A sodium ferric pyrophosphate phosphate positive electrode material, a preparation method and application thereof
By co-doping with Ti, K, and Al and coating with organic and inorganic carbon sources, the crystal structure and conductivity of sodium iron pyrophosphate cathode material were optimized, solving the conductivity and density problems of existing materials and achieving high actual density and high specific capacity.
Patent Information
- Application Number
- CN202510907858.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-07-02
AI Technical Summary
Existing sodium iron pyrophosphate cathode materials have poor electronic conductivity, low ionic conductivity, and low compaction density, making them difficult to commercialize.
A Ti, K, and Al co-doped sodium iron pyrophosphate cathode material was adopted, and a three-dimensional conductive network was formed by coating with organic and inorganic carbon sources. By precisely controlling the proportion of each element and process parameters, the crystal structure and conductivity of the material were optimized.
It improves the ionic and electronic conductivity of the material, enhances the specific capacity and true density, strengthens the compaction density of the material, and promotes the full utilization of the material's capacity.
Smart Images

Figure CN120727795B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, and in particular to a high-density sodium iron pyrophosphate cathode material, its preparation method, and its application. Background Technology
[0002] Sodium-ion batteries currently show promising application prospects. In sodium-ion batteries, the design of the cathode material is crucial. Currently, common cathode materials for sodium-ion batteries mainly include iron-based materials, such as sodium iron pyrophosphate (NFPP). However, existing NFPPs suffer from poor electronic conductivity and low ionic conductivity, resulting in low specific capacity. Simultaneously, their low compaction density hinders commercial application. Therefore, improving the specific capacity and compaction density of NFPP has become an urgent problem to be solved. Summary of the Invention
[0003] In view of the above analysis, the present invention aims to provide a high-density sodium pyrophosphate cathode material, its preparation method and application, in order to at least solve one of the following problems: the preparation process of sodium pyrophosphate in the prior art is complicated, with low compaction density and relatively low specific capacity.
[0004] This invention provides a sodium iron pyrophosphate cathode material, comprising a matrix material and a coating layer covering the surface of the matrix material; the molecular formula of the matrix material is Na. 4-x Fe 3-y M z (PO4)2P2O7N a Where M includes Ti, K and Al, N is F, the value range of x is: 0 < x ≤ 0.02, the value range of y is: 0 < y ≤ 0.1, the value range of z is: 0 < z ≤ 0.025, the value range of a is: 0 < a ≤ 0.01, and the coating layer is carbon material.
[0005] Furthermore, the mass fraction of the coating layer is 1% to 2%.
[0006] Furthermore, the materials for the coating layer include both organic and inorganic carbon sources.
[0007] Furthermore, the mass ratio of organic carbon source to inorganic carbon source is 9–12:1.
[0008] Furthermore, the organic carbon source is glucose, and the inorganic carbon source is carbon nanotubes.
[0009] The present invention also provides a method for preparing the above-mentioned sodium iron pyrophosphate cathode material, comprising the following steps:
[0010] S1. Sodium source, iron source, phosphorus source, titanium source, potassium source, aluminum source, fluorine source and glucose are mixed and ground, and then carbon nanotubes are added and stirred to prepare a slurry;
[0011] S2. Spray dry the slurry to obtain spherical dried powder;
[0012] S3. After pulverizing the dry powder, mix it according to the particle size to obtain a mixture;
[0013] S4. Sinter the mixture to obtain sintered material;
[0014] S5. After pulverizing the sintered material, sodium iron pyrophosphate cathode material is obtained.
[0015] Furthermore, in S1, the molar ratio of sodium, iron, phosphorus, titanium, potassium, aluminum, and fluorine is controlled as Na:Fe:P:Ti:K:Al:F = 3.98~4:2.9~3:4:0.001~0.01:0.001~0.01:0.001~0.01:0.001~0.01.
[0016] Furthermore, the sodium and phosphorus sources include at least one of sodium phosphate, sodium monohydrogen phosphate, sodium dihydrogen phosphate, sodium pyrophosphate, and disodium dihydrogen pyrophosphate; the iron source includes at least one of iron phosphate and iron trioxide.
