PBT-petg alloy material, preparation method and application thereof
By adding compatibilizers and transesterification inhibitors to PBT and PETG alloys and controlling the temperature and rotation speed, PBT-PETG alloys with high transparency and good chemical resistance were prepared, solving the problems of insufficient transparency and mechanical properties in the existing technology and reducing production costs and difficulties.
Patent Information
- Application Number
- CN202511166122.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-20
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-08-20
AI Technical Summary
Existing technologies struggle to achieve PBT-PETG alloy materials with high transparency and excellent mechanical properties while maintaining the superior performance of PBT resin. Furthermore, the synthesis process of PETG is complex, costly, and has a narrow processing window, which increases the difficulty of production.
By mixing PBT and PETG polymers in a specific ratio and adding compatibilizers, transesterification inhibitors, epoxy compounds and antioxidants, and then extruding and granulating the mixture using a twin-screw extruder while controlling the temperature and speed, a PBT-PETG alloy material with high transparency and good chemical resistance was prepared.
This technology achieves high transparency, good chemical resistance, easy molding, short molding time, and good compatibility in PBT-PETG alloy materials, thereby reducing production costs and improving the processing conditions of PETG.
Smart Images

Figure BDA0005556623740000081 
Figure BDA0005556623740000091 
Figure BDA0005556623740000101
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, and more specifically, to a PBT-PETG alloy material, its preparation method, and its application. Background Technology
[0002] Polybutylene terephthalate (PBT), one of the five major engineering plastics, occupies an important position in electronic and electrical components, automotive parts, and industrial machinery parts due to its excellent mechanical strength, heat resistance, electrical insulation, and chemical corrosion resistance. This material is industrially produced through transesterification or direct esterification. The benzene ring structure and butanediol segments in its molecular chain endow the material with good rigidity and dimensional stability. However, due to the highly ordered crystalline structure within PBT resin, light is scattered within the material, resulting in a milky white appearance. This characteristic makes it unsuitable for applications such as optical devices and transparent packaging, where strict requirements for light transmittance are necessary.
[0003] Polyethylene terephthalate-1,4-cyclohexanediethanol (PETG) is an amorphous copolyester produced by introducing a third monomer, 1,4-cyclohexanediethanol (CHDM), during the PET synthesis process. The steric hindrance effect of the CHDM monomer disrupts the regularity of the molecular chain, giving the material excellent transparency (light transmittance can reach over 90%), while maintaining the inherent chemical resistance and processing properties of polyester materials. This material is widely used in fields requiring high transparency, such as medical devices, food packaging, and display windows. However, the synthesis process of the CHDM monomer in PETG raw materials is complex, resulting in a price that is 2-3 times that of ordinary PET resin; in addition, its melt strength is low and its processing window is narrow (melt temperature range is only 230-250℃), requiring precise control of injection molding or extrusion process parameters, which significantly increases production costs and technical barriers.
[0004] Although polymer blending modification schemes have been proposed to address the shortcomings of single polymers in certain properties, the large differences in properties between different polymers lead to poor compatibility of the system during the polymer blending modification process. At the same time, how to ensure that the polymer blended modified material can simultaneously possess the advantages of each single polymer is one of the problems that urgently needs to be solved in this field.
[0005] In view of this, the present invention is proposed. Summary of the Invention
[0006] The purpose of this invention is to provide a PBT-PETG alloy material, its preparation method, and its application.
[0007] This invention is implemented as follows:
[0008] In a first aspect, the present invention provides a PBT-PETG alloy material, comprising, by weight:
[0009] 20-35 parts of polybutylene terephthalate;
[0010] 63-78 parts of polyethylene terephthalate-1,4-cyclohexanediol ester;
[0011] 0-1 part of epoxy compound;
[0012] Antioxidant 0.1–0.5 parts;
[0013] Release agent 0.1-0.5 parts;
[0014] Compatibilizer 0-2 parts;
[0015] Transesterification inhibitor 0.1 to 0.5 parts.
[0016] In a second aspect, the present invention provides a method for preparing a PBT-PETG alloy material as described in any of the foregoing embodiments, comprising mixing polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanediol ester, an epoxy compound, an antioxidant, a release agent, a compatibilizer, and an ester exchange inhibitor, followed by extrusion granulation.
