Modified positive electrode material and preparation method and application thereof

By doping Ti and S into the lithium manganese iron phosphate core and using a fluorine oxide coating layer, the interfacial side reactions, thermal stability, and conductivity issues of LMFP cathode materials were resolved, thereby improving their performance in lithium-ion batteries.

CN120809798BActive Publication Date: 2026-11-20GEM CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511225258.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-08-29
Publication Date
2026-11-20
Estimated Expiration
2045-08-29

AI Technical Summary

Technical Problem

Lithium manganese iron phosphate (LMFP) cathode materials face problems such as interfacial side reactions and HF corrosion, poor thermal stability, low electronic conductivity and slow ion diffusion rate in lithium-ion batteries, which affect their cycle performance and rate performance.

Method used

Ti and S are co-doped in the lithium manganese iron phosphate core to enhance electronic conductivity and lithium-ion channels. Meanwhile, fluorine oxide is used as a coating layer to block electrolyte contact, suppress interfacial side reactions, and improve thermal stability.

Benefits of technology

It improves the rate performance, cycle stability and thermal stability of cathode materials, reduces the risk of side reactions under high temperature conditions, and lays the foundation for its commercial application in the field of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005572472920000131
    Figure BDA0005572472920000131
  • Figure BDA0005572472920000141
    Figure BDA0005572472920000141
Patent Text Reader

Abstract

This invention provides a modified cathode material, its preparation method, and its applications. The modified cathode material comprises a lithium manganese iron phosphate (LFP) core and a coating layer covering the surface of the LFP core, the coating layer being made of fluorine oxide; the LFP core is co-doped with Ti and S. This invention co-dops Ti and S in the LFP core. Ti doping introduces additional electron-hole pairs, enhancing the intrinsic electronic conductivity of the material, while S doping expands the lithium-ion channels and improves the Li-ion conductivity. + The diffusion rate is optimized through a dual pathway of "electron conduction-ion migration," which improves the rate performance and cycle stability of the cathode material. Using fluorine oxide as a coating material can reduce HF corrosion and the dissolution of transition metals, and suppress interfacial side reactions. At the same time, the excellent thermal stability and wide electrochemical window of fluorine oxide can suppress electrolyte decomposition and gas production at high temperatures, thus improving the thermal and electrochemical stability of the modified cathode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery materials technology, specifically relating to a modified cathode material, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries possess outstanding advantages such as high discharge capacity, high voltage platform, safety, long lifespan, and environmental friendliness, and their application in various fields is becoming increasingly widespread. In lithium-ion batteries, the cathode material is the core technology for battery upgrades and replacements; therefore, in-depth research on lithium-ion battery cathode materials has significant practical implications.

[0003] Lithium manganese iron phosphate (LMFP), as an important candidate cathode material for lithium-ion batteries, has shown broad application prospects in power batteries, energy storage batteries, and other fields due to its high theoretical specific capacity, stable charge-discharge platform, excellent structural stability, and low cost, becoming a research hotspot in recent years. However, LMFP still faces the following key technical problems in practical applications, which seriously restrict its commercialization process: 1) Interfacial side reactions and HF corrosion problems. Because the electrolyte is prone to decomposition during charge-discharge (especially under high voltage) to produce acidic substances such as HF, these products will continuously corrode the crystal structure of the LMFP material surface, leading to the degradation of Mn. 2+ Fe 2+ When metal ions dissolve, HF reacts with Li on the surface of the LMFP material. + 1) The formation of LiF not only hinders the transport of electrons and ions but also increases interfacial impedance, leading to rapid capacity decay and deterioration of cycle performance; 2) Poor high-temperature performance: High temperatures accelerate electrolyte decomposition and HF generation, exacerbating interfacial corrosion. The tendency of Mn element dissolution within the LMFP material is enhanced, leading to lattice distortion and structural collapse. In addition, high temperatures can also cause rapid capacity decay and thermal runaway risks, making it difficult to meet the requirements of power batteries under high-temperature conditions; 3) Unstable CEI film: During charge-discharge cycles, the unstable CEI film will repeatedly rupture and regenerate, consuming electrolyte and active lithium, while continuously increasing interfacial impedance, ultimately affecting the cycle life and rate performance of the battery; 4) Low electronic conductivity: Low electronic conductivity prevents rapid charge transport between material particles, especially during high-rate charge-discharge, where polarization is prone to occur inside the electrode, limiting the rate performance of the battery; 5) Slow ion diffusion rate: In the olivine structure of LMFP, Li + The narrow diffusion channels result in a low Li+ diffusion coefficient, and the slow ion diffusion rate makes Li... + The difficulty in rapidly inserting / extracting from the lattice during charging and discharging exacerbates electrode polarization, leading to a decrease in the capacity utilization of the material.

