Cold heading process for taper forging
By optimizing the forging process and mold design, the problem of low forging yield was solved, and efficient forging production was achieved.
Patent Information
- Application Number
- CN202511145802.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-15
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-08-15
AI Technical Summary
The low yield of forgings is mainly due to the problem of the forming sequence of corresponding structures on the forgings.
By rationally designing the forming process of forgings, including steps such as cutting, chamfering, forming of reduced bar sections, forming of inner holes and forming of shoulders, and using specific molds for cold heading, the influence of the clamping process on size and shape is avoided, and the mold structure is optimized for easy operation.
It improved the yield of forgings, reduced the need for workshop equipment, and simplified the operation process.
Smart Images

Figure CN120696336B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cold heading technology, specifically to the cold heading process for tapered forgings. Background Technology
[0002] like Figure 1 The forging shown is mainly used in the receiving parts of drill bit excavation equipment. It is mainly formed by cold heading process. However, due to the problem of the forming sequence of the corresponding structure on the forging, the yield of the forging is not high and needs to be improved. Summary of the Invention
[0003] To address at least one of the aforementioned technical deficiencies, the present invention provides the following technical solution:
[0004] This application discloses a cold heading process for tapered forgings, including the following steps:
[0005] Step 1: Cut the raw material into the required dimensions for the forging;
[0006] The second step is to chamfer the tail of the raw material part, i.e., preform part one;
[0007] The third step is to reduce the lower shaft diameter of preform part one by cold heading process to preform the first shrink bar section, i.e., preform part two.
[0008] Step 4: The shaft diameter above the first shrinking section of preform 2 is reduced by cold heading process to form the second stepped section, i.e., preform 3;
[0009] Step 5: Form an inner hole on the first end face of preform 3 and reduce the first end shaft diameter of preform 3, i.e., preform 4;
[0010] Step 6: By using cold heading process, the overall length of the preform part 4 is shortened and the shaft between the upper part of the second step bar segment and the first end where the inner hole is located is expanded and a shoulder is formed at intervals. At the same time, the upper peripheral wall of the shoulder is made to match the taper of the lower part of the first end where the inner hole is located, and the second step bar segment is made to be tapered, i.e., preform part 5.
[0011] Step 7: Using cold heading process, the first shortened rod section and the second stepped rod section in the preform part 5 are connected to form a cone shape, which shortens the length of the preform part 5 and simultaneously expands the tail end of the preform part 5 to be larger than the diameter of the tail of the cone, which is the required forging.
[0012] This solution rationally designs the forging process. The first step is to cut and shape the raw material. The second and third steps are to pre-shape the chamfer and the first shrinkage section of the raw material. In the fourth step, the second step section is formed to facilitate the clamping of the subsequent clamps. In the fifth step, the inner hole is formed first, and the shoulder is formed in subsequent steps to avoid dimensional deformation of other parts when forming the inner hole. The first shrinkage section needs to be clamped and moved, so it is formed last, at which point clamping is no longer required, reducing the impact of the clamping process on the size or shape of the product. Under this forming process, the yield of forgings is high.
[0013] Furthermore, in the second step, the bottom of the raw material is squeezed and chamfered by impact with a punch, which facilitates operation through cold heading molds, and the workshop does not need to install other chamfering devices.
[0014] Furthermore, in the fifth step, the top of the preform three is formed with an inner hole by a punch, which facilitates operation through a cold heading die, eliminating the need for other hole-making devices in the workshop.
[0015] Furthermore, the mold used in the cold heading process includes a bottom mold and a moving mold. The bottom mold includes a lower mold outer sleeve, a lower mold middle sleeve, a mold pad, a mold core, and a punch. The mold pad is provided at the bottom opening of the lower mold outer sleeve. The lower mold middle sleeve is elastically and telescopically connected to the cavity of the lower mold outer sleeve. The lower mold middle sleeve has a tapered cavity in which the mold core is axially slidably connected. The mold core is composed of multiple mold segments, and adjacent mold segments are elastically connected to return to the open state. The mold pad has a mold cavity, and an alloy sleeve is provided at the first end of the mold cavity. The punch is located in the mold cavity of the mold pad, and its end extends into the cavity of the alloy sleeve. A pusher pad is provided at the tail end of the punch. The mold is reasonably designed to facilitate the forming of the first shrinkage section.
[0016] Furthermore, the moving mold includes an upper mold outer sleeve, an ejector pin, a sleeve, a second punch, a positioning plate, a fixing ring, and a thick pad. The positioning plate, the fixing ring, and the thick pad are fixed inside the cavity of the upper mold outer sleeve. The fixing ring is fitted onto the sleeve and the two are slidably engaged. The positioning plate is located between the thick pad and the fixing ring. The sleeve is fitted onto the second punch and the two are slidably engaged. An ejector pin is provided at the tail end of the sleeve, and a second pusher thick pad is provided at the tail end of the second punch to facilitate the forming of the inner hole of the forging head.
