Bimetallic supported cathode and method of making same, electrolytic descaling apparatus and method

By loading Ru and A metals onto the surface of a carbon steel or stainless steel electrode substrate to form a bimetallic layer, the problem of low descaling efficiency under low current density of carbon steel cathodes is solved, achieving efficient and economical electrostatic descaling and extending electrode life.

CN120757200BActive Publication Date: 2026-11-24BEIJING UNIV OF CHEM TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510901504.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-01
Publication Date
2026-11-24
Estimated Expiration
2045-07-01

AI Technical Summary

Technical Problem

Carbon steel cathodes have low electrolytic descaling efficiency at low current densities, making it difficult to reduce energy consumption in industrial applications. Furthermore, the catalytic layer of the cathode material is unevenly distributed and lacks sufficient bonding strength, failing to meet the requirements of industrial applications.

Method used

A bimetallic layer is formed by loading Ru and A metals (Ni, Co, Ce) onto the surface of a carbon steel or stainless steel electrode substrate. A bimetallic loaded cathode is prepared by impregnation method. The hydrogen evolution potential is reduced by utilizing the synergistic effect of bimetals, and the catalyst layer is ensured to be uniformly distributed and strongly bonded.

Benefits of technology

It improves the efficiency of electrostatic descaling, especially at low current densities, significantly enhancing descaling efficiency, reducing energy consumption, extending electrode life, and meeting the needs of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120757200B_ABST
    Figure CN120757200B_ABST
Patent Text Reader

Abstract

This invention provides a bimetallic loaded cathode and its preparation method, as well as an electrostatic descaling apparatus and method. The cathode is prepared by immersing a metal electrode substrate in a mixed solution containing a Ru source and an A metal source, wherein the A metal is selected from Ni, Co, and Ce. The molar ratio of the Ru source to the A metal source is 1-100:1, the molar amount of the Ru source is based on the molar amount of Ru, and the molar amount of the A metal source is based on the molar amount of A metal. The metal electrode substrate is carbon steel or stainless steel. Through the synergistic effect of the bimetallic cathode, the hydrogen evolution potential is reduced, thereby improving the electrostatic descaling efficiency, especially at low electrolysis current densities. It also ensures that the catalytic layer of the cathode material is uniformly distributed and has strong adhesion and corrosion resistance, further meeting the needs of industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrostatic descaling technology, specifically to a highly hydrogen evolution active bimetallic loaded carbon steel or stainless steel cathode for use in electrostatic descaling devices, its preparation method, and the corresponding electrostatic descaling method. Background Technology

[0002] Electrostatic descaling technology removes scale by causing cations such as calcium and magnesium in the water to migrate to the cathode under the action of a DC electric field. In the alkaline microenvironment of the cathode interface, they combine with hydroxide ions to form precipitates, thereby removing scale. It has advantages such as being environmentally friendly and easy to operate.

[0003] As the core component of the electrostatic descaling device, the hydrogen evolution performance of the cathode directly affects the descaling efficiency and energy consumption.

[0004] Carbon steel is the most commonly used cathode material for industrial electrolytic descaling due to its advantages such as high mechanical strength and low cost. However, carbon steel has low electrolytic descaling efficiency at low current densities, so industrial applications often rely on large electrolysis currents, making it difficult to reduce energy consumption in industrial applications. Summary of the Invention

[0005] (I) Purpose of the Invention

[0006] The purpose of this invention is to provide a bimetallic loaded metal cathode and its preparation method, as well as an electrostatic descaling device and method. By impregnating a carbon steel or stainless steel electrode substrate with a bimetal, the hydrogen evolution potential of the cathode is reduced through the synergistic effect of the bimetal, which not only improves the electrostatic descaling efficiency, especially the descaling efficiency at low electrolysis current densities, but also ensures that the cathode material catalyst layer is uniformly distributed and has strong bonding force and corrosion resistance, further meeting the needs of industrial applications.

[0007] (II) Technical Solution

[0008] To address the aforementioned problems, a first aspect of the present invention provides a bimetallic loaded cathode, which is prepared by immersing a metal electrode substrate in a mixed solution containing a Ru source and an A metal source, wherein the A metal is selected from any one of Ni, Co, and Ce, the molar ratio of the Ru source to the A metal source is 1-100:1, the molar amount of the Ru source is expressed as the molar amount of Ru, the molar amount of the A metal source is expressed as the molar amount of A metal, and the metal electrode substrate is carbon steel or stainless steel.

