Composite ferrite, method for producing the same, circulator, and use thereof
By integrating permanent magnet ferrite and rotary magnet ferrite into one, composite ferrite is prepared, which solves the problems of damage and high cost of thin sheet structure in circulators, and realizes efficient production and low-cost manufacturing of circulators.
Patent Information
- Application Number
- CN202510916952.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-03
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-07-03
AI Technical Summary
The thin-film structure of existing circulators, including spin magnet ferrite sheets and permanent magnet ferrite sheets, is prone to breakage during assembly, resulting in high production costs, environmental pollution, and strict requirements for flatness.
Composite ferrite is used to integrate permanent magnet ferrite and gyromagnetic ferrite into a whole structure, avoiding the stacking of thin sheet structures. The composite ferrite is prepared by dry pressing and sintering, including a permanent magnet ferrite layer, a gyromagnetic ferrite layer and a central conductor.
It reduces production costs, avoids damage to the thin sheet structure, simplifies processing procedures, improves production efficiency, and meets the signal transmission requirements of the circulator.
Smart Images

Figure CN120709018B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ferrite preparation technology, specifically relating to a composite ferrite, its preparation method, circulator, and applications. Background Technology
[0002] Circulators can transmit high-frequency signals in one direction and play roles such as circulation, isolation, and amplitude modulation in microwave circuits. They are mainly used in military radar systems and communications. With the large-scale construction of 5G base stations in recent years, the demand for circulators has increased significantly, which has also placed higher demands on their production costs and reliability.
[0003] Existing circulators, such as those shown in the attached document Figure 1 As shown, the structure includes a shell (7), a central conductor (1), a ferrite sheet (2), a grounding plate (3), an anti-rotation component (4), a permanent magnet ferrite sheet (5), and a cover plate (6). The cover plate (6) and the shell (7) form a cavity, in which the ferrite sheet, the permanent magnet ferrite sheet, the central conductor, etc., are placed. In the above structure: the ferrite sheet and the permanent magnet ferrite sheet are both thin sheet structures, which need to be stacked with metal sheets when assembled into a ring, making them prone to damage during production, transportation, and assembly. The stacking method requires strict requirements on the flatness of the ferrite sheet and the permanent magnet ferrite sheet after surface grinding. At the same time, electroplating is performed on the surface of the ferrite sheet and the permanent magnet ferrite sheet, resulting in high production costs and environmental pollution. Summary of the Invention
[0004] To address the aforementioned problems, this invention provides a composite ferrite, its preparation method, a circulator, and its applications. In this composite ferrite, gyromagnetic ferrite and permanent magnet ferrite are integrated into a single unit, solving the technical problems of breakage and high production costs caused by using gyromagnetic ferrite sheets and permanent magnet ferrite sheets.
[0005] This invention is achieved through the following technical solution: In a first aspect, the present invention provides a composite ferrite with a surface center magnetic field strength of 1150Gs~1170Gs and a center saturation magnetization of 1500Gs~1600Gs.
[0006] In some possible implementations, the composite ferrite includes a permanent magnet ferrite layer, a gyromagnetic ferrite layer, and a central conductor; The central conductor is located on one side of the ferrite layer of the gyromagnet; The permanent magnet ferrite layer is located on the opposite side of the gyromagnetic ferrite layer and away from the central conductor.
[0007] In some possible implementations, the raw materials for the permanent magnet ferrite layer include magnetic blocks and a first additive.
[0008] In some possible implementations, the raw materials for the gyromagnetic ferrite layer include YIG ferrite pre-sintered material, bismuth oxide, and a second additive.
[0009] In some possible implementations, the raw material for the magnetic block includes pre-sintered permanent magnet ferrite.
[0010] In some possible implementations, the raw materials for the magnetic block also include calcium carbonate, silicon dioxide, boric acid, and calcium gluconate.
[0011] In some possible implementations, the mass ratio of the magnetic block to the first additive is 1:(0.01~0.02).
[0012] In some possible implementations, the mass ratio of the YIG ferrite pre-sintered material, the calcium carbonate, the silica, the boric acid, and the calcium gluconate is 1:(0.005~0.007):(0.002~0.004):(0.002~0.004):(0.005~0.007).