[0017] Preferably, the extrusion is performed using a twin-screw extruder, which has 11 temperature zones from the feed section to the discharge section, and the temperatures of the 11 temperature zones along the direction from the feed section to the discharge section are as follows: 100~120℃, 220~230℃, 230~240℃, 230~240℃, 225~235℃, 225~235℃, 225~235℃, 225~235℃, 225~235℃, and 230~240℃.
[0018] Preferably, the twin-screw extruder rotates at a speed of 200–300 rpm.
[0019] Thirdly, the present invention provides the application of a PBT-PETG alloy material as described in any of the foregoing embodiments or a PBT-PETG alloy material prepared by the preparation method described in the foregoing embodiments in mechanical structures, packaging materials or medical devices.
[0020] The present invention has the following beneficial effects:
[0021] This invention provides a PBT-PETG alloy material, its preparation method, and its applications. By using polybutylene terephthalate (PBT) and polyethylene terephthalate-1,4-cyclohexanediol (PETG) as the main structural components, the addition of compatibilizers and transesterification inhibitors significantly improves the compatibility of the two materials while maintaining their original chemical resistance. Strictly controlling the ratio of PBT resin to PETG resin is crucial for maintaining the high transparency of this alloy material. Furthermore, as the PBT resin content increases, the PETG resin content decreases, further reducing the cost of the alloy material and mitigating the harsh processing conditions of PETG. Simultaneously, the addition of epoxy compounds in conjunction with the compatibilizer shortens the molding time and improves the mechanical properties of the alloy material. This PBT-PETG alloy material possesses advantages such as high transparency, good chemical resistance, ease of molding, short molding time, uniform polymer structure, and good compatibility, making it highly valuable for applications. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0023] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0024] Although mature alloy systems such as PC / ABS and PA / PP have been developed, phase separation still occurs in polymer alloy materials due to performance differences between different polymers. PBT and PETG each have their own advantages, but PBT is a crystalline polyester and PETG is an amorphous polyester. This blend of crystalline and amorphous polyesters is more prone to phase separation due to performance differences. In addition, transesterification can change the original properties of the material, making the development of alloy materials with both high transparency and excellent mechanical properties a technical challenge. Therefore, the inventors propose the following solution.
[0025] In a first aspect, the present invention provides a PBT-PETG alloy material, comprising, by weight:
[0026] 20-35 parts of polybutylene terephthalate (PBT);
[0027] 63-78 parts of polyethylene terephthalate-1,4-cyclohexanedimethyl ester (PETG);
[0028] 0-1 part of epoxy compound;
[0029] Antioxidant 0.1–0.5 parts;
[0030] Release agent 0.1-0.5 parts;
[0031] Compatibilizer 0-2 parts;
[0032] Transesterification inhibitor 0.1 to 0.5 parts.
[0033] Preferably, the PBT-PETG alloy material comprises, by weight, the following:
[0034] 20-35 parts of polybutylene terephthalate (PBT);
[0035] 63-78 parts of polyethylene terephthalate-1,4-cyclohexanedimethyl ester (PETG);
[0036] 0.05 to 1 part of epoxy compound;
[0037] Antioxidant 0.1–0.5 parts;
[0038] Release agent 0.1-0.5 parts;
[0039] Compatibilizer 1-2 parts;
[0040] Transesterification inhibitor 0.1 to 0.5 parts.
[0041] By selecting the appropriate formulation for the PBT-PETG alloy material, compatibilizers and transesterification inhibitors can significantly improve the compatibility of PBT and PETG while maintaining the original chemical resistance of both polymers. Furthermore, controlling the ratio of PBT resin to PETG resin is crucial for maintaining the high transparency of this alloy material. As the PBT resin content increases, the PETG resin content decreases, further reducing the cost of the alloy material and mitigating the harsh processing conditions of PETG. Simultaneously, the addition of epoxy compounds in conjunction with the compatibilizer can shorten the molding time and improve the mechanical properties of the alloy material. This PBT-PETG alloy material exhibits advantages such as high transparency, good chemical resistance, ease of molding, short molding time, uniform polymer structure, and good compatibility, making it highly valuable for applications.
