Optical fiber with both scattering enhancement and low loss characteristics and method of manufacture
By designing the materials and structures of the fiber core, cladding, and coating in optical fibers, a synergy between low loss and strong scattering in the 1550nm band was achieved, solving the compatibility problem between optical communication and sensing, and enabling the same optical fiber to be compatible with long-distance communication and high-sensitivity sensing.
Patent Information
- Application Number
- CN202511291259.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-10
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2045-09-10
AI Technical Summary
Existing optical fibers cannot simultaneously achieve low loss and strong scattering in optical communication and fiber optic sensing, which requires the separate deployment of optical fibers, increasing system complexity and cost, and making it difficult to achieve efficient integration of sensing and communication data.
The structure consists of a core, cladding, and low-loss UV-curable coating arranged from the inside out. The core contains uniformly distributed 20-50nm nanodots, which are doped with erbium and germanium. Combined with fluoride and silicon oxide composite materials and low-refractive-index silicon fluoride glass, the structure achieves synergistic effects of enhanced scattering and low loss by precisely controlling the refractive index distribution and material composition.
The loss was reduced to 0.14 dB/km in the 1550 nm band, and the Rayleigh scattering intensity was increased by about 30%. This enabled the same optical fiber to meet the requirements of long-distance communication and high-sensitivity sensing at the same time, and solved the technical bottleneck that low loss and strong scattering could not coexist.
Smart Images

Figure CN120802425B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of optical fiber technology, specifically relating to an optical fiber with both scattering enhancement characteristics and low loss characteristics, and its preparation method. Background Technology
[0002] In practical applications of fiber optic technology, there is a significant conflict between the core performance requirements of optical fibers in the fields of optical communication and fiber optic sensing: In the field of optical communication, especially in the 1550nm band, optical fibers need to achieve a theoretical loss limit of 0.14dB / km to ensure long-distance signal transmission. This requires the optical fiber material to be pure and the structure to be uniform, so as to minimize signal attenuation caused by scattering. In the field of fiber optic sensing, sensitivity is enhanced by relying on strong scattering characteristics (such as Rayleigh scattering). Existing technologies often enhance scattering by introducing doping or structural defects, but this inevitably leads to a significant increase in transmission loss.
[0003] This technical bottleneck of "low loss and strong scattering being incompatible" means that existing solutions require the deployment of separate optical fibers for communication and sensing, which not only increases system complexity and cost but also makes it difficult to achieve efficient integration of sensing and communication data.
[0004] Based on this, the present invention discloses an optical fiber with both scattering enhancement characteristics and low loss characteristics, and a method for its fabrication. Summary of the Invention
[0005] To address the problems in the prior art, the present invention aims to provide an optical fiber and a method for its fabrication that combine scattering enhancement characteristics with low loss characteristics.
[0006] To achieve the above objectives and technical effects, the technical solution adopted by this invention is as follows: An optical fiber with both scattering enhancement and low loss characteristics includes a core, a cladding, and a low-loss UV-curable coating arranged sequentially from the inside out. The core contains nanodots, which are doped with at least one metal.
[0007] Furthermore, the fiber core includes a central region and an outer edge region arranged sequentially from the inside to the outside, and the refractive index of the outer edge region is 0.1%-0.2% lower than that of the central region.
[0008] Furthermore, the diameter of the fiber core is 8.2 μm, the radius of the central region is 0-2 μm, and the radius of the outer edge region is 2-4.1 μm.
[0009] Furthermore, the core is uniformly distributed with nanodots of size 20-50nm.
[0010] Furthermore, the nanodots are doped with erbium and germanium, with an erbium doping concentration of 50-80 ppm and a germanium doping concentration of 20,000-30,000 ppm.
[0011] Furthermore, the fiber core is made of a composite material of fluoride and silicon oxide, with a molar ratio of fluoride to silicon oxide of 0.8%-1.5%.
[0012] Furthermore, the cladding is made of low-refractive-index silicon fluoride glass, and the fluorine doping concentration in the cladding is 3%-5%.
[0013] Furthermore, the refractive index of the cladding is 0.3%-0.5% lower than that of the fiber core.
[0014] Furthermore, the thickness of the low-loss UV-curable coating is 25-30 μm.