[0013] In some possible implementations, the mass ratio of the YIG ferrite pre-calcined material, the bismuth oxide and the second additive is 1:(0.005~0.015):(0.01~0.02).
[0014] In some possible implementations, the YIG ferrite pre-sintered material includes the following raw materials: Y2O3, Fe2O3, SnO2, Bi2O3 and CaCO3.
[0015] Secondly, the present invention provides a method for preparing the above-mentioned composite ferrite, comprising the following steps: The composite ferrite is obtained by combining the permanent magnet ferrite molding material, the gyromagnetic ferrite molding material and the center conductor.
[0016] In some possible implementations, the composite process includes the following steps: The permanent magnet ferrite molding material, the gyromagnetic ferrite molding material, and the central conductor are formed into a composite ferrite molding body and then sintered.
[0017] In some possible implementations, the preparation of the composite ferrite molded body includes the following steps: Under a strong magnetic field, the permanent magnet ferrite molding material, the gyromagnetic ferrite molding material, and the central conductor are pressed and molded.
[0018] Thirdly, the present invention provides a circulator comprising the aforementioned composite ferrite.
[0019] Fourthly, the present invention provides an application of the above-mentioned circulator in the field of communication.
[0020] The composite ferrite, its preparation method, and the circulator provided by this invention have at least the following beneficial technical effects compared with the prior art: (1) The composite ferrite provided by the present invention, which consists of permanent magnet ferrite, gyromagnetic ferrite and central conductor as a whole, can be directly used in the circulator without the need for layer-by-layer stacking of thin sheet structures, thereby avoiding unnecessary losses caused by damage during the production, transportation and assembly of permanent magnet ferrite and gyromagnetic ferrite.
[0021] (2) The method for preparing composite ferrite provided by the present invention integrates permanent magnet ferrite, gyromagnetic ferrite and central conductor into one piece, eliminating the need for flat grinding and surface electroplating of thin sheets. The method is simple and easy to implement, which reduces production costs. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of this drawing or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this drawing. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0023] Figure 1 This is a schematic diagram of the structure of the circulator provided in the background art of the present invention; Figure 2 This is a schematic diagram of the structure of the composite ferrite provided in the embodiment of the present invention.
[0024] Explanation of reference numerals in the attached drawings: 1-Center conductor, 2-Rotary ferrite sheet, 3-Grounding sheet, 4-Anti-rotation component, 5-Permanent ferrite sheet, 6-Cover plate, 7-Shell, 221-First rotary ferrite layer, 222-Second rotary ferrite layer, 231-First permanent ferrite layer, 232-Second permanent ferrite layer.
[0025] The purpose, features, and advantages of this accompanying drawing will be further explained in conjunction with the embodiments and with reference to the accompanying drawing. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the invention is described and illustrated below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. All other embodiments obtained by those skilled in the art based on the embodiments provided by this invention without inventive effort are within the scope of protection of this invention.
[0027] Obviously, the following description is merely some examples or embodiments of the present invention. Those skilled in the art can apply the present invention to other similar scenarios without any inventive effort. Furthermore, it is understood that although the effort involved in such development may be complex and lengthy, for those skilled in the art related to the content disclosed in this invention, modifications to design, manufacturing, or production based on the technical content disclosed in this invention are merely conventional technical means and should not be construed as insufficient disclosure of the present invention.
[0028] However, there may be instances where unnecessary detailed descriptions are omitted. For example, detailed descriptions of well-known matters or repetitive descriptions of essentially the same structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the following description is provided to enable those skilled in the art to fully understand the invention and is not intended to limit the subject matter of the claims.
[0029] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions, and all technical features and optional technical features of the present invention can be combined with each other to form new technical solutions.
[0030]
Composite Ferrite
[0031] The composite ferrite provided in this invention, after magnetization, ensures the gyromagnetic properties of the gyromagnetic ferrite layer at microwave frequencies, thus exhibiting excellent unidirectional signal transmission characteristics. The central saturation magnetization also enables the composite ferrite to possess good signal transmission sensitivity and low high-frequency loss. The composite ferrite provided in this invention is suitable for high-frequency / millimeter-wave circulators.