[0042] In an optional embodiment, the mass ratio of polybutylene terephthalate (PET) to polyethylene terephthalate-1,4-cyclohexanediol ester is 1 to 2:4, preferably 1 to 1.7:4. To optimize the high transparency of the PBT-PETG alloy material, controlling the mass ratio of PBT and PETG within the range of 1 to 2:4, while ensuring the above-mentioned weight proportions, is beneficial for improving the light transmittance of the PBT-PETG alloy material.
[0043] For example, the mass ratio of PBT to PETG can be any value or a range of any two values from 1:4, 1.2:4, 1.4:4, 1.6:4, 1.8:4, or 2:4.
[0044] Preferably, the melting point of polybutylene terephthalate (PBT) is 180–220°C, more preferably 200–220°C, and the melt index at 230°C and 2.16 kg load is 10–30 g / 10 min.
[0045] Preferably, the polyethylene terephthalate-1,4-cyclohexanediethanol ester (PETG) has a melting point of 160–180°C and a melt index of 10–30 g / 10 min at 230°C and a load of 2.16 kg.
[0046] By controlling the melting point and melt flow index of PBT and PETG within the above range, it is beneficial to improve the compatibility of PBT and PETG with the help of additives, and at the same time, it is beneficial to improve the transparency and chemical resistance of PBT-PETG alloy materials.
[0047] Preferably, the content of 1,4-cyclohexanediethanol ester in PETG is 40–60 mol%.
[0048] In an optional embodiment, the epoxy compound includes at least one of epoxidized soybean oil, epoxidized linseed oil, epoxy resin, epoxidized tetrahydrophthalic acid ester, epoxidized fatty acid octyl ester, epoxidized fatty acid butyl ester, and epoxidized fatty acid methyl ester; preferably, the epoxy compound is epoxidized linseed oil.
[0049] PBT and PETG materials are prone to thermal degradation and hydrolysis during extrusion, which leads to molecular chain breakage and the generation of a large number of reactive terminal carboxyl groups. By adding epoxy compounds, the epoxy groups can react efficiently with these terminal carboxyl groups to form new ester bonds, thereby stabilizing the molecular structure of PRT-PETG alloy materials.
[0050] In an optional embodiment, the compatibilizer includes at least one of styrene-acrylonitrile-maleic anhydride terpolymer, methyl methacrylate-butadiene-styrene copolymer, ethylene-methyl acrylate-glycidyl methacrylate terpolymer, butadiene-styrene copolymer, styrene-butadiene-styrene block copolymer, and ethylene-butyl acrylate-glycidyl methacrylate copolymer.
[0051] Preferably, the compatibilizer is a styrene-acrylonitrile-maleic anhydride terpolymer and / or an ethylene-methyl acrylate-glycidyl methacrylate terpolymer. Maleic anhydride (MAH) and glycidyl methacrylate (GMA), as reactive toughening agents, can improve interfacial properties and react chemically with the functional groups of PBT and other components in the alloy, significantly improving the phase state and interfacial bonding of originally incompatible or poorly compatible blend systems, thereby comprehensively enhancing the overall performance of PRT-PETG alloy materials.
[0052] In an optional embodiment, the transesterification inhibitor includes at least one of triphenyl phosphate, triphenyl phosphite, sodium dihydrogen phosphate, zinc dihydrogen phosphate, sodium pyrophosphate, sodium metaphosphate, ethyl orthosilicate, and triethyl phosphite; preferably, the transesterification inhibitor is sodium dihydrogen phosphate.
[0053] During the contact process between PBT and PETG, the hydroxyl and carboxyl groups at the molecular ends of both molecules will react with the ester bonds of the other, causing molecular chain breakage and forming PBT-PETG random copolymer. This disrupts the original phase separation structure, and the interface between the two gradually disappears. Ester exchange inhibitors can effectively control the degree of reaction between the two, reduce the formation of PBT-PETG random copolymer, and improve the stability of PBT-PETG alloy materials.
[0054] In optional embodiments, the antioxidant includes at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris[2,4-di-tert-butylphenyl] phosphite, oxaloyl(diimino-2,1-ethylidene)propionate (3,5-di-tert-butyl-4-hydroxyphenyl)propionate, bis(2,4-dicumylphenyl) pentaerythritol diphosphite, bis(2,4-diisodecylphenyl) pentaerythritol diphosphite, and bisoctadecyl pentaerythritol diphosphite.
[0055] Preferably, the antioxidant is octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and / or pentaerythritol diphosphite (2,4-diisodecylphenyl)phosphite.