[0004] Therefore, how to effectively suppress interfacial side reactions, reduce HF corrosion and dissolution of transition metals, and improve the thermal stability, electronic conductivity and ion diffusion rate of cathode materials, thereby improving the cycle performance and rate performance of cathode materials, is an urgent technical problem to be solved. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a modified cathode material, its preparation method, and its applications. This invention co-dops Ti and S in the lithium manganese iron phosphate core. Ti doping introduces additional electron-hole pairs, enhancing the intrinsic electronic conductivity of the material, while S doping expands the lithium-ion channels and improves the Li-ion conductivity. + The diffusion rate is optimized through a dual pathway of "electron conduction-ion migration," which improves the rate performance and cycle stability of the cathode material. Using fluorine oxides as a coating material can reduce HF corrosion and the dissolution of transition metals, and suppress interfacial side reactions. At the same time, the excellent thermal stability and wide electrochemical window of fluorine oxides can suppress electrolyte decomposition and gas production at high temperatures, thus improving the thermal and electrochemical stability of the modified cathode material.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a modified cathode material comprising a lithium manganese iron phosphate core and a coating layer covering the surface of the lithium manganese iron phosphate core, wherein the coating layer is made of fluorine oxide; and the lithium manganese iron phosphate core is co-doped with Ti and S.

[0008] In one aspect, this invention co-dops Ti and S in the core of lithium manganese iron phosphate. Ti doping introduces additional electrons and holes, enhancing the intrinsic electronic conductivity of the material and accelerating charge transport between particles, while S doping expands the lithium-ion channels and reduces PO4 content. 3- Tetrahedron to Li + Spatial barriers to migration, enhancing Li + The diffusion rate, through synergistic optimization of the "electron conduction-ion migration" dual pathway, fundamentally improves the rate performance and cycle stability of the cathode material. On the other hand, using fluorine oxide as the coating material can prevent direct contact between the electrolyte and the lithium manganese iron phosphate core, reducing HF corrosion and transition metal dissolution, thereby effectively suppressing interfacial side reactions. Simultaneously, the excellent thermal stability and wide electrochemical window of fluorine oxide can suppress electrolyte decomposition and gas generation at high temperatures, significantly reducing the risk of side reactions under high temperature and high pressure conditions, and improving the thermal and electrochemical stability of the modified cathode material. Therefore, the above modification strategies comprehensively improve the rate performance, cycle life, and thermal stability of the cathode material, laying the foundation for its commercial application in the field of rechargeable batteries.

[0009] Preferably, the fluorine oxide is a metal fluorine oxide.

[0010] Preferably, the metal fluoride oxide comprises AlOF.

[0011] In this invention, due to the crystal structure of AlOF, Al 3+ The ionic radius of lithium manganese iron phosphate is related to the Fe in the lattice. 2+ Mn 2+ The AlOF coating has a similar bond length to the Fe-O and Mn-O bonds in the LMFP core, and this structural similarity allows the AlOF coating to form a coherent or semi-coherent interface with the LMFP core, reducing interfacial stress and defects. This makes the AlOF coating less prone to peeling due to volume changes during charge and discharge, and it can continuously resist electrolyte erosion during long-term cycling. Furthermore, Al… 3+ Empty orbitals can form "ion transport channels," allowing not only Li + Rapid diffusion can also enhance interfacial electronic conduction through the electronic delocalization of Al-O bonds.

[0012] Preferably, the thickness of the coating layer is 5-50 nm, for example, it can be 5 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm.