[0032] In some embodiments, the composite ferrite includes a permanent magnet ferrite layer, a gyromagnetic ferrite layer, and a central conductor; The central conductor is located on one side of the ferrite layer of the gyromagnet; The permanent magnet ferrite layer is located on the opposite side of the gyromagnetic ferrite layer and away from the central conductor.
[0033] In some specific embodiments, the composite ferrite includes a first permanent magnet ferrite layer, a first gyromagnetic ferrite layer, a central conductor, a second gyromagnetic ferrite layer, and a second permanent magnet ferrite layer connected in sequence.
[0034] In some embodiments, the raw materials for the permanent magnet ferrite layer include magnetic blocks and a first additive; The mass ratio of magnetic material block to first additive is 1:(0.01~0.02).
[0035] In some embodiments, the first additive includes at least one of an adhesive and a lubricant.
[0036] In some embodiments, the adhesive includes at least one of camphor powder, polyvinyl alcohol, and methylcellulose.
[0037] In some embodiments, the lubricant includes at least one of calcium stearate, paraffin wax, and polyethylene glycol.
[0038] In some embodiments, the raw material for the magnetic block includes pre-sintered permanent magnet ferrite.
[0039] In some embodiments, the raw materials for the magnetic block also include calcium carbonate, silicon dioxide, boric acid, and calcium gluconate; The mass ratio of the permanent magnet ferrite pre-sintered material, calcium carbonate, silicon dioxide, boric acid and calcium gluconate is 1:(0.005~0.007):(0.002~0.004):(0.002~0.004):(0.005~0.007).
[0040] In some embodiments, the grade of the permanent magnet ferrite pre-sintered material is Y40.
[0041] In some embodiments, the thickness of the permanent magnet ferrite layer is 1 mm to 3 mm.
[0042] In some embodiments, the raw materials for the ferromagnetic ferrite layer include YIG ferrite pre-sintered material, bismuth oxide, and a second additive. The mass ratio of YIG ferrite pre-sintered material, bismuth oxide, and the second additive is 1:(0.005~0.015):(0.01~0.02).
[0043] In some embodiments, the YIG ferrite pre-sintered material includes the following raw materials: Y2O3, Fe2O3, SnO2, Bi2O3 and CaCO3.
[0044] In some embodiments, the molar ratio of Y2O3:Fe2O3:SnO2:Bi2O3:CaCO3 is (13~13.5):(20.5~21):(2.2~2.6):1:(2.2~2.6).
[0045] In some embodiments, the thickness of the ferrite layer is 0.2 mm to 2 mm.
[0046] In some embodiments, the second additive includes at least one of an adhesive and a lubricant.
[0047] In some embodiments, the center conductor is a Y-shaped center conductor.
[0048] In some embodiments, the Y-shaped center conductor comprises a tungsten-copper alloy.
[0049] In some embodiments, the tungsten-copper alloy comprises the following components by mass fraction: Copper 40%~50%, tungsten 50%~60%.
[0050] In some specific embodiments, the tungsten-copper alloy is designated CuW50.
[0051] In some embodiments, the thickness of the center conductor is 0.2 mm to 1 mm.
[0052] [Preparation method of composite ferrite] A second aspect of this invention provides a method for preparing the above-mentioned composite ferrite, comprising the following steps: S10. A composite ferrite is obtained by dry pressing and sintering the permanent magnet ferrite molding material, the rotary magnet ferrite molding material and the center conductor.
[0053] In some embodiments, the preparation of the permanent magnet ferrite molding material in step S10 above includes the following steps: S101. Prepare magnetic blocks.
[0054] S102. The magnetic material block and the first additive are mixed in a first mixing process to obtain permanent magnet ferrite molding material.
[0055] In some embodiments, in step S101 above, preparing the magnetic block includes the following steps: S1011. The mixture is subjected to wet ball milling to obtain permanent magnet ferrite slurry; wherein the mixture contains permanent magnet ferrite pre-calcined material, calcium carbonate, silicon dioxide, boric acid and calcium gluconate.
[0056] S1012. The permanent magnet ferrite slurry is subjected to wet pressing to obtain a permanent magnet ferrite green body.
[0057] S1013. The permanent magnet ferrite green blank is subjected to dehydration treatment to obtain magnetic material blocks.