[0056] In optional embodiments, the release agent includes at least one of calcium stearate, polyethylene wax, paraffin wax, vinyl bis-stearamide, pentaerythritol stearate, palm wax, polydimethylsiloxane, and montan wax; preferably, the release agent is pentaerythritol stearate.
[0057] In a second aspect, the present invention provides a method for preparing a PBT-PETG alloy material as described in any of the foregoing embodiments, comprising mixing polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanediol ester, an epoxy compound, an antioxidant, a release agent, a compatibilizer, and an ester exchange inhibitor, followed by extrusion granulation.
[0058] Specifically, the preparation method of PBT-PETG alloy material includes: high-speed premixing of polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanediol ester, epoxy compound, antioxidant, release agent, compatibilizer and transesterification inhibitor, followed by extrusion, cooling, granulation, drying and injection molding of the premix.
[0059] Preferably, the extrusion is performed using a twin-screw extruder, which has 11 temperature zones from the feed section to the discharge section. The temperatures of the 11 temperature zones along the direction from the feed section to the discharge section are as follows: 100-120℃, 220-230℃, 230-240℃, 230-240℃, 225-235℃, 225-235℃, 225-235℃, 225-235℃, 225-235℃, and 230-240℃.
[0060] Preferably, the twin-screw extruder rotates at a speed of 200–300 rpm.
[0061] By controlling the temperature and speed of the twin-screw extruder, the premix can be fully melted and mixed evenly in the twin-screw extruder, resulting in high material uniformity. The obtained PBT-PETG alloy material has high transparency, uniform mechanical properties, and good chemical resistance.
[0062] Thirdly, the present invention provides the application of a PBT-PETG alloy material as described in any of the foregoing embodiments or a PBT-PETG alloy material prepared by the preparation method described in the foregoing embodiments in mechanical structures, packaging materials or medical devices.
[0063] Examples and Comparative Examples
[0064] The following examples and comparative examples all provide a PBT-PETG alloy material, including polybutylene terephthalate (PBT), polyethylene terephthalate-1,4-cyclohexanedimethyl ester (PETG), epoxy compound, antioxidant, release agent, compatibilizer and transesterification inhibitor. The proportions of each raw material are shown in Table 1. In Table 1, S refers to the example and D refers to the comparative example.
[0065] Among them, polybutylene terephthalate (PBT) was purchased from Jiangsu Changchun Chemical Co., Ltd., model number 1100-211M.
[0066] The polyethylene terephthalate-1,4-cyclohexanediethanol ester (PETG) was purchased from SK Group in South Korea, model number K2012.
[0067] Antioxidant 1076 was purchased from Tianjin Lianlong New Materials Co., Ltd.
[0068] Antioxidant 608 was purchased from Tianjin Lianlong New Materials Co., Ltd.
[0069] Pentaerythritol stearate (PETS) was purchased from Lonza Corporation, USA.
[0070] The styrene-acrylonitrile-maleic anhydride terpolymer was purchased from Jiaxing Huawen Chemical Co., Ltd., model SMA-800, containing 6-10% maleic anhydride.
[0071] The ethylene-methyl acrylate-glycidyl methacrylate terpolymer was purchased from SK Group in South Korea, model number LOTADER AX8900.
[0072] The epoxidized linseed oil was purchased from Adico (China) Investment Co., Ltd., model number O-108A.
[0073] Sodium dihydrogen phosphate was purchased from Sinopharm Chemical Reagent Co., Ltd., and its purity was analytical grade.
[0074] Table 1. Formulation of PBT-PETG alloy material (unit: parts by weight)
[0075]
[0076]
[0077] The preparation method of the PBT-PETG alloy material provided in the above embodiments and comparative examples is as follows: polybutylene terephthalate, polyethylene terephthalate-1,4-cyclohexanedimethyl ester, epoxy compound, antioxidant, release agent, compatibilizer and transesterification inhibitor are premixed at high speed, and then the premix is extruded, cooled, granulated, dried and injection molded.
[0078] The extrusion is performed using a twin-screw extruder with a rotation speed of 240 rpm. The twin-screw extruder has 11 temperature zones from the feed section to the discharge section, and the temperatures of the 11 temperature zones along the direction from the feed section to the discharge section are as follows: 100~120℃, 220~230℃, 230~240℃, 230~240℃, 225~235℃, 225~235℃, 225~235℃, 225~235℃, 225~235℃, and 230~240℃.