[0017] Furthermore, in S4, the sintering holding temperature is 500–600°C.
[0018] The present invention also discloses a sodium-ion battery, which includes the above-mentioned positive electrode material.
[0019] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0020] The sodium iron pyrophosphate cathode material of this invention employs Ti, K, and Al co-doping, which reduces crystal volume and expands sodium ion transport channels. Simultaneously, the synergistic effect of these three elements stabilizes the crystal structure. F ion doping increases the number of vacancies and defects in the crystal, which is beneficial for improving the intrinsic conductivity of the material. Using Ti, K, Al, and F for co-doping, and precisely controlling the proportions of each element, can improve the ionic conductivity of the material while optimizing its crystal structure, thus enhancing its specific capacity and true density.
[0021] The sodium iron pyrophosphate cathode material of the present invention adopts a combination of organic and inorganic carbon sources for coating to form a three-dimensional conductive network, which can help improve the electronic conductivity of the material and promote the utilization of the material capacity. The coating material of the sodium iron pyrophosphate cathode material of the present invention includes organic and inorganic carbon sources. By precisely controlling the quality of organic and inorganic carbon sources, the organic carbon pyrolysis generates amorphous carbon materials that cross-link with carbon nanotubes and adhere to the matrix material to form a three-dimensional conductive network, which can help improve the electronic conductivity of the material and promote the utilization of the material capacity.
[0022] In the preparation method of sodium iron pyrophosphate cathode material of the present invention, by precisely controlling the types of raw materials, the introduction of raw materials that are prone to gas generation during the synthesis process can be reduced, so that the sodium iron pyrophosphate material has a lower porosity and thus a higher density, which is beneficial to improving the compaction density of the material.
[0023] In the preparation method of sodium iron pyrophosphate cathode material of the present invention, by controlling the optimal selection of materials, combined with the control of process parameters and particle size distribution in each step, the obtained sodium iron pyrophosphate cathode material is guaranteed to have high compaction density and high specific capacity.
[0024] The sodium-ion battery of the present invention includes a high-density sodium iron pyrophosphate cathode material. The beneficial effects of the sodium-ion battery are brought about by the high-density sodium iron pyrophosphate cathode material, which will not be elaborated further.
[0025] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0026] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0027] Figure 1 The image shows the XRD pattern of the high-density sodium iron pyrophosphate cathode material of Example 1.
[0028] Figure 2 The charge-discharge curves are for the button cell battery assembled in Example 1. Detailed Implementation
[0029] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0030] This invention provides a sodium iron pyrophosphate cathode material, comprising a matrix material and a coating layer covering the surface of the matrix material; the molecular formula of the matrix material is Na. 4-x Fe 3-y M z (PO4)2P2O7N a Where M includes Ti, K and Al, and N is F; the range of x is 0 < x ≤ 0.02, the range of y is 0 < y ≤ 0.1, the range of z is 0 < z ≤ 0.025, the range of a is 0 < a ≤ 0.01, and the coating layer is carbon material.
[0031] For example, the molecular formula of the matrix material is Na4Fe 2.9 Ti 0.003 K 0.003 Al 0.004 P4O 15 F 0.005 Na4Fe 2.9 Ti 0.0 1K 0.003 Al 0.005 P4O 15 F 0.002 Na4Fe 2.92 Ti 0.01 K 0.005 Al 0.01 P4O 15 F 0.005 Na 3.98 Fe 2.95 Ti 0.003 K 0.01 Al 0.005 P4O 15 F 0.01 .
[0032] Specifically, considering that excessive coating mass leads to low compaction density, while insufficient coating mass results in poor conductivity and affects the material's specific capacity, the mass fraction of the coating is controlled to be 1%–2%, for example, 2%, 1.8%, 1.5%, 1.3%, or 1%.
[0033] Specifically, the materials for the aforementioned coating layer include both organic and inorganic carbon sources.
[0034] Preferably, the organic carbon source is glucose and the inorganic carbon source is carbon nanotubes.
[0035] It should be noted that after the organic carbon is pyrolyzed, the resulting amorphous carbon material cross-links with carbon nanotubes and attaches to the matrix material, forming a three-dimensional conductive network. This can help improve the electronic conductivity of the material and promote the utilization of the material's capacity.