[0058] In some embodiments, in step S1011 above, the mass ratio of material to ball and water in the wet ball milling process is 1:(3~5):(1.5~3).
[0059] In some embodiments, in step S1011 above, the ball milling time in the wet ball milling process is 11h to 13h.
[0060] In some embodiments, in step S1011 above, the average particle size of the permanent magnet ferrite slurry is 0.8 μm to 1.0 μm. In this case, the powder is easily oriented in the forming magnetic field, while also possessing good activity and sintering controllability.
[0061] In some embodiments, in step S1012 above, the wet pressing process includes: S10121. Under magnetic field conditions, the permanent magnet ferrite slurry is pressed into a preset shape.
[0062] In some embodiments, in step S10121 above, the magnetic field strength is (8.9~9.1)×10 3 Oe.
[0063] In some embodiments, in step S10121 above, the pressing pressure is 12MPa~16MPa.
[0064] In some embodiments, the pressing time in step S10121 is 30s to 60s.
[0065] In some embodiments, in step S1013 above, the water removal treatment includes the following steps: S10131. Dry the permanent magnet ferrite green blank at 190℃~210℃.
[0066] In some embodiments, the drying time in step S10131 is 5h to 6h.
[0067] In some embodiments, during step S1013 described above, the moisture content of the magnetic material is below 0.3%. In this case, the powder dispersion effect can be guaranteed, while preventing sintering cracking.
[0068] In some embodiments, in step S102 above, the first mixing process includes: S1021. The magnetic material block and the first additive are mixed, dispersed, and then sieved.
[0069] In some embodiments, the mixing and dispersing step in step S1021 includes: S10211. The magnetic material blocks and the first additive are mixed, dispersed and crushed using a pulverizer.
[0070] In some embodiments, in step S10211 above, the dispersion and pulverization time is 2 min to 4 min.
[0071] In some embodiments, in step S1021 above, the mesh size of the sieve is 55 mesh to 65 mesh.
[0072] In some embodiments, the preparation of the gyromagnetic ferrite molding material in step S10 above includes the following steps: S103. Preparation of YIG ferrite pre-sintered material.
[0073] S104.YIG ferrite pre-calcined material, bismuth oxide and a second additive are subjected to a second mixing treatment to obtain a gyromagnetic ferrite molding material.
[0074] In some embodiments, in step S103 above, the preparation of YIG ferrite pre-sintered material includes the following steps: S1031. The raw materials of YIG ferrite pre-sintered material are mixed and subjected to a single wet ball milling process before sintering.
[0075] In some embodiments, in step S1031 above, the mass ratio of material to ball and water in a single wet ball milling process is 1:(5~7):(2~4).
[0076] In some embodiments, in step S1031 above, the ball milling time in a single wet ball milling process is 11h to 13h.
[0077] In some embodiments, in step S1031 above, the sintering temperature is 1190°C to 1210°C.
[0078] In some embodiments, in step S1031 above, the sintering atmosphere is an oxygen atmosphere.
[0079] In some embodiments, the sintering time in step S1031 is 2h to 3h.
[0080] In some embodiments, the preparation of YIG ferrite pre-sintered material in step S103 above further includes a post-processing step: coarsely crushing the sintered product.
[0081] In some embodiments, in step S104 above, the second mixing process includes the following steps: S1041. YIG ferrite pre-calcined material and bismuth oxide are subjected to secondary wet ball milling and then dried to obtain a ferromagnetic ferrite mixture.
[0082] S1042. The mixture of ferromagnetic ferrite and the second additive is sieved after being mixed and dispersed.
[0083] In some embodiments, in step S1041 above, the mass ratio of material to ball and water in the secondary wet ball milling process is 1:(5~7):(2~4).
[0084] In some embodiments, in step S1041 above, the ball milling time in the secondary wet ball milling process is 11h to 13h.
[0085] In some embodiments, in step S1041 above, the average particle size of the slurry obtained by ball milling in the secondary wet ball milling process is 0.7 μm to 0.9 μm.
[0086] In some embodiments, during step S1041, the drying temperature is 180°C to 220°C. In some embodiments, during step S1041, the moisture content of the dried ferrite mixture is below 0.3%. In this case, the powder dispersion effect can be guaranteed, while preventing sintering cracking.