[0015] This invention also discloses a method for fabricating an optical fiber that combines scattering enhancement characteristics and low loss characteristics, comprising the following steps: 1) Precast bar manufacturing: First, chemical vapor deposition is used to form a composite matrix of fluoride and silicon oxide in the fiber core region by precisely controlling the deposition temperature and gas flow rate. At the same time, erbium and germanium doping is introduced to make nanodots with a size of 20-50nm uniformly distributed inside the fiber core. Subsequently, a cladding layer is formed by depositing a low-refractive-index fluorinated silicon glass material on the outside of the fiber core; 2) Wire drawing: The preform obtained in step 1) is drawn into an optical fiber, and the dimensional accuracy of the core and cladding is strictly controlled. 3) Coating and encapsulation: The optical fiber obtained in step 2) is coated with a low-loss UV-curable coating with a thickness of 25-30 μm, and then encapsulated after UV curing to form the optical fiber with both scattering enhancement and low-loss characteristics.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention discloses an optical fiber and its fabrication method that combine enhanced scattering characteristics with low loss characteristics. It innovatively breaks through the technical bottleneck of the inability of low loss and strong scattering to coexist by synergistic design of core and cladding materials (a core composed of fluoride and silicon oxide, and a cladding of silicon fluoride glass), precise control of nanodots (20-50 nm in size and doped with erbium and germanium), and optimization of refractive index distribution. In the 1550 nm band, it reduces the loss to the theoretical limit of 0.14 dB / km and increases the Rayleigh scattering intensity by about 30%, achieving compatibility between enhanced scattering and low loss for the first time. This solves the problem that a single optical fiber cannot simultaneously meet the requirements of long-distance communication and high-sensitivity sensing, and meets the needs of the fields of optical fiber sensing and long-distance optical communication. Attached Figure Description
[0017] Figure 1 This is a three-dimensional structural diagram of the present invention; Figure 2 This is a cross-sectional view of the present invention; Figure 3 This is a flowchart of the present invention; Figure 4 This is a schematic diagram illustrating the synergistic working principle of scattering and low loss in this invention. Figure 5 This is a graph showing the relationship between the nanodot size and optical fiber performance of the present invention; Figure 6 This is a graph showing the relationship between fluorine doping concentration and cladding performance in this invention. Detailed Implementation
[0018] The present invention will now be described in detail so that its advantages and features can be more easily understood by those skilled in the art, thereby providing a clearer and more explicit definition of the scope of protection of the present invention.
[0019] The following provides a brief overview of one or more aspects to offer a basic understanding of them. This overview is not an exhaustive summary of all conceived aspects, nor is it intended to identify key or decisive elements of all aspects, nor to define the scope of any or all aspects. Its sole purpose is to present some concepts of one or more aspects in a simplified form to prepare for the more detailed descriptions that follow.
[0020] like Figure 1-6 As shown, the present invention discloses an optical fiber with both scattering enhancement characteristics and low loss characteristics, comprising a fiber core 1, a cladding 2 and a low-loss UV-curable coating 3 arranged sequentially from the inside to the outside. The fiber core 1 has uniformly distributed nanodots with a size of 20-50nm that have high scattering enhancement, and the nanodots are doped with at least one metal.
[0021] In some embodiments, the fiber core 1 is made of a composite material doped with fluoride and silicon oxide. Specifically, the composite material refers to a glassy composite material formed by fluoride and silicon oxide, wherein the fluoride is selected from MgF2 or CaF2 and mixed with SiO2 at a molar ratio of 0.8%-1.5% to form a stable network structure. This composite material has both high light transmittance (transmittance ≥99.9% in the 1550nm band) and mechanical stability (Young's modulus ≥70GPa).
[0022] In some embodiments, the nanodots are doped with erbium and germanium, with erbium (Er) doping concentration of 50-80 ppm and germanium (Ge) doping concentration of 20,000-30,000 ppm, to enhance the Rayleigh scattering signal at a wavelength of 1550 nm.
[0023] Erbium doping exhibits strong absorption-radiation characteristics in the 1550nm band, which can enhance the Rayleigh scattering cross section, while germanium doping further enhances the scattering effect by adjusting the refractive index gradient.