[0036] Specifically, the total mass of the aforementioned organic and inorganic carbon sources should be controlled to account for 2.8% to 3.3% of the total mass of the raw materials, for example, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, and 3.3%.
[0037] Specifically, considering that too much organic carbon source will produce a large amount of amorphous carbon, leading to a decrease in the material's electrical conductivity, while too little will not achieve the desired coating effect, the mass ratio of organic carbon source to inorganic carbon source is controlled to be 9–12:1, for example, 9:1, 10:1, 11:1, or 12:1.
[0038] Compared with existing technologies, the sodium iron pyrophosphate cathode material of this invention utilizes Ti, K, and Al co-doping, which reduces crystal volume and expands sodium ion transport channels. Simultaneously, the synergistic effect of these three dopants stabilizes the crystal structure. F ion doping increases the number of vacancies and defects in the crystal, which is beneficial for improving the intrinsic conductivity of the material. Using Ti, K, Al, and F for co-doping improves the ionic conductivity while optimizing the crystal structure, thus enhancing the specific capacity and true density of the material. The combination of organic and inorganic carbon source coating forms a three-dimensional conductive network, which further improves the electronic conductivity and promotes the full utilization of the material's capacity.
[0039] Specifically, the space group of the crystal structure of the aforementioned sodium iron pyrophosphate cathode material is Pn21a.
[0040] This invention discloses a method for preparing the above-mentioned sodium iron pyrophosphate cathode material, comprising the following steps:
[0041] S1. Sodium source, iron source, phosphorus source, titanium source, potassium source, aluminum source, fluorine source and glucose are mixed and ground, and then carbon nanotubes are added and stirred to prepare a slurry;
[0042] S2. Spray dry the slurry to obtain spherical dried powder;
[0043] S3. After pulverizing the dry powder, mix it according to the particle size to obtain a mixture;
[0044] S4. Sinter the mixture to obtain sintered material;
[0045] S5. After pulverizing the sintered material, sodium iron pyrophosphate cathode material is obtained.
[0046] Specifically, in S1 above, considering that excessive titanium content easily generates impurities, while insufficient titanium content fails to stabilize the crystal structure; excessive potassium content can distort or block the sodium ion insertion / extraction channels, while insufficient potassium content fails to expand the sodium ion transport channels; excessive aluminum content will damage the crystal structure and generate impurities, while insufficient aluminum content cannot stabilize the crystal structure or improve ionic conductivity; excessive fluorine content will damage the crystal structure, while insufficient fluorine content cannot effectively fill the lattice interstices and stabilize the PO bond structure. Therefore, the molar ratio of sodium, iron, phosphorus, titanium, potassium, aluminum, and fluorine is controlled as Na:Fe:P:Ti:K:Al:F = 3.98~4:2.9~3:4:0.001~0.01:0.001~0.01:0.001~0.01:0.001~0.01.
[0047] Specifically, in S1 above, the sodium and phosphorus sources include at least one of sodium phosphate, sodium monohydrogen phosphate, sodium dihydrogen phosphate, sodium pyrophosphate, and disodium dihydrogen pyrophosphate; the iron source includes at least one of iron phosphate and ferric oxide. It should be noted that using the above raw materials can reduce the introduction of easily gas-producing raw materials during the synthesis process, resulting in sodium iron pyrophosphate material with lower porosity and thus higher density, which is beneficial for improving the compaction density of the material.
[0048] Specifically, in S1 above, the titanium source includes at least one of titanium dioxide and tetrabutyl titanate; the potassium source includes at least one of potassium oxide, potassium phosphate, and potassium hydroxide; the aluminum source includes at least one of aluminum oxide, aluminum phosphate, and aluminum hydroxide; and the fluorine source includes at least one of sodium fluoride and ammonium fluoride.
[0049] Specifically, in S1 above, adding glucose first and then carbon nanotubes helps to improve the grinding efficiency of materials and control the grinding particle size.
[0050] Specifically, in S1 above, the D50 of the material obtained by grinding is between 350 and 400 nm, and the D90 is less than 1 micrometer.
