Ternary layered selenide Ge3Sb4Se7 semiconductor material and preparation method thereof
By optimizing the high-temperature firing and cooling and insulation processes, single-phase and single-crystal materials of Ge3Sb4Se7 were successfully prepared, solving the problem of difficulty in obtaining single-phase materials in existing technologies and supporting its application in thermoelectric devices and photoelectric detection fields.
Patent Information
- Application Number
- CN202511269916.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-08
- Publication Date
- 2025-10-03
- Estimated Expiration
- 2045-09-08
AI Technical Summary
Existing technologies make it difficult to obtain single-phase and single-crystal materials of Ge3Sb4Se7, which limits its further application in fields such as thermoelectric devices and photoelectric detection.
Germanium powder, antimony powder and selenium powder with a molar ratio of 3:4:7 are used as raw materials, the temperature is raised to 900-950°C under vacuum conditions and kept warm for 12-24 hours, then the temperature is lowered to 475-500°C at a rate of 1-5°C/min and kept warm for 3-5 days, and the material is cooled to room temperature by furnace cooling or quenching to prepare Ge3Sb4Se7 semiconductor material.
The preparation of single-phase and single-crystal materials of Ge3Sb4Se7 has been achieved, providing support for its research in the fields of thermoelectric devices and photoelectric detection.
Smart Images

Figure CN120736476A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of crystal material preparation, and in particular to a ternary layered selenide Ge3Sb4Se7 semiconductor material and a preparation method thereof. Background Art
[0002] Layered chalcogenides are composed of two-dimensional or quasi-two-dimensional layered units stacked along a specific direction. The units are connected by stable ionic and covalent bonds within the plane, and van der Waals interactions exist between the layers. These materials offer ample tunable chemical composition and phase structure, exhibiting a rich variety of physical and chemical properties, and hold great potential for applications in field-effect transistors, photodetectors, gas sensors, spintronics, and thermoelectric devices.
[0003] Selenide Ge3Sb4Se7 is one of the first compounds discovered in the Ge-Sb-Se ternary system (Inorganic Chemistry, 2020, 59(16), 11207-11212.). This compound is composed of two structural units, Sb2Se2 and Ge3Sb2Se5, stacked alternately and has an orthorhombic structure ( Fmm 2), where Sb cations are in the form of Sb-Sb chain structures in the Sb2Se2 layer. This selenide exhibits layered structural characteristics similar to black phosphorus and SnSe, and is an indirect bandgap semiconductor material. Due to its low thermal conductivity and low resistivity, it is expected to be used in thermoelectric devices, photoelectric detection and other fields. However, in the currently disclosed preparation process of Ge3Sb4Se7, other phases (such as GeSb2Se 3、 Sb2Se3), it is difficult to obtain the single phase and single crystal material of this compound, which limits its further research on its intrinsic properties and potential applications. Summary of the Invention
[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a ternary layered selenide Ge3Sb4Se7 semiconductor material and a preparation method thereof, aiming to solve the technical problem in the prior art that it is difficult to obtain single-phase and single-crystalline materials of the compound Ge3Sb4Se7.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The first aspect of the present invention provides a method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material, comprising the following steps: S001. A molar ratio of 3:4:7 of germanium powder, antimony powder and selenium powder as raw materials was heated to 900-950°C under vacuum conditions and kept at this temperature for 12-24h; S002. After the insulation is completed, the temperature is lowered to 475-500°C at a cooling rate of 1-5°C / min and maintained at this temperature for 3-5 days; after the insulation is completed, the material is furnace cooled or quenched to room temperature to obtain a layered ternary selenide single-phase material with the chemical formula Ge3Sb4Se7.
[0006] The method for preparing the ternary layered selenide Ge3Sb4Se7 semiconductor material, wherein, in step S001, the purity of the germanium powder, antimony powder, and selenium powder are all ≥99.99%.
[0007] The method for preparing the ternary layered selenide Ge3Sb4Se7 semiconductor material, wherein, in step S001, the vacuum degree of the vacuum condition is ≤1Pa.
[0008] The method for preparing the ternary layered selenide Ge3Sb4Se7 semiconductor material, wherein in step S001, the heating rate is 1-5°C / min.
[0009] The second aspect of the present invention provides a ternary layered selenide Ge3Sb4Se7 semiconductor material, which is prepared by the preparation method of the ternary layered selenide Ge3Sb4Se7 semiconductor material as described above, wherein the single crystal layer growth direction of the ternary layered selenide Ge3Sb4Se7 semiconductor material is crystallographically c Axis orientation.