[0009] In this embodiment of the invention, the metal electrode substrate is sheet-shaped carbon steel or sheet-shaped stainless steel.

[0010] By loading bimetals onto the surface of a metal electrode substrate through an impregnation method, the hydrogen evolution potential at the cathode is reduced through the synergistic effect of the bimetals. This not only improves the efficiency of electrolytic descaling but also ensures that the catalytic layer of the cathode material is uniformly distributed and has strong adhesion and corrosion resistance, thus better meeting the needs of industrial applications.

[0011] In a preferred embodiment, metal A is Ni or Ce, and the molar ratio of Ru source to metal A source is 5-50:1; or metal A is Co, and the molar ratio of Ru source to metal A source is 90-100:1.

[0012] While improving hydrogen evolution capability, it can ensure that the bimetallic layer loaded on the cathode surface is uniformly and densely distributed.

[0013] In a more preferred embodiment, the metal A is Ce, and the molar ratio of the Ru source to the metal A source is 9-11:1.

[0014] When Ru and Ce are mixed in the above molar ratio, the bimetallic loaded carbon steel cathode at 1 mA·dm -2 At the current density, the hydrogen evolution potential can be reduced to -1.28V, and the catalyst layer on the surface of the bimetallic supported carbon steel cathode is uniform, dense, and has good adhesion.

[0015] Meanwhile, this bimetallic-loaded carbon steel cathode operates at 0.05-0.1 A·dm. -2 Compared to carbon steel electrodes, this method achieves a hardness removal rate increase of over 27% and an alkalinity removal rate increase of over 30% at the same current density, comparable to carbon steel electrodes at commonly used industrial current densities (0.2 A·dm³). -2 With a considerable scale removal efficiency, in an electrostatic descaling system that operates continuously and stably for a long time, low current density operation can effectively reduce energy consumption and operating costs, while also reducing electrode wear and deterioration under high current, providing good protection for electrode life and facilitating more economical and long-term system operation.

[0016] Specifically, the Ru source is selected from organic solvent-soluble salts of Ru, preferably ruthenium trichloride trihydrate; the A metal source is selected from organic solvent-soluble salts of A metal, preferably nickel chloride hexahydrate, cobalt chloride hexahydrate, or cerium chloride heptahydrate.

[0017] In an optional embodiment, the organic solvent is a mixed solution of ethanol and isopropanol, wherein the volume ratio of ethanol to isopropanol is 1:15-25, and the molar concentration of the Ru source in the mixed solution is 0.01-0.02 mol / L. The molar concentration of the A metal source is 0.00015-0.015 mol / L.

[0018] The metal electrode substrate is impregnated in a mixed solution containing Ru source and A metal source. The specific preparation method is consistent with the preparation method of the second aspect of the present invention. For details, please refer to the description of the preparation method below.

[0019] A second aspect of the present invention provides a method for preparing a bimetallic loaded cathode, the method comprising:

[0020] Step 1: Pre-treat the metal electrode substrate;

[0021] Step 2: Immerse the pretreated metal electrode substrate in a mixed solution containing Ru source and A metal source, and dry it to obtain a bimetallic supported carbon steel cathode.

[0022] The metal electrode substrate described in step 1 of this invention undergoes pretreatment, specifically including: polishing, degreasing, ultrasonic cleaning, etching, and drying.

[0023] Specifically, the polishing conditions include: using 600-1200 grit sandpaper to polish along the same direction on the surface of the metal electrode substrate to remove surface impurities and oxide layers, making the surface smooth and uniform.

[0024] Specifically, surfactants such as laundry detergent are used to scrub and remove oil from the polished metal electrode substrate;

[0025] The ultrasonic cleaning specifically includes: using ethanol as the cleaning agent, and the cleaning time is 20-40 seconds;

[0026] The specific etching conditions include: the etching solution is a mixture of concentrated sulfuric acid, concentrated nitric acid and water, wherein the concentrated sulfuric acid is 5-10 mL / L and the concentrated nitric acid is 3-10 mL / L, and the etching time is 30-60 s.

[0027] By using a pretreatment process involving sanding, degreasing, ultrasonic cleaning, and etching, the surface of the carbon steel substrate can be kept clean and have a certain degree of roughness, which is more conducive to the subsequent impregnation of elements.

