Method for secondary lithium extraction and resource utilization of lithium extraction residue
By using copper-based additives and ball milling and water leaching treatment of lithium extraction slag, the problems of high difficulty and poor performance in secondary lithium extraction from lithium extraction slag were solved, achieving efficient lithium extraction and improved concrete performance.
Patent Information
- Application Number
- CN202511011693.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-07-22
AI Technical Summary
In existing technologies, secondary lithium extraction from lithium-extraction slag is difficult, and high-temperature treatment can affect the slag phase and slag shape, which is detrimental to its application performance in concrete.
Copper-based additives such as copper sulfate and copper chloride are mixed with lithium extraction slag and ball-milled, followed by water leaching treatment to obtain lithium liquid and secondary lithium extraction slag, which are then used to prepare high-performance concrete slurry.
The secondary extraction of lithium was achieved under mild conditions, which improved the wear resistance and compressive strength of concrete, making it suitable for resource utilization.
Smart Images

Figure CN120776137B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource utilization, specifically relating to the secondary utilization of lithium extraction slag. Background Technology
[0002] With the rapid rise of the new energy storage industry, represented by lithium batteries, the lithium extraction industry, including lithium carbonate, lithium hydroxide, and lithium chloride, has experienced tremendous growth. However, the corresponding output of lithium slag, a byproduct of industrial smelting, has been increasing year by year. Lithium slag is an industrial solid waste generated during the lithium extraction process. Currently, the main lithium extraction methods are sulfuric acid roasting, limestone roasting, salt roasting, and high-temperature chloroform processes. Typically, producing 1 ton of lithium salt generates 10 to 50 tons of lithium slag, resulting in a total stockpile of tens of millions of tons per year.
[0003] The large volume of lithium extraction slag and its low resource utilization rate lead to its primary reliance on stockpiling. This not only occupies significant land resources but also incurs high costs for the construction and maintenance of stockpiles. The accumulation of lithium slag results in substantial land waste and environmental pollution. Therefore, the rational utilization of lithium slag is a major challenge facing the industry's development and upgrading.
[0004] Existing technologies also provide some methods for utilizing lithium slag. For example, Chinese patent CN116770098A discloses a method for high-temperature lithium extraction from clay-type lithium ore after acid leaching with sulfuric acid and ammonium sulfate. This method mainly involves mixing clay-type lithium ore with sulfuric acid to form a slurry, reacting the filter residue with ammonium sulfate, and then dissolving it at high temperature to obtain a lithium-aluminum leachate. Chinese patent CN116065038A discloses a method for high-temperature lithium extraction from clay-type lithium ore after acid leaching with concentrated sulfuric acid. This method mainly involves reacting lithium-containing materials with concentrated sulfuric acid, followed by high-temperature roasting, and repeating this process to finally obtain a lithium-containing leachate. Chinese patent CN119194106A discloses a method for efficiently extracting lithium carbonate from clay-type lithium ore using selective adsorption. Specifically, this method describes crushing and finely grinding clay-type lithium ore to obtain powdered clay-type lithium ore; roasting the powdered clay-type lithium ore at high temperature to obtain a roasting product; adding a dilute acid solution to the roasting product for leaching and separation to obtain a leachate and high-silica slag, which is used as a raw material for cement production.
[0005] Chinese patent document CN118290058A discloses a method for the resource-based and harmless treatment of lithium slag, comprising the following steps: S1 mixing lithium slag with sulfuric acid-containing materials to obtain a slurry mixture; S2 calcining the slurry mixture at a temperature of 180–750 °C to obtain calcined slag, which is then leached and filtered to obtain leaching residue and leachate; S3 drying the leaching residue, adding alkaline substances, and then ball milling the mixture, which is then used as a cement admixture.
[0006] In summary, secondary lithium extraction of lithium extraction slag is difficult, and most industries rely on high-temperature treatment to achieve a certain degree of secondary lithium extraction. However, this also increases the composition of the slag and may affect its performance in cement mix applications. Summary of the Invention
[0007] To address the difficulty of secondary lithium extraction from existing lithium extraction slag, the primary objective of this invention is to provide a method for secondary lithium extraction from lithium extraction slag, aiming to achieve secondary lithium extraction from lithium extraction slag in a gentle manner and obtain secondary lithium extraction slag that is beneficial to the performance of cementitious mixes.