[0010] Beneficial effects: The present invention provides a method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material. The preparation method solves the problem in the prior art of being unable to obtain Ge3Sb4Se7 single-phase material by optimizing the high-temperature firing temperature and the cooling and insulation temperature, thereby providing support for the physical property research and functional device development of such materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 This is an optical photograph of the Ge3Sb4Se7 material in Example 1.
[0012] Figure 2 This is the powder X-ray diffraction pattern of the Ge3Sb4Se7 material in Example 1.
[0013] Figure 3 This is a scanning electron microscope image of the microscopic morphology of the Ge3Sb4Se7 material in Example 1.
[0014] Figure 4 This is the X-ray energy spectrum of the Ge3Sb4Se7 material in Example 1.
[0015] Figure 5 This is the atomic resolution structure diagram of the Ge3Sb4Se7 material in the [00l] projection direction in Example 1.
[0016] Figure 6 This is an optical photograph of the Ge3Sb4Se7 single crystal material in Example 1.
[0017] Figure 7 This is the X-ray diffraction pattern of the Ge3Sb4Se7 single crystal material in Example 1.
[0018] Figure 8 This is an optical photograph of the material prepared in Comparative Example 1.
[0019] Figure 9 This is the powder X-ray diffraction pattern of the material prepared in Comparative Example 1.
[0020] Figure 10 This is the powder X-ray diffraction pattern of the material prepared in Comparative Example 3. DETAILED DESCRIPTION
[0021] The present invention provides a ternary layered selenide Ge3Sb4Se7 semiconductor material and a preparation method thereof. To further clarify the objectives, technical solutions, and effects of the present invention, the present invention is further described below with reference to the accompanying drawings and examples. It should be understood that the specific examples described herein are intended only to illustrate the present invention and are not intended to limit the present invention.
[0022] The present invention provides a method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material, comprising the following steps: S001. With a molar ratio of 3:4:7 of germanium powder, antimony powder, and selenium powder as raw materials, under vacuum conditions, the temperature is raised to 900~950 ℃ and kept at this temperature for 12~24h; within this temperature range, the germanium powder, antimony powder, and selenium powder are fully melted and reacted, thereby avoiding the formation of impurities; S002. After the holding period, cool the material to 475-500°C at a rate of 1-5°C / min and hold at this temperature for 3-5 days. After the holding period, cool the material to room temperature by furnace cooling or quenching to obtain a layered ternary selenide single-phase material with the chemical formula Ge3Sb4Se7. Selecting an appropriate cooling rate and holding the material within the temperature range of 475-500°C can promote homogenization of the chemical composition and structure of the Ge3Sb4Se7 material.
[0023] Preferably, in step S001, the purity of the germanium powder, antimony powder, and selenium powder is ≥99.99%.
[0024] Preferably, in step S001, the vacuum degree of the vacuum condition is ≤1 Pa to avoid the influence of air.
[0025] Preferably, in step S001, the heating rate is 1-5°C / min. In step S001, the heating rate cannot be too fast, otherwise the prepared material will easily experience component segregation and low density.
[0026] Example 1 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature melting and firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the tube close to the thermocouple. Raise the temperature from room temperature to 950°C at a rate of 5°C / min and keep it at this temperature for 12 h. Step 3: Material annealing For the material after heat preservation and firing in step 2, the temperature was cooled from 950°C to 475°C at a cooling rate of 2.5°C / min and kept at this temperature for 3 days; the vacuum-sealed quartz tube was cooled to room temperature along with the furnace, and then the material was taken out of the quartz tube.
[0027] Material organization and structural analysis The morphology, chemical composition and structure of the prepared materials were analyzed and characterized by optical microscopy, X-ray diffractometer, scanning electron microscopy, X-ray energy spectrum analysis and transmission electron microscopy. The specific characterization results are as follows: Figures 1 to 5 As shown. By analyzing the powder X-ray diffraction pattern ( Figure 2 ) and the comparison results with the standard card, and the microscopic morphology of the material was obtained by comprehensive analysis of scanning electron microscopy and X-ray energy spectrum ( Figure 3 ), the atomic ratio of each element ( Figure 4 ), and the crystal structure was obtained by high-angle annular dark field image obtained by transmission electron microscopy ( Figure 5 ), it was determined that the material obtained under this condition was a single-phase material, and its chemical composition was Ge3Sb4Se7.