[0079] Experimental Example 1
[0080] The PBT-PETG alloy materials provided in Examples 1-6 and Comparative Examples 1-14 were tested, and the results are shown in Table 2.
[0081] Transmittance was tested using the ASTM D1003 method.
[0082] Haze was measured using the ASTM D1003 method.
[0083] Notched impact strength was tested using the ISO 180 method.
[0084] The molding time starts from when the injection molding machine closes the mold and ends when the injection molding machine opens the mold and the sample is ejected.
[0085] The chemical resistance test method is as follows: immerse the PBT-PETG alloy material in glacial acetic acid for 30 seconds and observe whether there are any changes in the appearance of the PBT-PETG alloy material.
[0086] Table 2 Properties of PBT-PETG Alloy Materials
[0087]
[0088]
[0089] As shown in Table 2, the PBT-PETG alloy material provided in this embodiment of the invention has high light transmittance and low haze, indicating that the alloy material has excellent light transmittance and can be applied to application scenarios requiring material transparency. Furthermore, the PBT-PETG alloy material has high notched impact strength, short molding time, and no change in appearance after chemical resistance testing, indicating that the alloy material has good mechanical properties, good chemical resistance, and high production efficiency.
[0090] Comparative Example 1, with a PBT matrix, exhibited poor light transmittance and low notched impact strength. Comparative Example 2, with a PETG matrix, while possessing good light transmittance, suffered from long molding time and low production efficiency. Comparative Example 3, with increased compatibilizer and no epoxy compound, showed a slight decrease in light transmittance and increased haze, resulting in poor transparency of the PBT-PETG alloy material. Comparative Example 4, with increased PBT content and no compatibilizer or epoxy compound, showed a significantly lower transparency compared to the previous examples. Comparative Example 5, with increased compatibilizer and no epoxy compound, showed a slight decrease in light transmittance and increased haze, resulting in poor transparency of the PBT-PETG alloy material and poor chemical resistance.
[0091] Comparative Example 6 increased the amount of epoxy compound added but did not add a compatibilizer. The resulting PBT-PETG alloy material showed slight cracking and poor chemical resistance after immersion in glacial acetic acid. Comparative Examples 7 and 8, without the addition of sodium dihydrogen phosphate, both resulted in slight changes in the transparency of the PBT-PETG alloy material, reduced notched impact strength, and a significant decrease in chemical resistance.
[0092] Comparative Example 9, with the addition of 0.05% sodium dihydrogen phosphate, did not effectively control the transesterification reaction during extrusion, resulting in a yellowish PBT-PETG alloy material with poor chemical resistance. Comparative Example 10, with the addition of 0.5% sodium dihydrogen phosphate, did not exhibit any transesterification reaction during extrusion, but the alloy material showed poor compatibility and decreased transparency, and was prone to material inclusions during injection molding (excessive sodium dihydrogen phosphate can cause some degradation of the resin during extrusion).
[0093] In Comparative Examples 11 and 12, the contents of PBT and PETG were adjusted. When the PBT content was equal to or greater than 40%, the PBT-PETG alloy material was almost opaque to the naked eye, and the higher the PBT content, the worse the transparency of the alloy material. In Comparative Examples 13 and 14, the PBT content was 10% and 20%, respectively. The molding time of the PBT-PETG alloy material was longer than that of the examples, resulting in a decrease in production efficiency.
[0094] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A PBT-PETG alloy material, characterized in that, By weight, it includes: 20-35 parts of polybutylene terephthalate; 63-78 parts of polyethylene terephthalate-1,4-cyclohexanediol ester; 0.05 to 1 part of epoxy compound; Antioxidant 0.1~0.5 parts; Release agent 0.1~0.5 parts; Compatibilizer 1-2 parts; Transesterification inhibitor, 0.1-0.5 parts; The epoxy compound includes at least one of epoxidized soybean oil, epoxidized linseed oil, epoxy resin, epoxidized tetrahydrophthalic acid ester, epoxidized fatty acid octyl ester, epoxidized fatty acid butyl ester, and epoxidized fatty acid methyl ester.