[0028] Specifically, the reaction described in step 2 includes:

[0029] The reaction temperature is 20-60℃, and the reaction time is 3-28h.

[0030] Specifically, the Ru source is selected from organic solvent-soluble salts of Ru, preferably ruthenium trichloride trihydrate; the A metal source is selected from organic solvent-soluble salts of A metal, preferably nickel chloride hexahydrate, nickel nitrate hexahydrate, cobalt chloride hexahydrate, cobalt nitrate hexahydrate, cerium chloride heptahydrate, and cerium nitrate hexahydrate. In an optional embodiment, the organic solvent is a mixed solution of ethanol and isopropanol, wherein the volume ratio of ethanol to isopropanol is 1:15-25, and the molar concentration of the Ru source in the mixed solution is 0.01-0.02 mol / L. The molar concentration of the A metal source is 0.00015-0.015 mol / L.

[0031] After the reaction is complete, the product can be air-dried naturally or dried in an oven at 50–200℃ for 15–120 minutes.

[0032] In a specific embodiment of the present invention, a process for preparing a highly hydrogen evolution active Ce-Ru dual-loaded carbon steel cathode for use in an electrostatic descaling device includes the following steps:

[0033] S1. Pretreatment of the metal electrode substrate: The carbon steel sheet is polished with sandpaper of different grits until the surface is smooth, then immersed in an ethanol solution for ultrasonic cleaning to remove surface oil and impurities. After removal, it is rinsed with deionized water and dried for later use. Next, it is etched in an etching solution, then quickly rinsed with deionized water and dried for later use.

[0034] Preparation of S2 and Ru-based bimetallic supported component solutions: With a fixed amount of ruthenium trichloride trihydrate (RuCl3·3H2O), weigh out nickel chloride hexahydrate (NiCl2·6H2O), cobalt chloride hexahydrate (CoCl2·6H2O), cerium chloride heptahydrate (CeCl3·7H2O), and lanthanum chloride heptahydrate (LaCl3·7H2O). Adjust the molar ratio of Ni / Co / Ce / La and Ru according to the specified proportions. First, add ethanol to completely dissolve the Ni / Co / Ce / La salts. Then, weigh out RuCl3·3H2O and dissolve the above substances together with isopropanol to prepare four bimetallic solutions: Ni-Ru, Co-Ru, Ce-Ru, and La-Ru. Make up to a final volume for later use.

[0035] S3. Impregnation and drying of Ru-based bimetallic loaded carbon steel cathode: The pretreated carbon steel sheet is vertically immersed in the above solution. The temperature is kept constant throughout the impregnation process. After a certain period of impregnation, the carbon steel sheet is removed and placed in an oven for drying. After a certain period of time, the carbon steel sheet is allowed to cool down slowly with the oven until it reaches room temperature, thus obtaining the bimetallic loaded carbon steel cathode.

[0036] Furthermore, in step S1, the ultrasonic cleaning time is 2 minutes.

[0037] Furthermore, in step S1, the etching solution is a sulfuric acid-nitric acid mixture, containing 8.3 mL / L concentrated sulfuric acid and 5.5 mL / L concentrated nitric acid, and the etching time is 30 s.

[0038] Furthermore, in step S3, the immersion temperature is controlled at 20-60℃ throughout the experiment, the immersion time is 3-48h, the drying temperature is natural air drying at 50-200℃, and the drying time is 15-120min.

[0039] Furthermore, in step S2, the amount of ruthenium trichloride trihydrate (RuCl3·3H2O) is 4 g / L, and the molar ratio of Ni / Co / Ce / La and Ru is adjusted to 1:1 to 1:100.

[0040] Furthermore, in step S2, the amount of ethanol used to dissolve the Ni / Co / Ce / La salt is 5 mL.

[0041] A third aspect of the present invention provides an electrostatic descaling apparatus, comprising an electrolyte, a DC power supply, and a cathode connected to the DC power supply, wherein the electrolyte comprises water, and the cathode is any one of the bimetallic loaded carbon steel cathode described above or the bimetallic loaded carbon steel cathode prepared by the above preparation method.

[0042] For a detailed description of the cathode, please refer to the description of the cathode and its preparation method above, which will not be repeated here.