[0013] In this invention, an appropriate thickness facilitates the formation of a complete and dense protective barrier on the surface of the lithium manganese iron phosphate core. This effectively prevents direct contact between the electrolyte and the core, reducing HF corrosion and transition metal ion dissolution, and suppressing interfacial side reactions. Furthermore, it avoids increased impedance due to prolonged ion / electron transport paths caused by excessive thickness, thus ensuring the integrity of the Li-Fe core. + This allows for efficient migration of electrons between the coating layer and the core; at the same time, the appropriate thickness can match the volume changes of lithium manganese iron phosphate during charging and discharging, reducing the risk of the coating layer cracking due to stress concentration and ensuring the stability of the coating layer during long-term cycling.

[0014] Preferably, a carbon layer is further present between the lithium manganese iron phosphate core and the coating layer.

[0015] Preferably, the thickness of the carbon layer is 1-10 nm, for example, it can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm.

[0016] Preferably, the lithium manganese iron phosphate core has the general chemical formula LiMn. 1-x-y Fe x Ti y PO 4-z S zWhere 0.2≤x≤0.8, for example, it can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8, etc.; 0<y<0.05, for example, it can be 0.01, 0.02, 0.03 or 0.04, etc.; and 0<z<0.02, for example, it can be 0.01, 0.015 or 0.018, etc.

[0017] Preferably, the molar ratio of Ti to S is 1:(0.04-0.4), for example, it can be 1:0.04, 1:0.05, 1:0.1, 1:0.12, 1:0.2, 1:0.25, 1:0.3, 1:0.35 or 1:0.4, etc.

[0018] In this invention, an appropriate doping molar ratio is beneficial to fully leveraging the synergistic effect of the two elements. This not only allows the electronic conductivity to match the ion diffusion rate, avoiding a deterioration in transport performance due to excessive doping of a particular element (e.g., excessive Ti may cause lattice distortion or excessive S may damage the stability of the crystal structure), but also ensures that the doping elements are uniformly distributed in the core, reducing local defects. While improving the rate performance of the material, it maintains the integrity of the lattice structure and reduces the risk of capacity decay due to structural collapse during cycling. Ultimately, this achieves a dual improvement in both the synergistic optimization of electron-ion transport and structural stability.

[0019] Preferably, the particle size D50 of the lithium manganese iron phosphate core is 100-800nm, for example, it can be 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm or 800nm, etc.

[0020] In a second aspect, the present invention provides a method for preparing the modified cathode material as described in the first aspect, the method comprising the following steps:

[0021] Lithium, manganese, iron, phosphorus, sulfur, titanium, and carbon sources are mixed and sintered to obtain sintered products.

[0022] A coating layer is deposited on the surface of the sintered product to obtain the modified cathode material; wherein the material of the coating layer includes fluorine oxide.

[0023] In this invention, the carbon source plays an important role in the sintering process, including reduction effects (such as inducing the reduction of ternary iron to divalent iron), confined growth effects, and suppression of dopant element segregation.

[0024] Preferably, the sulfur source includes ammonium sulfide and / or thiourea.

[0025] Preferably, the titanium source includes titanium dioxide and / or tetrabutyl titanate.

[0026] Preferably, the lithium source includes any one or a combination of at least two of lithium hydroxide monohydrate, lithium carbonate, lithium nitrate, or lithium chloride.

[0027] Preferably, the manganese source includes any one or a combination of at least two of manganese carbonate, manganese acetate, manganese dioxide, manganese tetroxide, or manganese nitrate.

[0028] Preferably, the iron source includes any one or a combination of at least two of ferrous oxalate dihydrate, ferric oxide, ferric oxide, ferrous chloride, or ferrous nitrate.

[0029] Preferably, the phosphorus source includes any one or a combination of at least two of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, or phosphoric acid.

[0030] Preferably, the carbon source includes any one or a combination of at least two of starch, sucrose, glucose, citric acid, phenolic resin, acetylene black, carbon black, or carbon nanotubes.

[0031] Preferably, the sintering process includes pre-firing and main firing performed sequentially.

[0032] This invention employs a stepwise sintering method, which helps to fully decompose the carbon source and construct lithium manganese iron phosphate crystal nuclei.