[0028] In addition, the millimeter-scale needle-shaped material obtained by the reaction was observed, and it was determined that the macrostructure of the material had a layered morphology ( Figure 6 ), using X-ray testing and indexing of its diffraction pattern ( Figure 7 ), the diffraction peak was determined to be the crystal structure of Ge3Sb4Se7 (00 l ) crystal plane, the growth direction of the lamellae is the crystallographic cAxis-oriented, Ge3Sb4Se7 single crystal.
[0029] Example 2 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature melting and firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the tube close to the thermocouple. Raise the temperature from room temperature to 950°C at a rate of 5°C / min and keep it at this temperature for 12 h. Step 3: Material quenching treatment For the material after heat preservation and firing in step 2, the temperature is lowered from 950°C to 475°C at a cooling rate of 2.5°C / min and kept at this temperature for 3 days; the vacuum-sealed quartz tube is quenched and cooled to room temperature, and then the material is removed from the quartz tube; Material organization and structural analysis For the prepared materials, the morphology, chemical composition and structure of the obtained materials were analyzed and characterized by optical microscopy, X-ray diffractometer, scanning electron microscopy, X-ray energy spectrum analysis and transmission electron microscopy, and it was determined that Ge3Sb4Se7 material with a clear layered structure was obtained.
[0030] Example 3 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature melting and firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the tube close to the thermocouple. Raise the temperature from room temperature to 950°C at a rate of 5°C / min and keep it at this temperature for 12 h. Step 3: Material annealing For the material after heat preservation and firing in step 2, the temperature was cooled from 950°C to 500°C at a cooling rate of 2.5°C / min and kept at this temperature for 3 days; the vacuum-sealed quartz tube was cooled to room temperature along with the furnace, and then the material was taken out of the quartz tube.
[0031] Material organization and structural analysis For the prepared materials, the morphology, chemical composition and structure of the obtained materials were analyzed and characterized by optical microscopy, X-ray diffractometer, scanning electron microscopy, X-ray energy spectrum analysis and transmission electron microscopy, and it was determined that Ge3Sb4Se7 material with a clear layered structure was obtained.
[0032] Example 4 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature melting and firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the tube close to the thermocouple. Raise the temperature from room temperature to 900°C at a rate of 5°C / min and keep it at this temperature for 12 h. Step 3: Material annealing For the material after heat preservation and firing in step 2, the temperature was cooled from 900°C to 500°C at a cooling rate of 2.5°C / min and kept at this temperature for 5 days; the vacuum-sealed quartz tube was cooled to room temperature along with the furnace, and then the material was taken out of the quartz tube.
[0033] Material organization and structural analysis For the prepared materials, the morphology, chemical composition and structure of the obtained materials were analyzed and characterized by optical microscopy, X-ray diffractometer, scanning electron microscopy, X-ray energy spectrum analysis and transmission electron microscopy, and it was determined that Ge3Sb4Se7 material with a clear layered structure was obtained.
[0034] Comparative Example 1 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the quartz tube close to the thermocouple. Raise the temperature of the quartz tube from room temperature to 475°C at a rate of 5°C / min and keep it at this temperature for 3 days. Step 3: Material quenching treatment After the heat preservation and firing, the vacuum-sealed quartz tube is directly quenched and the material is then removed from the quartz tube.
[0035] Material organization and structural analysis The morphology, chemical composition and structure of the prepared materials were analyzed and characterized using optical microscopy, X-ray diffractometer, scanning electron microscopy and X-ray energy spectrometer. Figure 8 For the optical photograph of the prepared material, it was found that no dense product was formed under the process conditions, and the raw materials were difficult to fully react; and the powder X-ray diffraction pattern ( Figure 9 ) showed that the obtained material included Ge3Sb4Se7 phase and other phases such as Sb2Se3 (significant characteristic diffraction peaks as indicated by arrows). The combination of multiple results showed that Ge3Sb4Se7 single-phase material was not obtained.
[0036] Comparative Example 2 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the quartz tube close to the thermocouple. Heat the quartz tube from room temperature to 475°C at a rate of 5°C / min and keep it at this temperature for 3 days. After the insulation and firing, cool the vacuum-sealed quartz tube to room temperature with the furnace, and then remove the material from the quartz tube.