[0043] Specifically, the current density of the DC power supply is 0.025–0.2 A·dm³. -2 Preferred concentration: 0.05–0.1 A·dm -2 At this current density, it is possible to achieve the same current density as a blank carbon steel electrode at the commonly used industrial current density (0.2 A·dm³). -2 It achieves a comparable scale removal efficiency. In an electrostatic descaling system that operates continuously and stably over a long period, low current density operation can effectively reduce energy consumption and operating costs, while also mitigating electrode wear and degradation under high current conditions, thus providing good protection for electrode life and facilitating more economical and long-term system operation.

[0044] Specifically, the initial total hardness of the water is 300-500 mg / L (calculated as CaCO3). When the water hardness is within this range, the device is used at a current density of 0.025-0.2 A·dm³. -2 At this time, the Ce-Ru dual-load carbon steel cathode with a Ce to Ru molar ratio of 1:9-11 can achieve a hardness removal rate of 14.8%-22.3% in about 1 hour, especially at a current density of 0.025 A·dm³. -2 At that time, the hardness removal rate of Ce-Ru dual-load carbon steel cathode was 78.3% higher than that of blank carbon steel.

[0045] In a fourth aspect, the present invention provides an electrostatic descaling method, which is carried out using the apparatus described in any of the preceding claims. For a description of the apparatus, please refer to the above-described apparatus, which will not be repeated here.

[0046] Preferably, the method includes:

[0047] A certain amount of water to be treated is subjected to pre-electrostatic descaling, wherein the current density for pre-electrostatic descaling is 0.025-0.2 A·dm³. -2 The time is 10-30 minutes;

[0048] After removing the water from the pre-electrolytic descaling process, add the water to be treated as the electrolyte to perform electrolytic descaling.

[0049] Pre-electrolysis can eliminate scale ion interference and activate the electrode, enabling scale removal and hydrogen evolution reaction to proceed synergistically and efficiently during the main electrolysis, thereby increasing the scale removal efficiency of the electrode by more than 10% within 1 hour.

[0050] (III) Beneficial Effects

[0051] The above-described technical solution of the present invention has the following beneficial technical effects:

[0052] This invention loads a bimetal onto the surface of a metal electrode substrate using an impregnation method. Through the synergistic effect of the bimetal, the hydrogen evolution potential at the cathode is reduced, which not only improves the electrolytic descaling efficiency, especially at low current densities, but also ensures that the cathode material catalyst layer is uniformly distributed and has strong adhesion and corrosion resistance, thus meeting the needs of industrial applications. Attached Figure Description

[0053] Figure 1 These are the hydrogen evolution effect diagrams provided in Examples 1-4 of the present invention, where a is the LSV curve of hydrogen evolution at the cathode, and b is the hydrogen evolution curve at the cathode at 1 mA·cm⁻¹. -2 Hydrogen evolution potential diagram at current density;

[0054] Figure 2 These are hydrogen evolution effect diagrams provided in Examples 5-8 of the present invention, where a is the LSV curve of hydrogen evolution at the cathode, and b is the hydrogen evolution effect at the cathode at 1 mA·cm⁻¹. -2 Hydrogen evolution potential diagram at current density;

[0055] Figure 3 The figures shown are for hydrogen evolution effect diagrams provided in Examples 9-12 of this invention, where a is the LSV curve of hydrogen evolution at the cathode, and b is the hydrogen evolution effect at the cathode at 1 mA·cm. -2 Hydrogen evolution potential diagram at current density;

[0056] Figure 4 These are cathode surface morphology diagrams provided in Embodiments 9-12 of the present invention, where a is Embodiment 9, b is Embodiment 10, c is Embodiment 11, and d is Embodiment 12;

[0057] Figure 5 The graphs show the change of open-circuit potential of blank carbon steel and Ce-Ru dual-load carbon steel cathodes provided in Example 10 over time. Detailed Implementation

[0058] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments and the accompanying drawings. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and techniques are omitted in the following description to avoid unnecessarily obscuring the concept of the invention.

[0059] The raw materials and reagents used in all embodiments of this invention are conventional commercially available products, wherein:

[0060] The carbon steel electrode substrate used in each embodiment of the present invention is a Q235 carbon steel sheet of type I purchased from Feiruida Machinery Equipment Business Department of Jinshan District, Shanghai.