[0051] Specifically, in S2 above, considering that excessively high inlet air temperature in spray drying can easily cause segregation, while excessively low temperature reduces efficiency; excessively high outlet air temperature also reduces efficiency, while excessively low temperature results in incomplete material drying. Therefore, the inlet air temperature for spray drying is controlled at 160–180℃ (e.g., 160℃, 170℃, 180℃), and the outlet air temperature is controlled at 95–110℃ (e.g., 95℃, 100℃, 110℃); the feed rate is 290–300 mL / min (e.g., 290 mL / min, 295 mL / min, 300 mL / min), and the atomizer speed is 23000–24000 r / min (e.g., 23000 r / min, 23500 r / min, 24000 r / min).
[0052] Specifically, in S3 above, the average particle size of the large particles in the mixture is 3.5-4 micrometers, and the average particle size of the small particles is 0.4-0.6 micrometers. Mixing large and small particles can achieve the effect of particle gradation. Considering that too much or too little of the large particles in the mixture will not achieve the purpose of particle mixing, the mass ratio of large particles is controlled to be 50%-85% of the total mass, for example, 50%, 60%, 70%, 80%, 85%.
[0053] Specifically, the sintering steps in S4 above are as follows:
[0054] In a tube furnace, the gas atmosphere is controlled to be nitrogen, the holding temperature is 500-600℃, and the holding time is 6-10h; the sintered material is obtained by natural cooling to room temperature.
[0055] During the sintering process, considering that excessively high temperatures and prolonged holding times can easily lead to the formation of impurity phases such as sodium iron pyrophosphate, while excessively low temperatures and short holding times result in incomplete crystal growth, the holding temperature is controlled at 500–600℃, for example, 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, and 600℃; and the holding time is controlled at 6–10h, for example, 6h, 7h, 8h, 9h, and 10h.
[0056] Specifically, the above preparation method also includes pulverizing the sintered material to an average particle size of 1-2 micrometers to obtain a high-energy-density sodium iron pyrophosphate cathode material.
[0057] The sodium iron pyrophosphate cathode material of the present invention has a high compaction density. For example, the compaction density is 2.41 g / cm³. 3 The above, for example, 2.41~2.5g / cm³ 3 The button cell assembled using the sodium iron pyrophosphate cathode material of the present invention has a 0.33C charging capacity of 116 mAh / g or more, for example 116.2 to 120 mAh / g, and a 0.33C discharge capacity of 106 mAh / g or more, for example 106.1 to 111 mAh / g.
[0058] The present invention also provides the application of the above-mentioned sodium iron pyrophosphate cathode material, which can be used in sodium-ion batteries.
[0059] The present invention also discloses a sodium-ion battery, wherein the sodium-ion battery comprises the above-described positive electrode material or the positive electrode material prepared by the above-described preparation method.
[0060] Example 1
[0061] This embodiment provides a sodium iron pyrophosphate cathode material and its preparation method, the preparation method including:
[0062] Sodium phosphate, ferric phosphate, titanium dioxide, aluminum oxide, potassium oxide, ferric oxide, and sodium fluoride were weighed according to the stoichiometric ratio of Na:Fe:P:Ti:K:Al:F = 4:2.9:4:0.003:0.003:0.004:0.005. 2.9% glucose was added, and the mixture was ground to control the particle size (D50) between 350 and 400 nm and D90 < 1 μm. Then, 0.25% carbon nanotubes were added and stirred for 1 h. The prepared slurry was spray-dried at an inlet air temperature of 175℃ and an outlet air temperature of 105℃, with a feed rate of 300 mL / min and an atomizer speed of 24000 r / min, to obtain spherical dried powder. After further pulverization, the dried powder was mixed according to particle size, with the average particle size of large particles being 4 μm and the average particle size of small particles being 0.6 μm, and the mass proportion of large particles being 80%. The optimized graded spray material was sintered under a nitrogen atmosphere: held at 500℃ for 8 hours to obtain sodium iron pyrophosphate cathode material; the sintered material was then pulverized to an average particle size of about 1.5 micrometers to obtain high energy density sodium iron pyrophosphate cathode material.