[0033] Preferably, the preheating temperature is 300-500℃, for example, 300℃, 400℃ or 500℃, and the time is 2-6h, for example, 2h, 3h, 4h, 5h or 6h.

[0034] Preferably, the pre-burning atmosphere is an inert atmosphere. For example, it may be nitrogen or argon.

[0035] Preferably, the temperature of the main firing is 650-800℃, for example, 650℃, 700℃, 750℃ or 800℃, and the time is 5-15h, for example, 5h, 10h or 15h.

[0036] Preferably, the atmosphere for the main combustion is an inert atmosphere. For example, it could be nitrogen or argon.

[0037] Preferably, the deposition method of the coating layer includes co-precipitation or sol-gel method.

[0038] Preferably, the deposition method for the coating layer is a co-precipitation method, and the specific steps include:

[0039] (a) The metal fluorine mixture and the sintering product are mixed to obtain a suspension.

[0040] (b) Adjust the pH of the suspension to carry out a co-precipitation reaction so that the surface of the sintered product is coated with metal hydroxy fluoride, and then perform a calcination treatment to convert the metal hydroxy fluoride into metal fluoride oxide.

[0041] Preferably, in the metal-fluorine mixture in step (a), the total concentration of metal ions and fluorine ions is 300-5000 mg / L, for example, it can be 300 mg / L, 500 mg / L, 1000 mg / L, 2000 mg / L, 3000 mg / L, 4000 mg / L or 5000 mg / L, etc.

[0042] Preferably, the temperature of the coprecipitation reaction in step (b) is 70-90°C, for example, 70°C, 80°C or 90°C, and the time is 1-5h, for example, 1h, 2h, 3h, 4h or 5h.

[0043] Preferably, the calcination temperature in step (b) is 400-600℃, for example, 400℃, 500℃ or 600℃, and the time is 2-6h, for example, 2h, 3h, 4h, 5h or 6h.

[0044] Preferably, the preparation method includes the following steps:

[0045] (1) After mixing lithium source, manganese source, iron source, phosphorus source, sulfur source, titanium source and carbon source, add alcohol solvent and perform wet ball milling. Then, perform pre-calcination for 2-6 hours in an inert atmosphere at 300-500℃ and main calcination for 5-15 hours in an inert atmosphere at 650-800℃. After completion, grind and sieve to obtain sintered products with particle size D50 of 100-800nm ​​(e.g., 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm or 800nm, etc.).

[0046] (2) An aluminum source (exemplary, such as aluminum nitrate, aluminum chloride, aluminum sulfate or aluminum isopropoxide, etc.), a fluorine source (exemplary, such as ammonium fluoride, hydrofluoric acid, ammonium bifluoride or sodium fluoride, etc.) and a solvent are mixed to obtain an aluminum-fluorine mixture; wherein, the total concentration of aluminum ions and fluorine ions in the aluminum-fluorine mixture is 300-5000 mg / L.

[0047] The sintered product is dispersed in the aluminum-fluorine mixture and ultrasonically treated for 20-40 minutes (e.g., 20 minutes, 30 minutes, or 40 minutes) to obtain a suspension.

[0048] The pH of the suspension is adjusted to 2-4 (e.g., 2, 2.5, 3, 3.5, or 4, etc.), and a co-precipitation reaction is carried out at 70-90°C for 1-5 hours to allow the surface of the sintered product to be coated with aluminum hydroxy fluoride precursor. Then, the product is centrifuged, washed, and dried to obtain an intermediate.

[0049] The intermediate is calcined under an inert atmosphere to convert the aluminum hydroxy fluoride precursor into AlOF, thereby obtaining a modified cathode material; wherein the calcination temperature is 400-600℃ and the time is 2-6h.

[0050] Thirdly, the present invention provides an application of the modified cathode material as described in the first aspect in the field of secondary batteries.