[0017] Furthermore, the forging has a shoulder at the middle interval, a groove between the two shoulders, the forging above the upper shoulder is in the shape of a shortened rod, the forging below the lower shoulder is in the shape of a shortened rod, the tail of the forging is outwardly flared, and the head end face of the forging is formed with an inner hole.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] 1. The present invention rationally designs the forming process of forgings, which can improve the yield of forgings. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 This is a schematic diagram of the structure of this forging;
[0022] Figure 2 This is a structural diagram of a cold heading die;
[0023] Figure 3 This is a structural schematic diagram of the raw material and the preform.
[0024] Figure 4 These are structural schematic diagrams of preform two and preform three;
[0025] Figure 5 These are structural schematic diagrams of preform four and preform five;
[0026] Figure 6 This is a schematic diagram of the structure of this forging;
[0027] The attached figures are labeled as follows:
[0028] 1. Moving mold; 2. Bottom mold; 3. Shoulder; 4. Inner hole; 11. Upper mold outer sleeve; 12. Fixing ring; 13. Ejector pin; 14. Punch bar two; 15. Sleeve; 16. Positioning plate; 17. Thick pad; 18. Ejector thick pad two; 21. Lower mold outer sleeve; 22. Lower mold middle sleeve; 23. Lower mold cover plate; 24. Mold core; 25. Spring; 26. Punch bar one; 27. Mold pad; 28. Alloy sleeve; 29. Ejector thick pad one. Detailed Implementation
[0029] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0030] Example 1
[0031] The structure of the forging is as follows Figure 1 As shown, the forging has a shoulder 3 in the middle, and a groove is formed between the two shoulders 3. The forging is in the shape of a truncated rod above the upper shoulder and below the lower shoulder. The tail of the forging is outwardly flared, and the head end face of the forging is formed with an inner hole.
[0032] The basic configuration of the cold heading die used is as follows: Figure 2As shown, it includes a bottom mold 2 and a moving mold 1. The bottom mold 2 includes a lower mold outer sleeve 21, a lower mold middle sleeve 22, a mold pad 27, a mold core 24, and a punch 26. The mold pad 27 is fixed at the bottom opening of the lower mold outer sleeve 21. The lower mold middle sleeve 22 is elastically connected to the cavity at the front end of the lower mold outer sleeve 21 by a spring. The lower mold middle sleeve 22 has a tapered cavity in which the mold core 24 is slidably connected along the axial direction. The mold core is composed of four common mold segments, and adjacent mold segments are also elastically connected by springs. The springs are used to reset the mold segments to the open state (for the connection structure of the springs, please refer to the scheme described in patent CN102248109A).
[0033] The die pad 27 has a die cavity, and an alloy sleeve 28 is fixed at the opening of the die cavity. The punch 26 is located in the die cavity of the die pad 27, and its first end extends into the cavity of the alloy sleeve 28. The pusher pad 29 is placed at the tail end of the punch 26. The required configuration of the corresponding part of the forging can be formed by changing the configuration of the die petals in the die core.
[0034] The moving mold 1 includes an upper mold outer sleeve 11, ejector pins 13, a sleeve 15, a second punch 14, a positioning plate 16, a retaining ring 12, and a thick pad 17. The positioning plate 16, retaining ring 12, and thick pad 17 are fixed inside the cavity of the upper mold outer sleeve 11. The retaining ring 12 is fitted onto the sleeve 15 and the two are in sliding engagement. The positioning plate 16 is located between the thick pad 17 and the retaining ring 12, supporting the thick pad. The sleeve 15 is fitted onto the second punch 14 and the two are in sliding engagement. An ejector pin 13 is installed at the tail end of the sleeve 15. If there are three ejector pins, the ejector pins push the sleeve in front to facilitate the forging's removal. A second pusher thick pad 18 is installed at the tail end of the second punch.
[0035] The cold heading process for tapered forgings includes the following steps:
[0036] The first step is to cut the raw material to the required size for the forging using a die, such as... Figure 3 As shown.
[0037] The second step involves placing the raw material part in the corresponding cold heading die. The punch is then pressed down, and with the cooperation of the corresponding die core, the tail of the raw material part is extruded and formed into a chamfer, thus creating pre-formed part one. Figure 3 As shown.
[0038] The third step involves placing preform 1 at the corresponding cold heading die, and pressing it down with punch 2. Under the cooperation of the corresponding die core, the lower shaft diameter of preform 1 is reduced to preform the first shrinkage section, i.e., preform 2. Figure 4 As shown.
[0039] Step 4: Using a cold heading process, the shaft diameter above the first shortened section of preform 2 is reduced to form the second stepped section, i.e., preform 3, as shown below. Figure 4 As shown.