[0087] In some embodiments, the composite process in step S10 above includes the following steps: S105. The permanent magnet ferrite molding material, the rotary magnet ferrite molding material and the center conductor are made into a composite ferrite molding body and then sintered.
[0088] In some embodiments, the preparation of the composite ferrite molded article in step S105 above includes the following steps: S1051. The ferrite molding material and the center conductor are subjected to a first pressing process to obtain the pre-molded body.
[0089] S1052. Under a strong magnetic field, the pre-formed body and the permanent magnet ferrite molding material undergo a second pressing process to obtain a composite ferrite molding body.
[0090] In some embodiments, in step S1051 above, the pressing pressure in the first pressing process is 14MPa~16MPa.
[0091] In some embodiments, in step S1051 above, the pressing time in the first pressing process is 10~60s.
[0092] In some embodiments, in step S1051 above, the pre-formed body is a cylinder with a bottom diameter of 10mm to 20mm.
[0093] In some embodiments, in step S1052 above, the diameter of the composite ferrite molded body is 0.1~0.5 mm larger than the diameter of the preceding molded body.
[0094] In some embodiments, in step S1052 above, the magnetic field strength of the strong magnetic field is 8 × 10⁻⁶. 3 Oe and above.
[0095] In some embodiments, in step S1052 above, the strong magnetic field is an axially parallel magnetic field.
[0096] In some embodiments, in step S1052 above, the pressure during the second pressing process is 14MPa~16MPa.
[0097] In some embodiments, in step S1052 above, the pressing time in the second pressing process is 15s to 17s.
[0098] In some embodiments, the maximum sintering temperature in step S105 is 1170°C to 1190°C.
[0099] In some embodiments, in step S105 above, the holding time at the highest sintering temperature is 2h to 3h.
[0100] In some embodiments, in step S105 above, the composite ferrite sintered body obtained after sintering is a cylinder, and the ratio of the diameter of the composite ferrite molded body to the diameter of the sintered body is 1.13~1.15:1.
[0101] In some embodiments, the absolute value of the difference between the bottom diameter of the composite ferrite sintered body and the bottom diameter of the composite ferrite molded body is 1 mm to 2 mm.
[0102] In some embodiments, step S10 above further includes a post-processing step: the composite ferrite sintered body obtained after composite processing can be subjected to external cylindrical grinding according to the size requirements of the circulator.
[0103] A third aspect of the present invention provides a circulator comprising the composite ferrite described above.
[0104] The following is a further explanation with reference to specific embodiments. For ease of explanation, unless otherwise specified, tap water is used as the medium in the wet ball milling process in the following embodiments or comparative examples.
[0105] The grade of the permanent magnet ferrite pre-sintered material is Y40.
[0106] The center conductor is a tungsten copper alloy, grade CuW50.
[0107] Example 1 Example 1 provides a composite ferrite, which consists of a first permanent magnet ferrite layer, a first gyromagnetic ferrite layer, a central conductor, a second gyromagnetic ferrite layer, and a second permanent magnet ferrite layer connected in sequence.
[0108] The raw materials for both the first and second permanent magnet ferrite layers consist of magnetic blocks, camphor powder, and calcium stearate, with a mass ratio of 1:0.009:0.006.
[0109] The raw materials for the magnetic blocks are pre-sintered permanent magnet ferrite, calcium carbonate, silicon dioxide, boric acid, and calcium gluconate, in a mass ratio of 1:0.006:0.003:0.003:0.006.
[0110] The thickness of both the first permanent magnet ferrite layer and the second permanent magnet ferrite layer is 2 mm.
[0111] The raw materials for both the first and second spiral magnetic ferrite layers consist of YIG ferrite pre-calcined material, bismuth oxide, camphor powder, and calcium stearate, with a mass ratio of 1:0.01:0.009:0.006.
[0112] The raw materials for YIG ferrite pre-sintered feedstock consist of Y2O3, Fe2O3, SnO2, Bi2O3 and CaCO3, with a molar ratio of 13.2:20.8:2.4:1:2.4.
[0113] The thickness of both the first and second gyromagnetic ferrite layers is 1 mm.