[0063] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this embodiment is Na₄Fe₂O₃. 2.9 Ti 0.003 K 0.003 Al 0.004 P4O 15 F 0.005 .
[0064] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this embodiment are shown in Table 1 below, and the XRD pattern of the sodium iron pyrophosphate cathode material is shown in... Figure 1 As shown.
[0065] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. Figure 2 The charge-discharge curves of the button cell assembled in Example 1 are shown in Table 1.
[0066] Example 2
[0067] This embodiment provides a sodium iron pyrophosphate cathode material and its preparation method, the preparation method including:
[0068] Sodium phosphate, ferric phosphate, titanium dioxide, aluminum oxide, potassium oxide, ferric oxide, and sodium fluoride were weighed according to the stoichiometric ratio of Na:Fe:P:Ti:K:Al:F = 4:2.9:4:0.01:0.003:0.005:0.002. 2.9% glucose was added, and the mixture was ground to control the particle size (D50) between 360 and 400 nm and D90 < 1 μm. Then, 0.25% carbon nanotubes were added and stirred for 1 h. The prepared slurry was spray-dried at an inlet air temperature of 165℃ and an outlet air temperature of 100℃, with a feed rate of 290 mL / min and an atomizer speed of 24000 r / min, to obtain spherical dried powder. After further pulverization, the dried powder was mixed according to particle size, with the average particle size of large particles being 3.5 μm and the average particle size of small particles being 0.4 μm, and the mass proportion of large particles being 85%. The optimized graded spray material was sintered under a nitrogen atmosphere: held at 530℃ for 8 hours to obtain sodium iron pyrophosphate cathode material; the sintered material was then pulverized to an average particle size of about 2 micrometers to obtain high energy density sodium iron pyrophosphate cathode material.
[0069] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this embodiment is Na₄Fe₂O₃. 2.9 Ti 0.01 K 0.003 Al 0.005 P4O 15 F 0.002 .
[0070] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this embodiment are shown in Table 1 below.
[0071] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0072] Example 3
[0073] This embodiment provides a sodium iron pyrophosphate cathode material and its preparation method, the preparation method including:
[0074] Sodium pyrophosphate, ferric phosphate, titanium dioxide, aluminum oxide, potassium oxide, ferric oxide, and sodium fluoride were weighed according to the stoichiometric ratio of Na:Fe:P:Ti:K:Al:F = 4:2.92:4:0.01:0.005:0.01:0.005. 2.9% glucose was added, and the mixture was ground to control the particle size (D50) between 350 and 390 nm and D90 < 1 μm. Then, 0.25% carbon nanotubes were added and stirred for 1 h. The prepared slurry was spray-dried at an inlet air temperature of 170℃ and an outlet air temperature of 100℃, with a feed rate of 300 mL / min and an atomizer speed of 24000 r / min, to obtain spherical dried powder. After further pulverization, the dried powder was mixed according to particle size, with the average particle size of large particles being 3.7 μm and the average particle size of small particles being 0.5 μm, and the mass proportion of large particles being 75%. The optimized graded spray material was sintered under a nitrogen atmosphere: held at 540℃ for 6 hours to obtain sodium iron pyrophosphate cathode material; the sintered material was then pulverized to an average particle size of about 1 micrometer to obtain high energy density sodium iron pyrophosphate cathode material.
[0075] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this embodiment is Na₄Fe₂O₃. 2.92 Ti 0.01 K 0.005 Al 0.01 P4O 15 F 0.005 .
[0076] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this embodiment are shown in Table 1 below.