2. The PBT-PETG alloy material according to claim 1, characterized in that, The mass ratio of the polybutylene terephthalate to the polyethylene terephthalate-1,4-cyclohexanediol ester is 1~2:
4.
3. The PBT-PETG alloy material according to claim 1, characterized in that, The polybutylene terephthalate has a melting point of 180~220℃ and a melt index of 10~30g / 10min at 230℃ and 2.16kg load.
4. The PBT-PETG alloy material according to claim 1, characterized in that, The polyethylene terephthalate-1,4-cyclohexanediethanol ester has a melting point of 160~180℃ and a melt index of 10~30g / 10min at 230℃ and 2.16kg load.
5. The PBT-PETG alloy material according to claim 1, characterized in that, The content of 1,4-cyclohexanediethanol ester in polyethylene terephthalate-1,4-cyclohexanediethanol ester is 40~60 mol.
6. The PBT-PETG alloy material according to claim 1, characterized in that, The epoxy compound is epoxidized linseed oil.
7. The PBT-PETG alloy material according to claim 1, characterized in that, The compatibilizer includes at least one of the following: styrene-acrylonitrile-maleic anhydride terpolymer, methyl methacrylate-butadiene-styrene copolymer, ethylene-methyl acrylate-glycidyl methacrylate terpolymer, butadiene-styrene copolymer, and ethylene-butyl acrylate-glycidyl methacrylate copolymer.
8. The PBT-PETG alloy material according to claim 1, characterized in that, The compatibilizer is a styrene-acrylonitrile-maleic anhydride terpolymer and / or an ethylene-methyl acrylate-glycidyl methacrylate terpolymer.
9. The PBT-PETG alloy material according to claim 1, characterized in that, The transesterification inhibitor includes at least one of triphenyl phosphate, triphenyl phosphite, sodium dihydrogen phosphate, zinc dihydrogen phosphate, sodium pyrophosphate, sodium metaphosphate, ethyl orthosilicate, and triethyl phosphite.
10. The PBT-PETG alloy material according to claim 1, characterized in that, The antioxidant comprises at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris[2,4-di-tert-butylphenyl] phosphite, oxaloyl(diimino-2,1-ethylidene)propionate (3,5-di-tert-butyl-4-hydroxyphenyl)propionate, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, bis(2,4-diisodecylphenyl)pentaerythritol diphosphite, and bisoctadecyl pentaerythritol diphosphite.
11. The PBT-PETG alloy material according to claim 1, characterized in that, The antioxidant is octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and / or bis(2,4-diisodecylphenyl)pentaerythritol diphosphite.
12. The PBT-PETG alloy material according to claim 1, characterized in that, The release agent includes at least one of calcium stearate, polyethylene wax, paraffin wax, vinyl bis-stearamide, pentaerythritol stearate, palm wax, polydimethylsiloxane, and montan wax.
13. The PBT-PETG alloy material according to claim 1, characterized in that, The release agent is pentaerythritol stearate.
14. A method for preparing the PBT-PETG alloy material according to any one of claims 1 to 13, characterized in that, The process involves mixing the polybutylene terephthalate, the polyethylene terephthalate-1,4-cyclohexanediethanol ester, the epoxy compound, the antioxidant, the release agent, the compatibilizer, and the transesterification inhibitor, followed by extrusion granulation.
15. The preparation method according to claim 14, characterized in that, The extrusion is performed using a twin-screw extruder, which has 11 temperature zones from the feed section to the discharge section. The temperatures of the 11 temperature zones along the direction from the feed section to the discharge section are as follows: 100~120℃, 220~230℃, 230~240℃, 230~240℃, 225~235℃, 225~235℃, 225~235℃, 225~235℃, 225~235℃, and 230~240℃.
16. The preparation method according to claim 15, characterized in that, The twin-screw extruder operates at a speed of 200-300 rpm.
17. The use of a PBT-PETG alloy material as described in any one of claims 1 to 13 or a PBT-PETG alloy material prepared by the preparation method as described in any one of claims 14 to 16 in mechanical structures, packaging materials or medical devices.
Citation Information
Patent Citations
High-property polyester alloy material and preparation method thereof
CN104861596A
PETG-PC alloy with high light transmittance and high toughness as well as preparation method and application of PETG-PC alloy
CN114539740A
High-impact-resistance transparent chemical-resistant PC / PCTG alloy and preparation method thereof
CN119286206A