[0114] This embodiment also provides a method for preparing the composite ferrite provided in this embodiment, the steps of which are as follows: E10. Preparation of permanent magnet ferrite molding material E101. The pre-calcined permanent magnet ferrite material, calcium carbonate, silica, boric acid and calcium gluconate were mixed and then wet-milled for 12 hours to obtain a permanent magnet ferrite slurry with an average particle size of 0.9 μm; wherein, the mass ratio of material to ball and water in the wet ball milling was 1:4:2.
[0115] E102. In a magnetic field strength of 9 × 10 3 Under Oe pressure of 14MPa, the permanent magnet ferrite slurry is wet-pressed into rectangular blocks to obtain permanent magnet ferrite green blanks.
[0116] E103. The permanent magnet ferrite green blank is coarsely crushed and dried at 200℃ for 5 hours to obtain magnetic material blocks with a moisture content of 0.2%.
[0117] E104. After mixing, dispersing and pulverizing the magnetic material block, camphor powder and calcium stearate for 2 minutes, the mixture is passed through a 60-mesh sieve to obtain permanent magnet ferrite molding material.
[0118] E20. Preparation of gyromagnetic ferrite molding materials E201.Y2O3, Fe2O3, SnO2, Bi2O3 and CaCO3 were mixed and wet ball milled for 12 hours; wherein, the mass ratio of material, ball and water in the wet ball milling was 1:6:3.
[0119] E202. The ball-milled powder was sintered at 1200℃ in an oxygen atmosphere for 2 hours and then coarsely crushed to obtain YIG ferrite pre-sintered material.
[0120] E203.YIG ferrite pre-calcined material and bismuth oxide were wet ball-milled until the average particle size of the slurry was 0.8 μm. Then, the slurry was dried at 200°C until the water content was below 0.3% to obtain a ferromagnetic ferrite mixture. In the wet ball milling, the mass ratio of material to ball to water was 1:6:3.
[0121] E204. After mixing, dispersing and pulverizing the spinous ferrite mixture, camphor powder and calcium stearate for 2 minutes, the mixture is passed through a 60-mesh sieve to obtain the spinous ferrite molding material.
[0122] E30. Preparation of composite ferrite sintered bodies E301. After sequentially filling 1g of ferromagnetic ferrite molding material, 1 Y-shaped center conductor, and 1g of ferromagnetic ferrite molding material into a cylindrical mold cavity with a diameter of 15mm, a first pressing process is performed to obtain the pre-molded body; wherein, the thickness of the Y-shaped center conductor is 0.8mm. In the first pressing process, the pressing pressure is 15 MPa and the pressing time is 10 seconds.
[0123] E302. After sequentially filling a cylindrical mold cavity with 2g of permanent magnet ferrite molding material, 1 pre-molded body, and 2g of permanent magnet ferrite molding material, the cavity is then subjected to a magnetic field strength of 8×10⁻⁶. 3 Under the axial parallel magnetic field of Oe, a second pressing process is performed to obtain a composite ferrite molded body. In the second pressing process, the pressing pressure is 15 MPa and the pressing time is 15 seconds.
[0124] E303. The composite ferrite molded body is sintered at 1180℃ for 2 hours to obtain the composite ferrite sintered body.
[0125] E40. The composite ferrite sintered body is ground to a diameter of 13 mm by external cylindrical grinding to obtain the composite ferrite provided in this embodiment.
[0126] Comparative Example 1 Comparative Example 1 provides a ferrite comprising a first permanent magnet ferrite sheet, a first gyromagnetic ferrite sheet, a central conductor, a second gyromagnetic ferrite sheet, and a second permanent magnet ferrite sheet stacked together; The raw materials of the first and second gyromagnetic ferrite sheets are the same as those of the gyromagnetic ferrite layer provided in Example 1. The raw materials for the first and second permanent magnet ferrite sheets are the same as those for the permanent magnet ferrite layer provided in Example 1. The thickness of the first and second spiral ferrite sheets is 1 mm and the diameter is 13 mm. The thickness of the first permanent magnet ferrite sheet and the diameter of the second permanent magnet ferrite sheet are both 2 mm and 13 mm.