[0051] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] In one aspect, this invention co-dops Ti and S in the core of lithium manganese iron phosphate. Ti doping introduces additional electrons and holes, enhancing the intrinsic electronic conductivity of the material and accelerating charge transport between particles, while S doping expands the lithium-ion channels and reduces PO4 content. 3- Tetrahedron to Li + Spatial barriers to migration, enhancing Li + The diffusion rate, through synergistic optimization of the "electron conduction-ion migration" dual pathway, fundamentally improves the rate performance and cycle stability of the cathode material. On the other hand, using fluorine oxide as the coating material can prevent direct contact between the electrolyte and the lithium manganese iron phosphate core, reducing HF corrosion and transition metal dissolution, thereby effectively suppressing interfacial side reactions. Simultaneously, the excellent thermal stability and wide electrochemical window of fluorine oxide can suppress electrolyte decomposition and gas generation at high temperatures, significantly reducing the risk of side reactions under high temperature and high pressure conditions, and improving the thermal and electrochemical stability of the modified cathode material. Therefore, the above modification strategies comprehensively improve the rate performance, cycle life, and thermal stability of the cathode material, laying the foundation for its commercial application in the field of rechargeable batteries. Detailed Implementation

[0054] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0055] Example 1

[0056] This embodiment provides a modified cathode material, which includes a lithium manganese iron phosphate core and a coating layer covering the surface of the lithium manganese iron phosphate core. The coating layer is made of AlOF. The lithium manganese iron phosphate core is co-doped with Ti and S.

[0057] The coating layer has a thickness of 27 nm; a carbon layer with a thickness of 5 nm is also present between the lithium manganese iron phosphate core and the coating layer; the general chemical formula of the lithium manganese iron phosphate core is LiMn. 1-x-y Fe x Ti y PO 4-z S z x = 0.5, y = 0.025, z = 0.0055, the molar ratio of Ti to S doping is 1:0.22; the particle size D50 of the lithium manganese iron phosphate core is 450 nm.

[0058] This embodiment also provides a method for preparing the above-mentioned modified cathode material, the method comprising the following steps:

[0059] (1) Lithium hydroxide monohydrate, manganese carbonate, ferrous oxalate dihydrate, diammonium hydrogen phosphate, ammonium sulfide, titanium dioxide and sucrose were mixed and then ethanol was added. The mixture was wet ball milled and then pre-calcined at 400°C in a nitrogen atmosphere for 4 hours. The main calcination was carried out at 750°C in an inert atmosphere for 10 hours. After the main calcination was completed, the mixture was ground and sieved to obtain a sintered product with a particle size D50 of 450 nm.

[0060] (2) Add aluminum isopropoxide and hydrofluoric acid to deionized water and stir to obtain an aluminum-fluorine mixture; wherein the total concentration of aluminum ions and fluorine ions in the aluminum-fluorine mixture is 2600 mg / L.

[0061] The sintered product was dispersed in the aluminum-fluorine mixture and ultrasonically treated for 30 minutes to obtain a suspension.

[0062] The pH of the suspension was adjusted to 3, and a co-precipitation reaction was carried out at 80°C for 3 hours to allow the surface of the sintered product to be coated with aluminum hydroxy fluoride precursor. Then, the product was centrifuged, washed, and dried to obtain an intermediate.

[0063] The intermediate is calcined under a nitrogen atmosphere to convert the aluminum hydroxy fluoride precursor into AlOF, thereby obtaining a modified cathode material; wherein the calcination treatment is performed at a temperature of 500°C for 4 hours.

[0064] Example 2

[0065] This embodiment provides a modified cathode material, which includes a lithium manganese iron phosphate core and a coating layer covering the surface of the lithium manganese iron phosphate core. The coating layer is made of AlOF. The lithium manganese iron phosphate core is co-doped with Ti and S.

[0066] The coating layer has a thickness of 5 nm; a carbon layer with a thickness of 3 nm is also present between the lithium manganese iron phosphate core and the coating layer; the general chemical formula of the lithium manganese iron phosphate core is LiMn. 1-x-y Fe x Ti y PO 4-z S z x = 0.2, y = 0.03, z = 0.0012, the molar ratio of Ti to S doping is 1:0.04; the particle size D50 of the lithium manganese iron phosphate core is 100 nm.