[0037] Material organization and structural analysis For the prepared materials, the morphology, chemical composition and structure of the obtained materials were analyzed and characterized by optical microscope, X-ray diffractometer, scanning electron microscope and X-ray energy spectrometer. The materials prepared under the process conditions were consistent with those in comparative example 1. The obtained materials included Ge3Sb4Se7 phase and other phases such as Sb2Se3, and no Ge3Sb4Se7 single-phase material was obtained.
[0038] Comparative Example 3 A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material comprises the following steps: Step 1: Ingredients and packaging Germanium powder with a purity of 99.99%, antimony powder with a purity of 99.99%, and selenium powder with a purity of 99.99% were used as raw materials. The germanium powder, antimony powder, and selenium powder were weighed and prepared in a molar ratio of 3:4:7. The mixture was placed in a quartz tube and evacuated to ≤1 Pa. The quartz tube containing the sample was then sealed using a flame sealing device. Step 2: High temperature firing Place the vacuum-sealed quartz tube vertically in a single-temperature-zone pit furnace, with the quartz tube close to the thermocouple. Heat the quartz tube from room temperature to 600°C at a rate of 5°C / min and keep it at this temperature for 3 days. After the insulation and firing, cool the vacuum-sealed quartz tube to room temperature with the furnace, and then remove the material from the quartz tube.
[0039] Material organization and structural analysis The morphology, chemical composition and structure of the prepared materials were analyzed and characterized by optical microscopy, X-ray diffractometer, scanning electron microscopy and X-ray energy spectrometer. The materials prepared under the process conditions were similar to those in Comparative Example 1, and the characteristic peak intensity of impurities was reduced ( Figure 10 ), Ge3Sb4Se7 single-phase material has not yet been obtained.
[0040] In summary, the results of the above embodiments and comparative examples show that only within a specific firing temperature range and under a specific cooling and heat preservation process can the obtained material be ensured to be a single-phase material.
[0041] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and inventive concept of the present invention, and all these changes or substitutions should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a ternary layered selenide Ge3Sb4Se7 semiconductor material, characterized in that: The steps include: S001. A molar ratio of 3:4:7 of germanium powder, antimony powder and selenium powder as raw materials was heated to 900-950°C under vacuum conditions and kept at this temperature for 12-24h; S002. After the insulation is completed, the temperature is lowered to 475-500°C at a cooling rate of 1-5°C / min and maintained at this temperature for 3-5 days; after the insulation is completed, the material is furnace cooled or quenched to room temperature to obtain a layered ternary selenide single-phase material with the chemical formula Ge3Sb4Se7.
2. The method for preparing the ternary layered selenide Ge3Sb4Se7 semiconductor material according to claim 1, characterized in that: In step S001, the purity of the germanium powder, antimony powder, and selenium powder is ≥99.99%.
3. The method for preparing the ternary layered selenide Ge3Sb4Se7 semiconductor material according to claim 1, characterized in that: In step S001, the vacuum degree of the vacuum condition is ≤1Pa.
4. The method for preparing the ternary layered selenide Ge3Sb4Se7 semiconductor material according to claim 1, characterized in that: In step S001, the heating rate is 1-5°C / min.
5. A ternary layered selenide Ge3Sb4Se7 semiconductor material, characterized in that: The ternary layered selenide Ge3Sb4Se7 semiconductor material is prepared by the preparation method of any one of claims 1 to 4, wherein the single crystal layer growth direction of the ternary layered selenide Ge3Sb4Se7 semiconductor material is crystallographically c Axis orientation.
Citation Information
Patent Citations
Layered Ge1-xSb4+xTe7 single crystal and preparation method thereof
CN117822122A
Cubic tin selenide-based thermoelectric crystal and preparation method thereof
CN119530948A
Layered ternary selenide, layered ternary selenide single crystal material and preparation method of layered ternary selenide single crystal material
CN119637814A
dust petroleum
KR1020220165104A
Cited By
Layered selenide Ge3Sb2Se5 semiconductor material and preparation method thereof
CN121593165A
Layered selenide ge3sb2se5 semiconductor material and method of preparation thereof
CN121593165B
Ternary layered selenide Ge0. 85Bi2.15 +xSe4 semiconductor material and preparation method thereof
CN121990527A
A ternary layered selenide Ge 0.85 Bi 2.15+x Se4 semiconductor material and a method of preparing the same
CN121990527B