickness of 3μm; the welding hole 4 is sequentially plated with a nickel layer and a gold layer, with a nickel layer thickness of 4μm and a gold layer thickness of 1.0μm; the fiber optic tail tube 2 and the feedthrough connector 3 are sequentially plated with a nickel layer and a gold layer, with a nickel layer thickness of 5μm and a gold layer thickness of 0.9μm; and the brazing method in step S4 is to braze at 320℃ for 10 minutes. Five samples after brazing in Example 1 (numbered 1-5), five samples after brazing in Example 2 (numbered 6-10), and five samples from the comparative example (numbered 11-15) were randomly selected and tested for sealing performance according to Method 1014 of GJB548B-2005 "Test Methods and Procedures for Microelectronic Devices". The results are shown in the table below:
[0039] After testing, the airtightness of all 10 samples (numbered 1-10) prepared by this invention was found to be qualified, with all values less than 1.0 × 10⁻⁶. -8 Pa.m 3 .s -1 It can achieve the same or even better airtight effect as the comparative ratio.
[0040] Further, samples 1-10 and comparative samples 11-15 were subjected to 100 temperature cycles from -65℃ to +150℃ and 15 thermal shock cycles from -55℃ to +125℃, according to the environmental testing requirements of GJB2440A-2006 "General Specifications for Hybrid Integrated Circuit Housings". The purpose was to test whether the packaged housing obtained by this method could still maintain good sealing performance after the shock test. After the test, the airtightness was tested according to method 1014 of GJB548B-2005 "Test Methods and Procedures for Microelectronic Devices". The airtightness was qualified in all cases, and the sealing performance was less than 1.0 × 10⁻⁶. -8 Pa.m 3 .s -1 The results are shown in the table below:
[0041] Furthermore, for samples 1-10 and comparative samples 11-15, the welding strength tensile test of feedthrough connector 3 and fiber optic tail tube 2 was conducted according to the method in GJB548B-2005 "Test Methods and Procedures for Microelectronic Devices". The results are shown in the table below:
[0042] As can be seen from the comparison of the above tables, the present invention can maintain excellent welding reliability even when only nickel is plated on the chassis 1, fiber optic tail tube 2, and feedthrough connector 3, or when nickel is plated on the chassis 1 and nickel and gold are plated on the fiber optic tail tube 2 and feedthrough connector 3, which greatly reduces the difficulty of local gold plating on large and complex chassis 1.
[0043] The high-reliability packaging shell achieved by utilizing the brazing method and brazing structure of the present invention only requires nickel plating on the chassis 1 as a base and then electroplating a layer of nickel sulfamate. It eliminates the need for the chassis 1 to be nickel-plated first and then locally gold-plated, thereby greatly reducing the difficulty of local gold plating on large and complex chassis 1. It is easy to operate and suitable for mass production.
[0044] The fiber optic tail tube 2 and feedthrough connector 3 can be nickel-plated according to the method of this invention, or retain the gold-plated surface according to customer requirements, which can meet customer needs such as low-temperature soldering. The chassis 1 cavity only uses a nickel-plated surface to meet customer needs such as adhesive bonding. This invention realizes the welding of nickel-solder-gold interface and nickel-solder-nickel interface to replace the traditional gold-solder-gold interface, saving the process steps of local gold plating, reducing the difficulty of gold plating, and saving gold plating costs. This invention not only ensures the high reliability and low cost manufacturing requirements of the packaging shell, but also meets the micro-assembly requirements of traditional packaging shells, significantly improves the plating yield, and significantly reduces the overall manufacturing cost, and has good potential for promotion and application.
[0045] The above description, based on the embodiments shown in the figures, details the structure, features, and effects of the present invention. The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown in the figures. Any changes made in accordance with the concept of the present invention, or equivalent embodiments modified to have equivalent changes, that do not exceed the spirit covered by the specification and figures, should be within the protection scope of the present invention.