[0061] The ruthenium-iridium-titanium mesh anode used was purchased from Suzhou Shuertai Industrial Technology Co., Ltd., and the model is 65mm×130mm×1mm;

[0062] The Ru source used, ruthenium trichloride trihydrate, was purchased from Shanghai Maclean Biochemical Technology Co., Ltd., with a purity of 98%.

[0063] Nickel chloride hexahydrate, cobalt chloride hexahydrate, and cerium chloride heptahydrate in metal source A were all purchased from Shanghai Maclean Biochemical Technology Co., Ltd., and their purity was 99%.

[0064] The organic solvent isopropanol was purchased from Tianjin Fuyu Fine Chemical Co., Ltd., with a purity of 99.7%.

[0065] Anhydrous ethanol was purchased from Fuchen (Tianjin) Chemical Reagent Co., Ltd., with a purity of 95%.

[0066] The concentrated sulfuric acid and concentrated nitric acid used in the etching solution were purchased from Beijing Tongguang Fine Chemical Co., Ltd., with mass fractions of 98% and 68%, respectively.

[0067] Example 1

[0068] A Ni-Ru dual-loaded carbon steel cathode, the specific preparation steps of which are as follows:

[0069] Step 1: Pretreatment of carbon steel electrode substrate

[0070] The carbon steel sheet was polished in the same direction with 600-grit and 1200-grit sandpaper until the surface was smooth and uniform, removing impurities and oxide layers. The sheet was then scrubbed with a suitable amount of laundry detergent to remove oil, rinsed with deionized water, and quickly dried with cold air. Next, the sheet was ultrasonically cleaned in anhydrous ethanol for 30 seconds, rinsed thoroughly with deionized water, and quickly dried. Finally, it was etched in the etching solution for 30 seconds, immediately removed, quickly rinsed with deionized water, and dried for later use. The etching solution was a mixture of concentrated sulfuric acid, concentrated nitric acid, and water, with 8.3 mL / L of concentrated sulfuric acid and 5.5 mL / L of concentrated nitric acid.

[0071] Step 2: Preparation of Ni-Ru dual-loaded solution

[0072] Using NiCl2·6H2O as the nickel source and RuCl3·3H2O as the Ru source, the nickel source and Ru source were weighed according to a molar ratio of Ni to Ru of 1:1 and placed in a beaker.

[0073] First, dissolve the nickel source in 5 ml of ethanol, then slowly pour in 95 ml of isopropanol and stir slowly with a glass rod until the mixture is homogeneous, thus preparing a Ni-Ru dual-loaded solution with a Ru molar concentration of 0.015 mol / L.

[0074] Step 3: The carbon steel sheet obtained from the first step of pretreatment is vertically immersed in the dual-load solution obtained in the second step. The immersion temperature is kept constant at 30°C throughout the immersion process. After immersion for 24 hours, the carbon steel sheet is taken out and placed in an oven at 100°C for 30 minutes. After drying, the carbon steel sheet is allowed to cool with the oven to obtain the Ni-Ru dual-load carbon steel cathode.

[0075] Examples 2-4

[0076] Each of the following is a Ni-Ru dual-loaded carbon steel cathode, prepared in a manner similar to that of Example 1, except that: in the second step of Example 2, the molar ratio of Ni to Ru is 1:10; in the second step of Example 3, the molar ratio of Ni to Ru is 1:50; and in the second step of Example 4, the molar ratio of Ni to Ru is 1:100.

[0077] Example 5

[0078] The specific preparation steps of a Co-Ru dual-loaded carbon steel cathode are as follows:

[0079] Step 1: Same as Example 1;

[0080] Step 2: Basically the same as in Example 1, except that CoCl2·6H2O is used instead of nickel source to obtain a Co-Ru dual-loaded solution prepared according to a molar ratio of Co to Ru of 1:1.

[0081] Step 3: Same as in the example, a Co-Ru dual-loaded carbon steel cathode is obtained.

[0082] Examples 6-8

[0083] Each of the above provides a Co-Ru dual-load carbon steel cathode, and the preparation method is basically the same as that of Example 5. The difference is that the molar ratio of Co to Ru in the second step of Example 6 is 1:10, the molar ratio of Co to Ru in the second step of Example 7 is 1:50, and the molar ratio of Co to Ru in the second step of Example 8 is 1:100.