[0077] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0078] Example 4
[0079] This embodiment provides a sodium iron pyrophosphate cathode material and its preparation method, the preparation method including:
[0080] Sodium phosphate, ferric phosphate, titanium dioxide, aluminum oxide, potassium oxide, ferric oxide, and sodium fluoride were weighed according to the stoichiometric ratio of Na:Fe:P:Ti:K:Al:F = 3.98:2.95:4:0.003:0.01:0.005:0.01. 2.9% glucose was added, and the mixture was ground to control the particle size (D50) between 350 and 400 nm and D90 < 1 μm. Then, 0.25% carbon nanotubes were added and stirred for 1 h. The prepared slurry was spray-dried at an inlet air temperature of 180℃ and an outlet air temperature of 100℃, with a feed rate of 300 mL / min and an atomizer speed of 23500 r / min, to obtain spherical dried powder. After further pulverization, the dried powder was mixed according to particle size, with the average particle size of large particles being 3.6 μm and the average particle size of small particles being 0.45 μm, and the mass proportion of large particles being 80%. The optimized graded spray material was sintered under a nitrogen atmosphere: held at 520℃ for 7 hours to obtain sodium iron pyrophosphate cathode material; the sintered material was then pulverized to an average particle size of about 1.8 micrometers to obtain high energy density sodium iron pyrophosphate cathode material.
[0081] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this embodiment is Na. 3.98 Fe 2.95 Ti 0.003 K 0.01 Al 0.005 P4O 15 F 0.01 .
[0082] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this embodiment are shown in Table 1 below.
[0083] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0084] The inventors conducted extensive research during the research process, and some suboptimal solutions are presented here as comparative examples.
[0085] Comparative Example 1
[0086] Sodium phosphate, iron phosphate, titanium dioxide, aluminum oxide, potassium oxide, and ferric oxide were weighed according to a stoichiometric ratio of Na:Fe:P:Ti:K:Al = 4:2.9:4:0.003:0.003:0.004. 2.7% glucose was added, and the particle size (D50) was controlled between 350 and 400 nm. 0.25% carbon nanotubes were added and stirred for 1 hour. The prepared slurry was spray-dried at an inlet air temperature of 180℃ and an outlet air temperature of 110℃ to obtain spherical dried powder. After pulverizing, the sprayed material was mixed according to particle size, with large particles having an average particle size of 4 μm and small particles having an average particle size of 0.6 μm; the mass proportion of large particles was 70%. The optimized gradation of the sprayed material was sintered at 500℃ for 8 hours under a nitrogen atmosphere to obtain sodium iron phosphate pyrophosphate cathode material. The sintered material was then pulverized to an average particle size of 1.5 μm to obtain sodium iron phosphate pyrophosphate material.
[0087] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.9 Ti 0.003 K 0.003 Al 0.004 P4O 15 .
[0088] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0089] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0090] Comparative Example 2
[0091] Sodium phosphate, iron phosphate, titanium dioxide, and ferric oxide were weighed according to a stoichiometric ratio of Na:Fe:P:Ti:K = 4:2.9:4:0.005:0.005. 2.5% glucose was added, and the particles were ground to control the D50 between 350-400 nm. 0.25% carbon nanotubes were added and stirred for 1 hour. The prepared slurry was spray-dried at an inlet air temperature of 170℃ and an outlet air temperature of 100℃ to obtain spherical dried powder. After pulverizing, the sprayed material was mixed according to particle size, with large particles having an average particle size of 3.5 μm and small particles having an average particle size of 0.5 μm; the mass proportion of large particles was 75%. The optimized gradation of the sprayed material was sintered at 580℃ for 8 hours under a nitrogen atmosphere to obtain sodium iron phosphate pyrophosphate cathode material. The sintered material was then pulverized to an average particle size of 1.5 μm to obtain sodium iron phosphate pyrophosphate material.
[0092] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.9 Ti 0.005 K 0.005 P4O 15 .
[0093] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0094] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0095] Comparative Example 3
[0096] Sodium carbonate, ferrous oxalate, titanium dioxide, and sodium dihydrogen phosphate were weighed according to a stoichiometric ratio of Na:Fe:P:Ti = 4:2.9:4:0.01. 2.9% glucose was added, and the mixture was ground to control the particle size (D50) between 350-400 nm. 0.25% carbon nanotubes were added and stirred for 1 hour. The prepared slurry was spray-dried at an inlet air temperature of 180℃ and an outlet air temperature of 100℃ to obtain spherical dried powder. After pulverizing, the spray-dried material was mixed according to particle size, with large particles having an average particle size of 4 μm and small particles having an average particle size of 0.6 μm; the mass proportion of large particles was 60%. The optimized gradation of the spray-dried material was sintered at 550℃ for 8 hours under a nitrogen atmosphere to obtain sodium iron pyrophosphate cathode material. The sintered material was then pulverized to an average particle size of 1.5 μm to obtain sodium iron pyrophosphate material.