Claims
1. A brazing method for a packaged casing, characterized in that, Includes the following steps: The components, including the chassis and connectors, are sandblasted. The parts are chemically nickel-plated and then electroplated with nickel in sequence; The electroless nickel plating uses a nickel-phosphorus alloy plating solution. The content of each component in each liter of the nickel-phosphorus alloy plating solution is as follows: 240g of nickel sulfate, 45g of nickel chloride, 3-8g of phosphorous acid, and the balance of deionized water. The phosphorus content of the plating layer ranges from 8 to 12%, the temperature is 85-95℃, the pH value is 4.4-4.8, and the thickness of the nickel layer of the electroless nickel plating is 2.54-5.08μm. The electroplating of nickel uses a nickel sulfamate plating solution. The content of each component in each liter of the nickel sulfamate plating solution is as follows: 300-450g of nickel sulfamate, 5-15g of nickel chloride, 25-50g of boric acid, 0.1-1.0g of sodium dodecyl sulfonate, and the balance of deionized water. The temperature is 44-54℃, the pH value is 4-5, and the thickness of the nickel layer of the electroplated nickel is 2.54~5.08μm. The chassis and connectors are assembled using a T-shaped nested welding structure to obtain a chassis assembly. The T-shaped nested welding structure assembly method is as follows: before sandblasting, welding holes are opened on the chassis; a stepped groove is cut on the side of the connector that connects to the chassis; the stepped groove is adapted to the size of the welding hole; solder is placed on the groove surface of the connector; and the connector is positioned to the corresponding welding hole using a graphite mold. After assembly, the single-sided gap allowance is 0.02~0.05mm. The chassis assembly is subjected to multi-stage heating brazing in a vacuum environment to obtain the encapsulated shell; The multi-stage heating brazing method is as follows: When the vacuum degree is <1.0×10 -3 Under the condition of Pa, the temperature is first raised from room temperature to 200-250℃ at a heating rate of 5-15℃ / min, and held for 30-60min to fully clean the brazing surfaces of the chassis components. The temperature is increased to 250-270℃ at a rate of 2-5℃ / min, and then held for 5-10 minutes to fully preheat the chassis assembly. Rapidly heat to 380-400℃ at a heating rate of 30-50℃ / min, hold for 1-3 minutes, then rapidly cool to 260-280℃ at a cooling rate of 30-50℃ / min, and finally cool to room temperature at a cooling rate of 5-15℃ / min to complete the brazing. The components are made of Kovar alloy or iron-nickel alloy.
2. The brazing method for the encapsulation shell according to claim 1, characterized in that, The parts are obtained from raw materials through mechanical processing, with the processing accuracy controlled within ±0.02mm.
3. The brazing method for the encapsulation shell according to claim 1, characterized in that, The sandblasting method is as follows: using 200-1000 mesh silicon carbide cutting abrasive at a concentration of 0.5~1.0 kg / cm². 2 The parts are polished under impact, and the roughness is controlled at 0.6~0.8μm.
4. The brazing method for the encapsulation shell according to claim 1, characterized in that, The connector includes an optical fiber tailpipe and a feedthrough connector. Corresponding welding holes are formed on the chassis. The design method for the diameter of the welding holes is as follows: The welding holes at the fiber optic tail tube are arranged according to diameter Make an opening, where D represents the diameter of the fiber optic tail tube; The welding holes at the feedthrough connector are arranged according to length ,width Make an opening, where L represents the cross-sectional length of the feedthrough connector and W represents the cross-sectional width of the feedthrough connector.
5. The brazing method for the encapsulation shell according to claim 4, characterized in that, The nickel layer of the fiber optic tail tube and the feedthrough connector is plated with a gold layer, the nickel layer thickness being 2.54μm~8.9μm and the gold layer thickness being 0.5μm~1.5μm.
6. A packaging shell, characterized in that, It is produced by the brazing method described in any one of claims 1-5.
Citation Information
Patent Citations
Machining method of micro-rectangular electric connector
CN110026744A
Small-size heterogeneous eutectic method based on multiple chips
CN113808964A
Diamond / copper composite material plating process
CN117165942A
Ceramic relay shell secondary metallization nickel electroplating pretreatment process