[0008] The second objective of this invention is to provide a method for secondary lithium extraction and resource utilization of lithium extraction slag, aiming to use the slag after secondary lithium extraction as a raw material for preparing high-performance concrete slurry and / or concrete.
[0009] Lithium extraction slag is the residue left after lithium extraction from lithium ore such as lepidolite. It has a low lithium content, and the lithium is deeply embedded in the slag phase, making secondary lithium extraction extremely difficult. The conventional solution in the industry is high-temperature transformation and relatively harsh leaching conditions. While this achieves good secondary lithium extraction results, it also affects the slag phase and slag shape, hindering its application in concrete and negatively impacting the performance of concrete prepared from resources. To address this problem, this invention, after in-depth research, provides the following improved solution:
[0010] A secondary lithium extraction method for lithium extraction slag involves mixing and ball milling the lithium extraction slag with a copper-based additive, followed by water immersion treatment and solid-liquid separation to obtain lithium liquid and secondary lithium extraction slag.
[0011] The copper-based additives include at least one of copper sulfate, copper chloride, and copper nitrate.
[0012] To address the challenges of gentle secondary lithium extraction from lithium extraction slag and the unsatisfactory performance of secondary lithium extraction slag in concrete applications, this invention innovatively employs copper-based additives for ball milling-assisted modification of the slag. This unexpectedly improves the secondary extraction efficiency of deeply embedded lithium in the slag, enabling good lithium extraction without the need for high-temperature treatments such as calcination. Furthermore, it optimizes the physicochemical properties of the secondary lithium extraction slag, resulting in superior performance in its resource-based applications in concrete. For example, it can improve the wear resistance, flexural strength, and compressive strength of concrete prepared from secondary lithium extraction slag.
[0013] In this invention, the lithium extraction slag can be any slag after lithium extraction, such as the lithium extraction slag after hydrometallurgical and pyrometallurgical lithium extraction. As an optional option, it can be the leaching slag after lithium extraction from lepidolite concentrate by sulfate roasting.
[0014] In this invention, the lithium extraction slag includes at least one phase selected from aluminum phosphate silicate, leucite, and sodalite.
[0015] In this invention, the lithium extraction slag contains 0.2-0.5 wt.% lithium and 20-35 wt.% SiO2. The CaO content is 10~30 wt.%, the Al2O3 content is 8~10 wt.%, and the Fe2O3 content is 0.8~2.7 wt.%.
[0016] Preferably, the copper-based additive is at least one of copper sulfate and copper chloride. Studies have shown that the preferred copper-based additive can be combined with the process to further improve the secondary lithium extraction effect of lithium extraction slag and the concrete utilization performance of the secondary lithium extraction slag.
[0017] In this invention, the copper-based additive accounts for 0.5-3% of the weight of the lithium extraction slag, for example, 0.5-2%, preferably 0.8-1.2%, and more preferably 0.9-1.1%. Research in this invention shows that at this preferred ratio, the modification effect can be further improved, which helps to further enhance lithium leaching and the application performance of subsequent secondary lithium extraction slag in concrete.
[0018] In this invention, the ball mill speed can be, for example, 200-500 rpm, preferably 300-400 rpm. Studies have found that at the preferred ball mill speed, a good secondary lithium extraction effect can be obtained from the lithium extraction slag. In addition, it is beneficial to the physicochemical changes of the secondary lithium extraction slag, improving its utilization performance in concrete.
[0019] The ball-to-material ratio (weight ratio of grinding balls to lithium extraction slag) during ball milling can be 1~10:1; further, it can be 2~5:1; and more preferably, it is 2.5~3.5:1. Studies have found that under the optimized ball-to-material ratio, a good secondary lithium extraction effect can be obtained from the lithium extraction slag. In addition, it is also beneficial to the physicochemical changes of the secondary lithium extraction slag, improving its utilization performance in concrete.
[0020] Preferably, the ball milling time is 1 to 10 minutes, and more preferably 4 to 6 minutes.