[0024] In some embodiments, the fiber core 1 includes a central region 1-1 and an outer edge region 1-2 arranged sequentially from the inside out. The diameter of the fiber core 1 is 8.2 μm, the radius of the central region 1-1 is 0-2 μm, and the radius of the outer edge region 1-2 is 2-4.1 μm. The fiber core 1 adopts a step refractive index design, retains high scattering characteristics in the central region, and has a high nanodot density (10). 15 pcs / cm 3 The refractive index is 1.468, serving as the main scattering center. The refractive index of the outer edge region 1-2 is 0.1%-0.2% lower than that of the central region 1-1, resulting in a 30% reduction in nanodot density and reducing the scattering loss of light signals at the edge.
[0025] In some embodiments, the cladding 2 is made of low-refractive-index silicon fluoride glass, and the fluorine doping concentration in the cladding is 3%-5%. The fluorine doping reduces infrared absorption (absorption loss ≤0.02dB / km in the 1550nm band) and improves chemical stability (salt spray corrosion resistance ≥1000h). The refractive index of the cladding 2 is 0.3%-0.5% lower than that of the fiber core 1, ensuring that the optical signal is effectively confined and transmitted in the fiber core 1.
[0026] In some embodiments, the thickness of the low-loss UV-curable coating 3 is 25-30 μm, and a low-loss UV-curable acrylate coating is used, cured under 365 nm UV light with a power of 500-600 mW / cm². 2 After curing, a uniform and dense protective layer is formed.
[0027] The low-loss UV-curable coating 3 has a refractive index of 1.52, which matches that of the cladding 2 to reduce interface reflection. It has a Young's modulus ≥1.2 GPa, a tensile strength ≥80 MPa, and can withstand a strain of ±0.5% without cracking.
[0028] The optical fiber disclosed in this invention has both scattering enhancement and low loss characteristics, with an optical loss of less than or equal to 0.14 dB / km in the 1550 nm band.
[0029] like Figure 3 As shown, this invention also discloses a method for fabricating an optical fiber that combines scattering enhancement characteristics and low loss characteristics, comprising the following steps: 1) Precast bar manufacturing: First, chemical vapor deposition is used. By precisely controlling the deposition temperature and gas flow rate, the deposition temperature is controlled at 1300-1400℃ to form a composite matrix of fluoride and silicon oxide in the fiber core region. At the same time, erbium and germanium doping is introduced to make nanodots with a size of 20-50nm uniformly distributed inside the fiber core. These nanodots serve as Rayleigh scattering centers, laying the foundation for subsequent scattering enhancement properties. Preparation of central region 1-1: Reaction chamber preparation: Fix the high-purity quartz glass tube into the reaction chamber, which has precise temperature control and rotation functions, to ensure a stable and uniform reaction environment; Gas flow control: SiCl4 (flow rate set at 20-30 sccm) and CF4 (flow rate 0.5-1 sccm) are introduced as basic raw materials, while ErCl3 (flow rate 0.01-0.05 sccm) and GeCl4 (flow rate 0.5-1.5 sccm) are introduced for doping. These gases are thoroughly mixed in the reaction chamber, providing the material basis for subsequent reactions; Deposition temperature control: The reaction chamber temperature is raised to 1300-1400℃. Under this high-temperature environment, raw materials such as SiCl4 and CF4 undergo a chemical reaction to form a composite matrix of fluoride and silicon oxide. Simultaneously, erbium (Er) and germanium (Ge) elements from ErCl3 and GeCl4 are uniformly doped into the matrix, promoting the formation of nanodots with a size controlled at 20-50 nm and a density reaching 102. 15 pcs / cm 3 .