[0040] Step 5: Place preform 3 at the corresponding cold heading die, and use punch 2 to press down to impact the first end face of preform 3 to form an indentation, thus completing the inner hole forming and reducing the first end shaft diameter of preform 3, resulting in preform 4. Figure 5 As shown.
[0041] Step 6: Place preform 4 at the corresponding cold heading die. Press down with punch 2, and with the corresponding die core, use cold heading to shorten the overall length of preform 4. Expand the shaft between the upper part of the second step section and the first end where the inner hole is located, and form shoulders at intervals. Create a groove between the two shoulders. Simultaneously, make the upper peripheral wall of the upper shoulder match the taper of the lower part of the first end where the inner hole is located, and make the second step section tapered, i.e., preform 5. Figure 5 As shown.
[0042] Step 7: Place the preform five at the corresponding cold heading die. Press down with the punch two, and with the corresponding die core, use the cold heading process to connect the first shortened section and the second stepped section of the preform five to form a cone shape. This shortens the length of the preform five and simultaneously expands the tail end of the preform five to a diameter greater than the tail diameter of the cone, thus creating the desired forging. Figure 1 , Figure 6 As shown.
[0043] The above are merely preferred embodiments of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principle of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A cold heading process for a tapered forging, wherein the forging has a shoulder (3) at the middle interval, a groove is formed between the two shoulders, the forging is in the shape of a tapered rod above the upper shoulder, the forging is in the shape of a tapered rod below the lower shoulder, the tail of the forging is outwardly flared, and the head end face of the forging is formed with an inner hole (4), characterized in that, Includes the following steps: Step 1: Cut the raw material into the required dimensions for the forging; The second step is to chamfer the tail of the raw material part, i.e., preform part one; The third step is to reduce the lower shaft diameter of preform part one by using a cold heading process to preform the first shrinking rod section, which is preform part two. Step 4: The shaft diameter above the first shrinking section of preform 2 is reduced by cold heading process to form the second stepped section, i.e., preform 3; Step 5: Form an inner hole on the first end face of preform 3 and reduce the first end shaft diameter of preform 3, i.e., preform 4; Step 6: By using cold heading process, the overall length of the preform part 4 is shortened and the shaft between the upper part of the second step bar segment and the first end where the inner hole is located is expanded and a shoulder is formed at intervals. At the same time, the upper peripheral wall of the shoulder is made to match the taper of the lower part of the first end where the inner hole is located, and the second step bar segment is made to be tapered, i.e., preform part 5. Step 7: Using cold heading process, the first shortened rod section and the second stepped rod section in the preform part 5 are connected to form a cone shape, which shortens the length of the preform part 5 and simultaneously expands the tail end of the preform part 5 to be larger than the diameter of the tail of the cone, which is the required forging.
2. The cold heading process for the tapered forging as described in claim 1, characterized in that: In the second step, the bottom end of the raw material is squeezed and chamfered by impact with a punch.
3. The cold heading process for the tapered forging as described in claim 1, characterized in that: In the fifth step, the top of the preform three is formed into an inner hole by using a punch.
4. The cold heading process for the tapered forging as described in claim 1, characterized in that: The mold used in the cold heading process includes a bottom mold (2) and a moving mold (1). The bottom mold (2) includes a lower mold outer sleeve (21), a lower mold middle sleeve (22), a mold pad (27), a mold core (24), and a punch (26). The mold pad (27) is provided at the bottom opening of the lower mold outer sleeve. The lower mold middle sleeve (22) is elastically telescopically connected in the cavity of the lower mold outer sleeve (21). The lower mold middle sleeve (22) has a tapered cavity and the mold core (24) is axially slidably connected in the cavity. The mold core is composed of multiple mold pieces, and adjacent mold pieces are elastically connected to reset to the open state. The mold pad (27) has a mold cavity and an alloy sleeve (28) is provided at the first end of the mold cavity. The punch (26) is located in the mold cavity of the mold pad and its end extends into the cavity of the alloy sleeve. A pusher pad (29) is provided at the tail end of the punch.
5. The cold heading process for the tapered forging as described in claim 4, characterized in that: The moving mold (1) includes an upper mold outer sleeve (11), an ejector pin (13), a sleeve (15), a second punch (14), a positioning plate (16), a fixing ring (12), and a thick pad (17). The positioning plate (16), the fixing ring (12), and the thick pad (17) are fixed inside the cavity of the upper mold outer sleeve (11). The fixing ring (12) is fitted on the sleeve (15) and the two are slidably engaged. The positioning plate (16) is located between the thick pad (17) and the fixing ring (12). The sleeve (15) is fitted on the second punch (14) and the two are slidably engaged. An ejector pin (13) is provided at the tail end of the sleeve (15), and a second pusher thick pad (18) is provided at the tail end of the second punch.
Citation Information
Patent Citations
Cold heading forming die
CN102248109A
Forming tool and forming method for large forge piece with flange deep blind hole
CN120023281A
Cold heading die capable of heading parts with rod bosses