[0021] In this invention, the ball milling is a dry ball milling process.
[0022] In this invention, the liquid-to-solid ratio during the water immersion process is 2~10:1 (ml / g), and can be further 2.5~3.5 (ml / g); the process of this invention can achieve effective lithium extraction under a high solid-liquid ratio.
[0023] Preferably, the temperature during the immersion process is 10~40 ℃, and more preferably 15~25 ℃.
[0024] Preferably, the immersion time is 0.5 to 5 hours, and more preferably 1 to 3 hours. Considering efficiency, it can be further 1 to 1.5 hours.
[0025] In this invention, lithium liquid is directly subjected to lithium precipitation treatment, or lithium liquid is enriched and concentrated before lithium precipitation treatment to obtain lithium products.
[0026] In this invention, the lithium deposition and lithium enrichment methods can be conventional.
[0027] For example, as an optional solution, the present invention can pre-use components such as ferrophosphate slag, dolomite or zeolite as adsorbents to adsorb lithium, and then perform acid elution to obtain a lithium concentrate. The lithium concentrate is then subjected to conventional impurity removal followed by lithium precipitation treatment to obtain the lithium product.
[0028] This invention also provides a method for secondary lithium extraction and resource utilization of lithium extraction slag. The secondary lithium extraction method described in this invention is used to process the lithium extraction slag to obtain secondary lithium extraction slag. The secondary lithium extraction slag is used as an additive for the preparation of concrete slurry and / or concrete.
[0029] The research of this invention shows that, in addition to achieving a secondary and gentle extraction of lithium, the secondary lithium extraction process described in this invention can also optimize the physicochemical characteristics of the slag, which helps to meet the resource utilization requirements of concrete and can obtain better concrete performance.
[0030] The application described in this invention involves slurrying secondary lithium extraction slag, cement, and aggregate with water to obtain concrete slurry.
[0031] The application described in this invention involves a water content of 100-200 kg / m³ in the concrete slurry. 3 The cement usage is 200~300 kg / m³. 3 The amount of secondary lithium extraction slag used is 20~100 kg / m³. 3 The amount of aggregate used is 1500~2000 kg / m³ 3 The aggregates include, for example, sand and crushed stone. Preferably, the total amount of cement and secondary lithium extraction slag is 250-350 kg / m³. 3 The proportion of secondary lithium extraction slag in (cement and secondary lithium extraction slag) is 10~30 wt.%, and further 15~25 wt.%.
[0032] Furthermore, the water content in the concrete grout is 160±10 kg / m³. 3 The total amount of cement-secondary lithium extraction slag is 300±20 kg / m³. 3 Sand 750±30 kg / m 3 Crushed stone 1120±50 kg / m 3The content of secondary lithium slag in cement-secondary lithium extraction slag is 15~25 wt.%. Studies have shown that a better secondary lithium slag modification effect can be obtained under the optimized ratio.
[0033] The application described in this invention involves curing concrete slurry to obtain concrete.
[0034] Beneficial effects
[0035] This invention innovatively employs copper-based additives to ball mill-assisted modify lithium extraction slag. This unexpectedly improves the secondary extraction efficiency of deeply embedded lithium in the slag, enabling excellent lithium extraction without the need for high-temperature treatments such as roasting. Furthermore, it optimizes the physicochemical properties of the secondary lithium extraction slag, unexpectedly resulting in superior performance in the resource utilization of concrete. For example, it can improve the wear resistance, flexural strength, and compressive strength of concrete prepared from the secondary lithium extraction slag. Attached Figure Description
[0036] Figure 1 XRD pattern of lithium extraction residue;
[0037] Figure 2 The image shows the XRD pattern of the secondary lithium extraction residue from Example 1.
[0038] Figure 3 The image shows the XRD pattern of the lithium-enriched material from Example 1.
[0039] Figure 4 The image shows the XRD pattern of lithium carbonate prepared in Example 1. Detailed Implementation
[0040] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0041] In the following cases, lithium residue extraction (see XRD) is an optional approach. Figure 1 It mainly contains 20-35% SiO2, 10-30% CaO, 5-30% Al2O3, and about 0.35% lithium, and is produced in a lithium mine in Jiangxi Province. In this invention, the "about" can be, for example, ±0.05%.