[0030] Central Region 1-1 Formation: As the reaction continues, nanodots are stably distributed in the matrix, forming the central region 1-1. The refractive index of this region is precisely controlled at 1.468, serving as the main scattering center and laying the foundation for the scattering enhancement properties of the optical fiber; Preparation of outer edge region 1-2: Gas flow rate adjustment: Keep the flow rates of SiCl4 and CF4 constant, and finely adjust the flow rates of ErCl3 (flow rate reduced to 0.007-0.035 sccm) and GeCl4 (flow rate reduced to 0.35-1.05 sccm) to reduce the amount of erbium and germanium entering the reaction chamber; Deposition process: Under the same high-temperature environment as the central region, due to the reduction in doping elements, the density of the generated nanodots is reduced by about 30% compared to the central region. The composite matrix formed at this time constitutes the outer edge region 1-2; Refractive index control: By adjusting the proportion of doping elements and reaction conditions, the refractive index of the outer edge region 1-2 is made 0.1%-0.2% lower than that of the central region 1-1. This refractive index difference design effectively reduces the scattering loss of optical signals at the fiber core edge, while ensuring effective confinement and transmission of optical signals within the fiber core. Then, a low-refractive-index fluorinated silicon glass material is deposited on the outside of the fiber core to form cladding 2, in preparation for low-loss characteristics; 2) Wire drawing: The preform obtained in step 1) was drawn into an optical fiber using a high-precision drawing machine at a drawing temperature of 2100-2200℃ and a drawing speed of 800-1000m / min, ultimately forming an optical fiber structure with an outer diameter of 125μm and a core diameter of 8.2μm. During the drawing process, the dimensional accuracy of the core and cladding was strictly controlled, and the step refractive index distribution of the core 1 was preserved. The high scattering enhancement nanodot structure in the central region 1-1 and the low-loss optimized refractive index distribution in the outer region 1-2 remained stable, ensuring the structural basis for scattering enhancement and low-loss characteristics. 3) Coating and encapsulation: The optical fiber obtained in step 2) is coated with a low-loss UV-curable coating 3 with a thickness of 25-30 μm, and then encapsulated after UV curing. The UV wavelength is 365 nm and the power is 500-600 mW / cm². 2 This process forms the optical fiber that combines enhanced scattering characteristics with low loss characteristics. The low-loss UV-cured coating 3 reduces the impact of external environment (such as mechanical friction, humidity, etc.) on the performance of the optical fiber, further ensuring the stability of the optical fiber in complex environments.
[0031] When a 1550nm optical signal is transmitted in the optical fiber, the erbium- and germanium-doped nanodots in the fiber core 1 enhance the Rayleigh scattering intensity (by approximately 30%), meeting the requirements of optical fiber sensing for scattered signals. Simultaneously, the fluorinated silicon glass material in the cladding 2, due to fluorine doping, lowers the infrared absorption band. Combined with the use of ultrapure gas and high-precision processes during fabrication (fiber surface defect density ≤ 10), this enhances the fiber's performance. 15 pcs / mm 2 This reduces the transmission loss in the 1550nm band to the theoretical limit of 0.14dB / km, meeting the low-loss requirements of long-distance optical communication, thus achieving the synergistic effect of scattering enhancement and low-loss characteristics.
[0032] In this invention, nanodots serve as scattering centers, providing sufficient signals for sensing by enhancing Rayleigh scattering. The low nanodot density design at the outer edge of the fiber core, combined with the synergistic effect of fluorine doping in the cladding reducing infrared absorption, achieves low-loss optical signal transmission, with a transmission loss ≤0.14dB / km. This realizes the core advantage of simultaneously satisfying both scattering enhancement (sensing requirements) and low-loss transmission (communication requirements) in a single optical fiber, enabling dual-purpose use of a single fiber, such as... Figure 4 As shown.
[0033] Figure 5 The graph showing the relationship between the nanodot size and optical fiber performance of this invention uses a dual vertical axis design. The horizontal axis represents the nanodot size (nm), the left vertical axis represents the Rayleigh scattering intensity (relative value), and the right vertical axis represents the transmission loss at 1550nm (dB / km). Figure 5 The image clearly shows two key curves: The scattering intensity curve gradually increased from 1.30 to 1.50 as the nanodot size increased from 20 nm to 50 nm, marked "enhancement of 30%-50%", which intuitively demonstrates the promoting effect of size increase on scattering signal; The transmission loss curve increases slowly from 0.14 dB / km to 0.16 dB / km as the nanodot size increases, and the label "always ≤0.16 dB / km" indicates that the loss change is within a controllable range. Nanodot sizes in the 20-50nm range can simultaneously meet the dual requirements of enhanced scattering and low loss, representing the optimal size range for balancing fiber optic sensing sensitivity and communication transmission performance, and providing a key basis for the process control of nanodot sizes.