[0084] Example 9

[0085] The specific preparation steps of a Ce-Ru dual-loaded carbon steel cathode are as follows:

[0086] Step 1: Same as Example 1;

[0087] Step 2: Basically the same as in Example 1, except that CeCl3·7H2O is used instead of nickel source to prepare Ce-Ru dual-loaded solution according to the molar ratio of Ce to Ru of 1:1.

[0088] Step 3: Same as in Example 1, a Ce-Ru dual-loaded carbon steel cathode is obtained.

[0089] Examples 10-12

[0090] Each of the following is a Ce-Ru dual-load carbon steel cathode, prepared in a manner similar to that of Example 9. The difference is that in the second step of Example 10, the molar ratio of Ce to Ru is 1:10; in the second step of Example 11, the molar ratio of Ce to Ru is 1:50; and in the second step of Example 12, the molar ratio of Ce to Ru is 1:100.

[0091] Comparative Example 1

[0092] The specific preparation steps for a single-load Ru carbon steel cathode are as follows:

[0093] Step 1: Pretreatment of carbon steel substrate

[0094] The carbon steel sheet was polished in the same direction with 600-grit and 1200-grit sandpaper until the surface was smooth and uniform, removing impurities and oxide layers. The sheet was then scrubbed with a suitable amount of laundry detergent to remove oil, rinsed with deionized water, and quickly dried with cold air. Next, the sheet was ultrasonically cleaned in anhydrous ethanol for 30 seconds, rinsed thoroughly with deionized water, and quickly dried. Finally, it was etched in an etching solution for 30 seconds, immediately removed, quickly rinsed with deionized water, and dried for later use. The etching solution was a mixture of concentrated sulfuric acid, concentrated nitric acid, and water, containing 8.3 mL / L of concentrated sulfuric acid and 5.5 mL / L of concentrated nitric acid.

[0095] Step 2: Preparation of single-loaded Ru solution

[0096] Weigh a measured amount of ruthenium trichloride trihydrate (RuCl3·3H2O), place it in a beaker, and slowly pour in an appropriate amount of isopropanol. Stir slowly with a glass rod until the ruthenium trichloride trihydrate is completely dissolved. Then, transfer the solution to a brown volumetric flask using a glass rod. Continue to rinse the inner wall of the beaker with isopropanol several times and transfer the solution to the volumetric flask. Make up to the mark to prepare a Ru solution with a concentration of 4 g / L.

[0097] Step 3: Impregnation and drying of single-load Ru carbon steel cathode

[0098] The pretreated carbon steel sheet was vertically immersed in the Ru loading solution, and the temperature was kept constant at 30°C throughout the immersion process. After immersion for 24 hours, the carbon steel sheet was removed and placed in an oven at 100°C for 30 minutes. After drying, the carbon steel sheet was allowed to cool with the oven to obtain a single-load Ru carbon steel cathode.

[0099] Comparative Example 2

[0100] The specific preparation steps of the La-Ru dual-load carbon steel cathode are as follows:

[0101] Step 1: The carbon steel substrate pretreatment method is the same as in Example 1.

[0102] Step 2: Preparation of La-Ru dual-loaded solution

[0103] With a fixed amount of RuCl3·3H2O and LaCl3·7H2O as the La source, adjust the La-Ru loading molar ratio to 1:1. Calculate the required amount of LaCl3·7H2O according to the ratio. First, add a small amount of ethanol to completely dissolve the La salt. Then, weigh out a fixed amount of RuCl3·3H2O, place it in a beaker, and slowly pour in an appropriate amount of isopropanol. Stir slowly with a glass rod until the mixture is evenly dissolved. Then, transfer the solution to a brown volumetric flask using a glass rod. Continue to add appropriate amounts of isopropanol several times to repeatedly rinse the inner wall of the beaker and transfer the solution. Make up to the mark.

[0104] Step 3: The impregnation and drying methods for the La-Ru dual-loaded carbon steel cathode are the same as in Example 1, to obtain the La-Ru dual-loaded carbon steel cathode.

[0105] Hydrogen evolution performance tests were conducted on the carbon steel cathodes obtained in Examples 1-12 and Comparative Examples 1 and 2:

[0106] The testing methods include:

[0107] A three-electrode system was used, with carbon steel cathodes obtained in Examples 1-12 and Comparative Examples 1 and 2 as working electrodes, saturated calomel electrodes as reference electrodes, and platinum electrodes as counter electrodes. Linear voltammetric scans were performed in simulated circulating water (calculated as CaCO3) with a hardness of 400 mg / L. The scan range was set to 0 to -3 V, and the scan rate was 5 mV·s. -1 .