[0127] To verify the advancement of the composite ferrite and its preparation method according to the embodiments of the present invention, the composite ferrite or ferrite provided in the embodiments and comparative examples of the present invention were tested according to GB / T 43264-2023 and GB / T 9633-2012 standards, respectively, for the surface center magnetic field strength, saturation magnetization of the intermediate gyromagnetic ferrite, resonance linewidth and dielectric constant after magnetization. The results are shown in Table 1 below.
[0128] Table 1
[0129] It can be seen from Table 1 above: The composite ferrite provided in Example 1, after magnetization, exhibits similar surface center magnetic field strength, saturation magnetization of the intermediate gyromagnetic ferrite, resonant linewidth, and dielectric constant to Comparative Example 1. This demonstrates that the method for preparing the composite ferrite provided in this embodiment of the invention first uses gyromagnetic ferrite molding material and a Y-shaped central conductor pre-molded body, then combines the pre-molded body with the permanent magnet ferrite molding material to form a composite ferrite molding body, and finally sintersects it to obtain a sintered composite ferrite body. This step-by-step method for preparing the sintered composite ferrite body ensures that the surface center magnetic field strength, saturation magnetization of the intermediate gyromagnetic ferrite, resonant linewidth, and dielectric constant of the resulting composite ferrite, after magnetization, meet the operational requirements of the circulator.
[0130] It should be noted that the present invention is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments that have the same structure and perform the same effects as the technical concept within the scope of the present invention are included within the scope of the present invention. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of the present invention, are also included within the scope of the present invention.
Claims
1. A composite ferrite, characterized in that, The surface center magnetic field strength is 1150 Gs~1170 Gs, and the center saturation magnetization is 1500 Gs~1600 Gs; The composite ferrite comprises a permanent magnet ferrite layer, a gyromagnetic ferrite layer, and a central conductor; the central conductor is located on one side of the gyromagnetic ferrite layer; the permanent magnet ferrite layer is located on the other side of the gyromagnetic ferrite layer and faces away from the central conductor; The raw materials for the permanent magnet ferrite layer include magnetic blocks and a first additive; The raw materials for the gyromagnetic ferrite layer include YIG ferrite pre-sintered material, bismuth oxide, and a second additive. The center conductor is a Y-shaped center conductor; the center conductor comprises a tungsten-copper alloy. The method for preparing the composite ferrite includes the following steps: S1: The magnetic material block and the first additive are mixed in a first mixing process to obtain permanent magnet ferrite molding material; the YIG ferrite pre-sintered material, bismuth oxide and the second additive are mixed in a second mixing process to obtain gyromagnetic ferrite molding material. S2: The ferrite molding material and the center conductor are subjected to a first pressing process to obtain a pre-molded body; under a strong magnetic field, the pre-molded body and the permanent magnet ferrite molding material are subjected to a second pressing process to obtain a composite ferrite molding body, which is then sintered at a maximum temperature of 1170℃~1190℃.
2. The composite ferrite according to claim 1, characterized in that, The raw materials for the magnetic blocks include pre-sintered permanent magnet ferrite; And / or, the YIG ferrite pre-sintered material includes the following raw materials: Y2O3, Fe2O3, SnO2, Bi2O3 and CaCO3.
3. The composite ferrite according to claim 2, characterized in that, The raw materials for the magnetic blocks also include calcium carbonate, silicon dioxide, boric acid, and calcium gluconate.
4. The composite ferrite according to claim 3, characterized in that, The mass ratio of the magnetic material block to the first additive is 1:0.01~0.02; And / or, the mass ratio of the permanent magnet ferrite pre-sintered material, calcium carbonate, silicon dioxide, boric acid and calcium gluconate is 1:(0.005~0.007):(0.002~0.004):(0.002~0.004):(0.005~0.007); And / or, the mass ratio of the YIG ferrite pre-calcined material, bismuth oxide, and the second additive is 1:(0.005~0.015):(0.01~0.02).
5. A circulator, characterized in that, Includes the composite ferrite as described in any one of claims 1 to 4.
6. An application of the circulator as described in claim 5 in the field of communication.
Citation Information
Patent Citations
Preparation method of permanent magnetic ferrite anisotropic dry-pressed powder
CN105622082A
YIG ferrite material with high dielectric constant and high saturation magnetization and preparation method thereof