[0034] Figure 6 The graph shows the relationship between fluorine doping concentration and cladding performance in this invention. The horizontal axis represents the fluorine doping concentration (%), the left vertical axis represents the cladding refractive index, and the right vertical axis represents the infrared absorption loss (dB / km). Figure 6 The curve contains two curves: the blue curve represents the cladding refractive index, and the red curve represents the infrared absorption loss. The blue curve shows that as the fluorine doping concentration gradually increases from 1% to 7%, the cladding refractive index gradually decreases from approximately 1.468 to approximately 1.458, and... Figure 6 The label "Refractive index decreases with increasing fluorine concentration" clearly indicates a negative correlation between fluorine doping concentration and cladding refractive index. The red curve shows that infrared absorption loss decreases with increasing fluorine doping concentration, especially after the fluorine doping concentration reaches 3%, at which point the decreasing trend gradually slows down. Figure 6 The label "stable in the 3%-5% range" indicates that within this concentration range, the infrared absorption loss changes little and tends to stabilize. Meanwhile, Figure 6 The green rectangular area in the figure represents the "preferred concentration of 3%-5%". This is based on a comprehensive consideration of the changing trends of the two curves. Within this concentration range, the cladding refractive index is at a relatively reasonable level, while the infrared absorption loss can also be kept at a low and stable level, which can better meet the requirements of fiber cladding performance. Therefore, it has been determined as the preferred concentration range for fluorine doping.
[0035] Any parts or structures not specifically described in this invention can be made using existing technologies or products, and will not be elaborated upon here.
[0036] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. An optical fiber possessing both scattering enhancement and low-loss characteristics, characterized in that, It includes a fiber core, a cladding and a low-loss UV-curable coating arranged sequentially from the inside to the outside, wherein nanodots are distributed inside the fiber core and at least one metal is doped in the nanodots; The fiber core is uniformly distributed with nanodots of size 20-50nm; The nanodots are doped with erbium and germanium, with an erbium doping concentration of 50-80 ppm and a germanium doping concentration of 20,000-30,000 ppm. The fiber core is made of a composite material of fluoride and silicon oxide, with a molar ratio of fluoride to silicon oxide of 0.8%-1.5%.
2. The optical fiber with both scattering enhancement and low loss characteristics according to claim 1, characterized in that, The fiber core includes a central region and an outer edge region arranged sequentially from the inside to the outside, and the refractive index of the outer edge region is 0.1%-0.2% lower than that of the central region.
3. The optical fiber with both scattering enhancement and low loss characteristics according to claim 2, characterized in that, The diameter of the fiber core is 8.2 μm, the radius of the central region is 0-2 μm, and the radius of the outer edge region is 2-4.1 μm.
4. The optical fiber with both scattering enhancement and low loss characteristics according to claim 1, characterized in that, The cladding is made of low-refractive-index silicon fluoride glass, and the fluorine doping concentration in the cladding is 3%-5%.
5. The optical fiber with both scattering enhancement and low loss characteristics according to claim 1, characterized in that, The refractive index of the cladding is 0.3%-0.5% lower than that of the fiber core.
6. The optical fiber with both scattering enhancement and low loss characteristics according to claim 1, characterized in that, The thickness of the low-loss UV-curable coating is 25-30 μm.
7. A method for fabricating an optical fiber possessing both scattering enhancement and low-loss characteristics as described in any one of claims 1-6, characterized in that, Includes the following steps: 1) Precast bar manufacturing: First, chemical vapor deposition is used to form a composite matrix of fluoride and silicon oxide in the fiber core region by precisely controlling the deposition temperature and gas flow rate. At the same time, erbium and germanium doping is introduced to make nanodots with a size of 20-50nm uniformly distributed inside the fiber core. Subsequently, a cladding layer is formed by depositing a low-refractive-index fluorinated silicon glass material on the outside of the fiber core; 2) Wire drawing: The preform obtained in step 1) is drawn into an optical fiber, and the dimensional accuracy of the core and cladding is strictly controlled. 3) Coating and encapsulation: The optical fiber obtained in step 2) is coated with a low-loss UV-curable coating with a thickness of 25-30 μm, and then encapsulated after UV curing to form the optical fiber with both scattering enhancement and low-loss characteristics.
Citation Information
Patent Citations
Low loss optical fiber designs and methods for their manufacture
CN102411168A
Low-loss large-effective area single mode fiber and manufacturing method thereof
CN103472525A