[0042] Example 1
[0043] 1. Crushing and screening: Crush the approximately 10 mm lumps of lithium extraction residue into 2 mm pieces using a crusher, and then crush the 2 mm pieces into powder using a disc crusher.
[0044] 2. Ball milling treatment: Weigh 300 g of the above lithium extraction slag, add 3 g of copper sulfate as a ball milling aid, ball-to-material ratio 3:1, rotation speed 350 rpm, ball milling time 5 min, to obtain ball milling mixture A.
[0045] 3. Water immersion treatment: The ball-milled mixture A was subjected to water immersion treatment at a liquid-to-solid ratio of 3:1 (ml / g). After stirring and washing for 1 hour, it was filtered to obtain secondary lithium extraction residue (XRD see...). Figure 2 (and lithium liquid, with a lithium dissolution rate of 98.3%).
[0046] 4. Lithium enrichment: The phosphorus-iron slag (mainly FePO4) after selective lithium extraction from waste lithium iron phosphate cathode material was added to the filtrate for lithium enrichment. The liquid-to-solid ratio was 10:1 (ml / g). The adsorption process was carried out at a temperature of 60–90 °C under alkaline conditions (pH adjusted to 11–12 by adding sodium hydroxide) for 2 h, achieving an adsorption rate of 93.61%. The XRD pattern of the enriched material is shown in the figure. Figure 3 (Iron is an amorphous phase). After enrichment, lithium was extracted by acid leaching with dilute hydrochloric acid (1 M concentration) at a liquid-to-solid ratio of 3:1 (ml / g) for 1 h, with the pH at the leaching endpoint controlled at 2-3, to obtain lithium-rich solution B and iron-containing filter residue.
[0047] 5. Lithium precipitation: Add sodium carbonate as a precipitant to lithium-rich solution B, adjust the pH to 9-10, filter to remove copper-containing residue, continue adding sodium carbonate to adjust the pH to 11-12, evaporate, crystallize, filter, and wash to obtain lithium carbonate with a purity of 99.5%; XRD is shown in [reference needed]. Figure 4 The final overall lithium recovery rate was 86.3%.
[0048] 6. Application of Lithium Slag: The concrete abrasion and compressive strength tests are conducted on a 10 cm × 10 cm × 10 cm sheet, and the flexural strength tests are conducted on a 10 cm × 10 cm × 40 cm sheet. The mix proportion of lithium slag-added concrete is calculated according to JGJ55-2011 "Standard for Mix Proportion Design of Ordinary Concrete". Lithium slag is used to replace cement by an equal mass. After the ingredients are thoroughly mixed and allowed to stand for 24 hours, the formwork is removed. After removal, the concrete is placed in a water tank for curing for 28 days before performance testing. For example, using 160 kg / m³ of water... 3 240 kg / m³ of cement 3 Secondary lithium extraction slag 60 kg / m 3 750 kg / m³ of sand 3 1120 kg / m³ of crushed stone 3 The mixture was stirred to obtain a slurry, which was then cured to obtain concrete with 20% lithium slag doping. The testing procedure was performed according to the "Standard for Test Methods of Mechanical Properties of Ordinary Concrete". The abrasion rate of the concrete with 20% lithium slag doping was measured to be 2.1 kg / m³. 2 The compressive strength per cubic meter is 37.7 MPa, and the flexural strength is 5.6 MPa.
[0049] Example 2
[0050] Compared with Example 1, the only difference is the change in the type of adjuvant, specifically:
[0051] Group A: The ball milling additive was copper chloride, and all other conditions remained unchanged. In step 3, the lithium dissolution rate was 92.84%, and the concrete abrasion rate was 2.5 kg / m³. 2 The compressive strength is 45.8 MPa and the flexural strength is 5.4 MPa.
[0052] Group B: Copper nitrate was used as the additive during ball milling, and all other conditions remained unchanged. In step 3, the lithium dissolution rate was 88.7%, and the abrasion rate of the concrete was 2.2 kg / m³. 2 The compressive strength is 41.8 MPa and the flexural strength is 4.4 MPa.