[0108] See test results Figure 1-3 The results show that the Ce-Ru dual-load carbon steel cathode provided in Example 10 exhibits the best synergistic effect: at 1 mA·cm -2 At the specified current density, the hydrogen evolution potential decreased to -1.28V, a further reduction of 110mV compared to the single-loaded Ru@carbon steel cathode (-1.39V) (Comparative Example 1), and a reduction of 580mV compared to the blank carbon steel cathode (-1.86V), representing a 32% decrease. This is superior to the bimetallic loaded carbon steel cathodes provided in other embodiments. This is because when the Ru / Ce ratio is maintained within the range of Example 10, the sufficient exposure of Ru active sites and the electronic structure regulation effect of Ce jointly reduce the energy barrier of the hydrogen evolution reaction. Ce regulates the d-band center position of Ru through electron transfer, thereby reducing the binding energy of hydrogen intermediates. At the same time, the interfacial anchoring effect of Ce anchors Ru nanoparticles to the carbon steel substrate interface, restricting their migration and aggregation, and maintaining a high active site density.

[0109] Referring to ASTM D3359-2017, "Standard Test Method for Assessing Adhesion by Adhesive Tape Test," the Ce-Ru dual-load carbon steel cathode provided in Examples 9-12 was placed on filter paper. 3M tape was then adhered to the cathode surface. A rubber eraser of the same width as the 3M tape was used to vigorously rub the tape surface, ensuring uniform contact between the tape and the cathode surface. After standing for 20 minutes, the 3M tape was quickly peeled off, and the cathode was weighed. The data are shown in Table 1.

[0110] Table 1 shows the changes in cathode material quality as provided in Examples 9-12.

[0111]

[0112] Combine the data in Table 1 and refer to... Figure 4 It can be seen that the catalytic layer of the Ce-Ru dual-loaded carbon steel cathode provided in Example 10 is uniform, dense and has good adhesion.

[0113] In addition, see Figure 1 Of the bimetallic loaded carbon steel cathodes provided in Examples 1-4, the cathode provided in Example 1 had the lowest hydrogen evolution potential of -1.30V, but the carbon steel surface exhibited poor adhesion and was prone to slagging. In contrast, the cathode provided in Example 2 had a hydrogen evolution potential as low as -1.34V, and by reducing the Ni content, structural distortion and stress problems were alleviated, maintaining the integrity of the load layer on the carbon steel cathode surface. See also... Figure 2 In the bimetallic loaded carbon steel cathodes provided in Examples 5-8, the carbon steel cathode provided in Example 8 not only reduced the hydrogen evolution potential but also alleviated the structural distortion and stress problems of the load layer, maintaining the integrity of the load layer. The La-Ru dual-loaded carbon steel cathode provided in Comparative Example 2, at a 1:1 load molar ratio, had a hydrogen evolution potential of -1.41V, higher than the -1.39V hydrogen evolution potential of the single-loaded Ru carbon steel cathode. Furthermore, at this molar ratio, the carbon steel surface exhibited poor adhesion and was prone to slagging.

[0114] like Figure 5 The results show that the graph depicts the open-circuit potential of the blank carbon steel cathode and the Ce-Ru dual-loaded carbon steel cathode provided in Example 10 as a function of time. The open-circuit potential of the blank carbon steel cathode remained stable at approximately -0.75V (vs. SCE), while that of the Ce-Ru dual-loaded carbon steel cathode remained stable at approximately -0.45V (vs. SCE). A more positive open-circuit potential indicates a lower tendency for corrosion and stronger corrosion resistance. Therefore, the Ce-Ru dual-loaded carbon steel cathode exhibits better corrosion resistance than the blank carbon steel cathode. The Ce-Ru dual loading effectively improves the corrosion resistance of the carbon steel cathode and reduces its tendency to undergo corrosion reactions such as cathodic hydrogen evolution.