[0097] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.9 Ti 0.01 P4O 15 .
[0098] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0099] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0100] Comparative Example 4
[0101] Sodium carbonate, iron phosphate, aluminum oxide, and sodium dihydrogen phosphate were weighed according to a stoichiometric ratio of Na:Fe:P:Al = 4:2.9:4:0.01. 2.7% glucose was added, and the particle size (D50) was controlled between 350-400 nm. 0.25% carbon nanotubes were added and stirred for 1 hour. The prepared slurry was spray-dried at an inlet air temperature of 170℃ and an outlet air temperature of 100℃ to obtain spherical dried powder. After pulverizing, the spray-dried material was mixed according to particle size, with large particles having an average particle size of 3.8 μm and small particles having an average particle size of 0.45 μm; the mass proportion of large particles was 55%. The optimized gradation of the spray-dried material was sintered at 530℃ for 6 hours under a nitrogen atmosphere to obtain sodium iron phosphate pyrophosphate cathode material. The sintered material was then pulverized to an average particle size of 2 μm to obtain sodium iron phosphate pyrophosphate material.
[0102] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.9 Al 0.01 P4O 15 .
[0103] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0104] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0105] Comparative Example 5
[0106] Sodium carbonate, ferric phosphate, potassium oxide, sodium fluoride, and disodium dihydrogen pyrophosphate were weighed according to a stoichiometric ratio of Na:Fe:P:K:F = 4:2.9:4:0.01:0.005. 2.7% glucose was added, and the particle size (D50) was controlled between 350-400 nm. 0.25% carbon nanotubes were added and stirred for 1 hour. The prepared slurry was spray-dried at an inlet air temperature of 175℃ and an outlet air temperature of 105℃ to obtain spherical dried powder. After pulverizing, the sprayed material was mixed according to particle size, with large particles having an average particle size of 3.7 μm and small particles having an average particle size of 0.55 μm; the mass proportion of large particles was 75%. The optimized gradation of the sprayed material was sintered at 550℃ for 8 hours under a nitrogen atmosphere to obtain sodium iron pyrophosphate cathode material. The sintered material was then pulverized to an average particle size of 1.2 μm to obtain sodium iron pyrophosphate material.
[0107] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.9 K 0.01P4O 15 F 0.005 .
[0108] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0109] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0110] Comparative Example 6
[0111] The raw materials used in this comparative example are the same as those in Example 1, except that:
[0112] The molar ratio is Na:Fe:P:Ti:K:Al:F = 4:2.98:4:0.02:0.02:0.03:0.02. The remaining steps are the same as in Example 1, and will not be repeated here.
[0113] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.98 Ti 0.02 K 0.02 Al 0.03 P4O 15 F 0.02 .
[0114] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0115] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0116] Comparative Example 7
[0117] The preparation method of this comparative example is roughly the same as that of Example 1, except that:
[0118] The mass ratio of large particles is 45%, the sintering temperature is 480℃, and the remaining steps are the same as in Example 1, and will not be repeated here.
[0119] The compaction density results of the sodium iron pyrophosphate cathode material obtained in this comparative example are shown in Table 1 below.
[0120] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0121] Comparative Example 8
[0122] Sodium carbonate, iron phosphate, and sodium dihydrogen phosphate were weighed according to a stoichiometric ratio of Na:Fe:P = 4:2.9:4. 2.7% glucose was added, and the particles were ground to control the D50 between 350-400 nm. 0.25% carbon nanotubes were added and stirred for 1 hour. The prepared slurry was spray-dried at an inlet air temperature of 180℃ and an outlet air temperature of 110℃ to obtain spherical dried powder. After pulverizing, the sprayed material was mixed according to particle size, with large particles having an average particle size of 4 μm and small particles having an average particle size of 0.6 μm; the mass proportion of large particles was 70%. The optimized gradation of the sprayed material was sintered at 500℃ for 8 hours under a nitrogen atmosphere to obtain sodium iron phosphate pyrophosphate cathode material. The sintered material was then pulverized to an average particle size of 1.5 μm to obtain sodium iron phosphate pyrophosphate material.