[0053] Group C: During ball milling, the copper sulfate content was 0.5% of the lithium extraction slag weight. The lithium dissolution rate in step 3 was 86.85%, and the concrete wear was 5.1 kg / m³. 2 The compressive strength is 31.4 MPa and the flexural strength is 4.1 MPa.
[0054] Group D: During ball milling, the copper sulfate content was 3% of the weight of the lithium extraction slag. The lithium dissolution rate in step 3 was 81.44%, and the concrete wear was 2.8 kg / m³. 2 The compressive strength is 39.8 MPa and the flexural strength is 5.9 MPa.
[0055] Group E: The ball milling speed was 500 rpm, and all other conditions remained unchanged. In step 3, the lithium dissolution rate was 91.91%, and the concrete abrasion was 5.1 kg / m³. 2 The compressive strength is 24.2 MPa and the flexural strength is 4.7 MPa.
[0056] Example 3
[0057] Compared with Example 1, the only difference is that the single-factor conditions in Table 1 are changed. The operation and parameters are the same as in Example 1. The results are shown in Table 1:
[0058]
[0059] Example 4
[0060] Compared to Example 1, the only difference is that the proportion of cement and secondary lithium extraction slag in the concrete is changed (the total amount of cement and secondary lithium extraction slag is 300 kg / m³). 3 The secondary lithium extraction slag concentrations were 0, 30, and 60 kg / m³, respectively. 3 The corresponding cement strengths are 300, 270, and 240 kg / m³. 3The lithium slag represented by the lithium slag doping ratios of 0%, 10%, and 20% was tested, and its wear rate was measured to be 6 kg / m. 2 4.1 kg / m 2 2.1 kg / m 2 The compressive strength per cubic meter is 24.6 kg / m³. 2 29.9 kg / m 2 37.7 MPa, flexural strength per cubic meter is 4.1 kg / m³ 2 4.7 kg / m 2 5.6 MPa.
[0061] Example 5
[0062] Compared with Example 1, the only difference is that in step 4, dolomite or zeolite is used instead of ferrophosphate slag to be added to the ball mill leachate for lithium enrichment. The lithium adsorption rate is 91.47% and 83.9%, respectively. The lithium-rich slag after adsorption or chemical precipitation is leached with dilute hydrochloric acid (concentration of 1~2 M) at 50-80 ℃, the liquid-solid ratio is 10~40 mL / g, the reaction time is 1~3 h, and a precipitant is added to the lithium-rich solution. The final lithium recovery rate is 81.5%~84.82%.
[0063] Comparative Example 1
[0064] Compared to Example 1, the only difference was that no additives were added during ball milling; all other operations and parameters were the same as in Example 1. The results showed that the lithium dissolution rate in step 3 was 80.77%. The measured concrete abrasion was 5.5 kg / m³. 2 The compressive strength per cubic meter is 22.3 MPa, and the flexural strength per cubic meter is 3.9 MPa.
[0065] Comparative Example 2
[0066] Compared with Example 1, the only difference is that in step 2, the same amount of the following components are used as adjuvants, while other operations and parameters are the same as in Example 1.
[0067] Group A: Ferric chloride was used to replace copper sulfate as an auxiliary agent;
[0068] Group B: Calcium chloride was used to replace copper sulfate as an auxiliary agent;
[0069] The results are as follows:
[0070] Group A: In step 3, the lithium dissolution rate was 82.31%, and the concrete abrasion amount was 4.5 kg / m³. 2 The compressive strength per cubic meter is 28.3 MPa, and the flexural strength per cubic meter is 5.4 MPa.
[0071] Group B: In step 3, the lithium dissolution rate was 77.31%, and the mechanical property test of the concrete showed an abrasion rate of 5.2 kg / m³. 2 The compressive strength per cubic meter is 33.7 MPa, and the flexural strength per cubic meter is 3.9 MPa.
[0072] It is evident that its extraction effect and the concrete performance of the secondary lithium extraction slag are inferior to those of the present invention.