[0115] Application Example 1

[0116] Using the dual-load carbon steel cathode provided in Example 10 as the cathode and the ruthenium-iridium-titanium mesh as the anode, the dual-load carbon steel cathode is connected to the negative terminal of the regulated DC power supply, and the anode is connected to the positive terminal of the DC power supply to obtain an electrolytic descaling device. The effective capacity of the electrolytic cell of the electrolytic descaling device is 1.5L.

[0117] The distance between the dual-load carbon steel cathode and anode is 12cm, and the electrolyte is simulated circulating water with a hardness of 480mg / L (calculated as CaCO3).

[0118] During electrolysis, first at 0.025 A·dm -2 Pre-electrolysis was performed for 20 minutes at a current density of 0.025 A·dm³, then the simulated circulating water in the electrolytic cell was removed, and simulated circulating water was added back in at 0.025 A·dm³. -2 Electrolyze at the specified current density for 60 minutes.

[0119] Application Examples 2-4

[0120] The application example is basically the same as in Example 1, except that the pre-electrolysis current density and the electrolysis current density are 0.05 A·dm³ in Example 2. -2 Application Example 3 is 0.1 A·dm -2 Application Example 4 is 0.2 A·dm -2 .

[0121] Using a blank carbon steel electrode as the cathode, tests were conducted under the same conditions as in Application Examples 1-4.

[0122] The test results are shown in Table 2.

[0123] Table 2. Descaling effect data of electrolytic descaling device

[0124]

[0125]

[0126] Experimental results show that at 0.025–0.2 A·dm -2 Within the current density range, the electrolysis apparatus using the Ce-Ru@carbon steel cathode provided in Example 10 consistently achieved higher removal rates of hardness and alkalinity than the blank carbon steel. This was especially true at 0.025 A·dm³. -2 At low current density, the hardness removal rate was increased by 78.3% compared to blank carbon steel.

[0127] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the appended claims, or equivalent forms of such scope and boundaries.

Claims

1. A bimetallic loaded cathode, characterized in that, The electrode is prepared by impregnating a metal electrode substrate in a mixed solution containing a Ru source and an A metal source, wherein the A metal is Ce, the molar ratio of the Ru source to the A metal source is 9-11:1, the Ru source is ruthenium trichloride trihydrate, the A metal source is cerium chloride heptahydrate, the solvent of the mixed solution is a mixture of ethanol and isopropanol, wherein the volume ratio of ethanol to isopropanol is 1:15-25, the molar concentration of the Ru source in the mixed solution is 0.01-0.02 mol / L, the molar concentration of the A metal source is 0.00015-0.015 mol / L, the molar amount of the Ru source is expressed as the molar amount of Ru, the molar amount of the A metal source is expressed as the molar amount of A metal, and the metal electrode substrate is carbon steel or stainless steel.

2. The method for preparing the bimetallic supported cathode according to claim 1, characterized in that, include: Step 1: Pre-treat the metal electrode substrate; Step 2: Immerse the pretreated metal electrode substrate in a mixed solution containing Ru source and A metal source, and dry it to obtain a bimetallic supported metal cathode.

3. The preparation method according to claim 2, characterized in that, The reaction described in step 2 includes: The reaction temperature is 20-60℃, and the reaction time is 3-28h.

4. An electrostatic descaling device, comprising an electrolyte, a DC power supply, and a cathode connected to the DC power supply, characterized in that, The electrolyte includes water, and the cathode is any one of the bimetallic loaded cathode of claim 1, or the bimetallic loaded cathode prepared by the preparation method of claim 2 or 3.

5. The apparatus according to claim 4, characterized in that, The current density of the DC power supply is 0.025-0.2 A·dm. -2 .

6. The apparatus according to claim 4, characterized in that, The initial total hardness of the water is 300-500 mg / L, calculated as CaCO3.

7. An electrostatic descaling method, characterized in that, The apparatus described in any one of claims 4-6 shall be used.

8. The electrostatic descaling method according to claim 7, characterized in that, include: A certain amount of water to be treated is subjected to pre-electrostatic descaling, wherein the current density for pre-electrostatic descaling is 0.025~0.2 A·dm³. -2 The time is 10-30 minutes; After removing the water from the pre-electrolytic descaling process, add the water to be treated as the electrolyte to perform electrolytic descaling.

Citation Information

Patent Citations

  • Nanometer material with precious metal single atoms dispersed on surface of non-precious metal substrate and preparation method and application of nanometer material

    CN114525521A