[0123] The molecular formula of the sodium iron pyrophosphate cathode material obtained in this comparative example is Na₄Fe₂O₃. 2.9 P4O 15 .
[0124] Using the above-mentioned sodium iron pyrophosphate positive electrode material as the positive electrode, sodium sheet as the negative electrode, and 1 mol / L NaClO4 (EC:DEC = 1:1 + 5% FEC) as the electrolyte, a CR2032 button cell was assembled, and the battery performance was tested. The results are shown in Table 1.
[0125] Table 1 Performance Data
[0126]
[0127]
[0128] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A sodium iron pyrophosphate cathode material, characterized in that, The sodium iron pyrophosphate cathode material comprises a matrix material and a coating layer covering the surface of the matrix material; the molecular formula of the matrix material is Na. 4-x Fe 3-y M z (PO4)2P2O7N a Wherein, M includes Ti, K and Al, N is F, the value range of x is: 0 < x ≤ 0.02, the value range of y is: 0 < y ≤ 0.1, the value range of z is: 0 < z ≤ 0.025, the value range of a is: 0 < a ≤ 0.01, and the coating layer is a carbon material. The material sources for the coating layer include organic carbon sources and inorganic carbon sources; The mass ratio of the organic carbon source to the inorganic carbon source is 9~12:
1.
2. The sodium iron pyrophosphate cathode material according to claim 1, characterized in that, The mass fraction of the coating layer is 1% to 2%.
3. The sodium iron pyrophosphate cathode material according to claim 1, characterized in that, The mass ratio of the organic carbon source to the inorganic carbon source is 10~12:
1.
4. The sodium iron pyrophosphate cathode material according to claim 1, characterized in that, The organic carbon source is glucose, and the inorganic carbon source is carbon nanotubes.
5. A method for preparing the sodium iron pyrophosphate cathode material according to any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Mix and grind the sodium source, iron source, phosphorus source, titanium source, potassium source, aluminum source, fluorine source and glucose. , Then carbon nanotubes were added and stirred to prepare a slurry; S2. Spray dry the slurry to obtain spherical dried powder; S3. After pulverizing the dry powder, mix it according to the particle size to obtain a mixture; S4. Sinter the mixture to obtain sintered material; S5. After crushing the sintered material, sodium iron pyrophosphate cathode material is obtained. In S1, the molar ratio of sodium, iron, phosphorus, titanium, potassium, aluminum, and fluorine is controlled as Na:Fe:P:Ti:K:Al:F = 3.98~4:2.9~3:4:0.001~0.01:0.001~0.01:0.001~0.01:0.001~0.
01.
6. The preparation method according to claim 5, characterized in that, In S1, the molar ratio of sodium, iron, phosphorus, titanium, potassium, aluminum, and fluorine is controlled as Na:Fe:P:Ti:K:Al:F = 3.98~4:2.9~3:4:0.003~0.01:0.001~0.01:0.001~0.01:0.001~0.
01.
7. The preparation method according to claim 5, characterized in that, The sodium and phosphorus sources include at least one of sodium phosphate, sodium monohydrogen phosphate, sodium dihydrogen phosphate, sodium pyrophosphate, and disodium dihydrogen pyrophosphate; the iron source includes at least one of iron phosphate and iron trioxide.
8. The preparation method according to any one of claims 5 to 7, characterized in that, In S4, the sintering holding temperature is 500-600℃.
9. A sodium-ion battery, characterized in that, The sodium-ion battery comprises the sodium iron pyrophosphate cathode material according to any one of claims 1 to 4 or the sodium iron pyrophosphate cathode material prepared by the preparation method according to any one of claims 5 to 8.
Citation Information
Patent Citations
Positive electrode active material, preparation method thereof, positive electrode plate, battery and electric equipment
CN117038973A
Modified ferric sodium pyrophosphate positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery
CN118588913A