[0073] Comparative Example 3
[0074] Compared to Example 1, the only difference is that the copper sulfate and lithium extraction residue were not pre-milled using a dry ball mill. Instead, the copper sulfate was directly dissolved in water, followed by the addition of the lithium extraction residue (the amount of copper sulfate was the same as in Example 1, and the liquid-to-solid ratio of the copper sulfate solution to the lithium extraction residue was 3 ml / g). The mixture was pre-milled for 5 minutes, followed by leaching for 1 hour. All other operations and parameters were the same as in Example 1. In step 3, the lithium dissolution rate was 91.79%, and the mechanical property test of the concrete showed an abrasion rate of 7.2 kg / m³. 2 The compressive strength per cubic meter is 23.5 MPa, and the flexural strength per cubic meter is 2.1 MPa.
[0075] It is evident that the extraction effect and concrete performance of pre-ball milling with additives followed by leaching are inferior to the improved lithium leaching and concrete application performance of the secondary lithium extraction slag of the present invention.
Claims
1. A method for secondary lithium extraction from lithium extraction slag, characterized in that, The lithium extraction residue and copper-based additives were mixed and ball-milled, followed by water immersion treatment and solid-liquid separation to obtain lithium liquid and secondary lithium extraction residue. The copper-based additives include at least one of copper sulfate, copper chloride, and copper nitrate; The lithium extraction residue is the leaching residue from lithium mica concentrate after sulfate roasting for lithium extraction. The copper-based additive is 0.5-3% of the weight of the lithium extraction slag.
2. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The lithium extraction residue includes at least one phase selected from aluminum phosphate silicate, leucite, and sodalite.
3. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The lithium extraction slag contains 0.2-0.5 wt.% lithium, 20-35 wt.% SiO2, 10-30 wt.% CaO, 8-10 wt.% Al2O3, and 0.8-2.7 wt.% Fe2O3.
4. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The copper-based additive is 0.8 to 1.2% of the weight of the lithium extraction slag.
5. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The copper-based additive is 0.9 to 1.1% of the weight of the lithium extraction slag.
6. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The ball mill speed is 200~500 rpm.
7. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The ball milling time is 1 to 10 minutes.
8. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The liquid-to-solid ratio during the water immersion process is 2~10:
1.
9. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, The temperature during the immersion process is 10~40℃.
10. The secondary lithium extraction method from lithium extraction slag as described in claim 1, characterized in that, Immersion time is 0.5 to 5 hours.
11. The secondary lithium extraction method from lithium extraction slag as described in any one of claims 1 to 10, characterized in that, Lithium products are obtained by directly precipitating lithium liquid or by precipitating lithium salt after concentration.
12. A method for secondary lithium extraction and resource utilization from lithium extraction slag, characterized in that, The lithium extraction slag is processed using the secondary lithium extraction method according to any one of claims 1 to 11 to obtain secondary lithium extraction slag; the secondary lithium extraction slag is used as an additive for the preparation of concrete slurry and / or concrete.
13. The method for secondary lithium extraction from lithium extraction slag and resource utilization for concrete preparation as described in claim 12, characterized in that, The secondary lithium extraction slag, cement, and aggregate are slurried with water to produce concrete slurry.
14. The method for secondary lithium extraction from lithium extraction slag and resource utilization for concrete preparation as described in claim 13, characterized in that, In concrete grout, water content is 100~200 kg / m³ 3 The cement usage is 200~300 kg / m³. 3 The amount of secondary lithium extraction slag used is 20~100kg / m³. 3 The amount of aggregate used is 1500~2000 kg / m³ 3 .
15. The method for secondary lithium extraction from lithium extraction slag and resource utilization for concrete preparation as described in claim 13 or 14, characterized in that, Concrete is obtained by curing concrete slurry.
Citation Information
Patent Citations
Lithium extraction method of lithium-containing material
CN116065038A
Method for extracting lithium from clay type lithium ore
CN116770098A
Recycling and innocent treatment method for lithium slag
CN118290058A
Method for efficiently extracting lithium carbonate from clay type lithium ore by selective adsorption method
CN119194106A
Method for treating lithium-containing minerals through mineral element phase transfer
CN110117020A