[0067] This embodiment also provides a method for preparing the above-mentioned modified cathode material, the method comprising the following steps:

[0068] (1) Lithium hydroxide monohydrate, manganese carbonate, ferrous oxalate dihydrate, diammonium hydrogen phosphate, ammonium sulfide, titanium dioxide and sucrose were mixed and then ethanol was added. The mixture was wet ball milled and then pre-calcined at 400°C in a nitrogen atmosphere for 6 hours. The main calcination was carried out at 650°C in a nitrogen atmosphere for 15 hours. After the main calcination was completed, the mixture was ground and sieved to obtain a sintered product with a particle size D50 of 100 nm.

[0069] (2) Add aluminum isopropoxide and hydrofluoric acid to deionized water and stir to obtain an aluminum-fluorine mixture; wherein the total concentration of aluminum ions and fluorine ions in the aluminum-fluorine mixture is 300 mg / L.

[0070] The sintered product was dispersed in the aluminum-fluorine mixture and ultrasonically treated for 20 minutes to obtain a suspension.

[0071] The pH of the suspension was adjusted to 2, and a co-precipitation reaction was carried out at 70°C for 5 hours to allow the surface of the sintered product to be coated with aluminum hydroxy fluoride precursor. Then, the product was centrifuged, washed, and dried to obtain an intermediate.

[0072] The intermediate is calcined under a nitrogen atmosphere to convert the aluminum hydroxy fluoride precursor into AlOF, thereby obtaining a modified cathode material; wherein the calcination treatment is performed at a temperature of 400°C for 6 hours.

[0073] Example 3

[0074] This embodiment provides a modified cathode material, which includes a lithium manganese iron phosphate core and a coating layer covering the surface of the lithium manganese iron phosphate core. The coating layer is made of AlOF. The lithium manganese iron phosphate core is co-doped with Ti and S.

[0075] The coating layer has a thickness of 50 nm; a carbon layer with a thickness of 10 nm is also present between the lithium manganese iron phosphate core and the coating layer; the general chemical formula of the lithium manganese iron phosphate core is LiMn. 1-x-y Fe x Ti y PO 4-z S z x = 0.8, y = 0.02, z = 0.008, the molar ratio of Ti to S doping is 1:0.4; the particle size D50 of the lithium manganese iron phosphate core is 800 nm.

[0076] This embodiment also provides a method for preparing the above-mentioned modified cathode material, the method comprising the following steps:

[0077] (1) Lithium hydroxide monohydrate, manganese carbonate, ferrous oxalate dihydrate, diammonium hydrogen phosphate, ammonium sulfide, titanium dioxide and sucrose were mixed and then ethanol was added. The mixture was wet ball milled and then pre-calcined at 500°C in a nitrogen atmosphere for 2 hours. The main calcination was carried out at 800°C in an argon atmosphere for 5 hours. After the main calcination was completed, the mixture was ground and sieved to obtain a sintered product with a particle size D50 of 800 nm.

[0078] (2) Add aluminum isopropoxide and hydrofluoric acid to deionized water and stir to obtain an aluminum-fluorine mixture; wherein, the total concentration of aluminum ions and fluorine ions in the aluminum-fluorine mixture is 5000 mg / L.

[0079] The sintered product was dispersed in the aluminum-fluorine mixture and ultrasonically treated for 40 minutes to obtain a suspension.

[0080] The pH of the suspension was adjusted to 4, and a co-precipitation reaction was carried out at 90°C for 1 hour to allow the surface of the sintered product to be coated with aluminum hydroxy fluoride precursor. Then, the product was centrifuged, washed, and dried to obtain an intermediate.

[0081] The intermediate is calcined under an argon atmosphere to convert the aluminum hydroxy fluoride precursor into AlOF, thereby obtaining a modified cathode material; wherein the calcination treatment is performed at a temperature of 600°C for 2 hours.

[0082] Example 4

[0083] The difference between this embodiment and embodiment 1 is that the aluminum isopropoxide in step (2) is replaced with ferric nitrate, so that the coating material is FeOF.

[0084] The remaining preparation methods and parameters are consistent with those in Example 1.

[0085] Example 5

[0086] The difference between this embodiment and Embodiment 1 is that the thickness of the coating layer is 2nm.

[0087] The remaining preparation methods and parameters are consistent with those in Example 1.

[0088] Example 6

[0089] The difference between this embodiment and Embodiment 1 is that the thickness of the coating layer is 100 nm.

[0090] The remaining preparation methods and parameters are consistent with those in Example 1.

[0091] Example 7

[0092] The difference between this embodiment and Embodiment 1 is that the molar ratio of Ti to S doping is 1:0.01.

[0093] The remaining preparation methods and parameters are consistent with those in Example 1.

[0094] Example 8

[0095] The difference between this embodiment and Embodiment 1 is that the molar ratio of Ti to S doping is 1:1.

[0096] The remaining preparation methods and parameters are consistent with those in Example 1.

[0097] Example 9

[0098] The difference between this embodiment and embodiment 1 is that pre-burning is not performed in step (1).

[0099] The remaining preparation methods and parameters are consistent with those in Example 1.

[0100] Comparative Example 1

[0101] The difference between this comparative example and Example 1 is that the ammonium sulfide in step (1) is replaced with ammonium chloride, so that Ti and Cl are co-doped in the lithium manganese iron phosphate core.

[0102] The remaining preparation methods and parameters are consistent with those in Example 1.

[0103] Comparative Example 2

[0104] The difference between this comparative example and Example 1 is that the coating layer is an aluminum oxide layer, that is, in step (2), hydrofluoric acid is replaced with an equal mass of aluminum isopropoxide.

[0105] The remaining preparation methods and parameters are consistent with those in Example 1.

[0106] Performance testing

[0107] Lithium-ion batteries were prepared based on the modified cathode materials provided in the above embodiments and comparative examples: The modified cathode materials, conductive carbon black and polyvinylidene fluoride prepared above were weighed in a mass ratio of 8:1:1 and added to N-methylpyrrolidone to make a slurry. The slurry was then coated on aluminum foil, dried, and sliced ​​to obtain a cathode sheet. A lithium metal sheet was used as the counter electrode, a polyethylene microporous membrane was used as the separator, and an electrolyte with a solute concentration of 1 mol / L was prepared (wherein, the solvent is a mixed solution of ethylene carbonate and dimethyl carbonate with a volume ratio of 1:1, and the solute is LiPF6). The batteries were assembled into CR2025 button batteries in an argon glove box.

[0108] Cycle performance and rate performance were tested on the CR2025 button cell.

[0109] Cyclic performance test conditions: After the assembled battery is left to stand for 2 hours, it is subjected to 300 cycles at 25℃, voltage range of 2.5-4.35V, and 2C rate.

[0110] Test conditions for rate performance: After the assembled battery is left to stand for 2 hours, it is subjected to 5 cycles at 0.2C, 0.5C, 1C, 2C and 5C respectively under the conditions of 25℃ and voltage range of 2.5-4.35V.

[0111] Thermal stability test method: The material was immersed in an electrolyte (1 mol / L electrolyte, wherein the solvent is a 1:1 volume ratio mixture of ethylene carbonate and dimethyl carbonate, and the solute is LiPF6) at 80℃ for 24 h. The Mn dissolved in the electrolyte was detected by ICP-MS. 2+ concentration.

[0112] The test results are shown in Table 1.

[0113] Table 1

[0114]

[0115]

[0116] analyze

[0117] As shown in Table 1, this invention co-dops Ti and S in the lithium manganese iron phosphate core. Ti doping introduces additional electrons and holes, enhancing the intrinsic electronic conductivity of the material and accelerating charge transport between particles, while S doping expands the lithium-ion channels and reduces PO4. 3- Tetrahedron to Li + Spatial barriers to migration, enhancing Li +The diffusion rate is optimized through a dual pathway of "electron conduction-ion migration," fundamentally improving the rate performance and cycle stability of the cathode material. On the other hand, the use of fluorine oxide as a coating material can block direct contact between the electrolyte and the lithium manganese iron phosphate core, reducing HF corrosion and the dissolution of transition metals, thereby effectively suppressing interfacial side reactions. At the same time, the excellent thermal stability and wide electrochemical window of fluorine oxide can suppress electrolyte decomposition and gas production at high temperatures, significantly reducing the risk of side reactions under high temperature and high pressure conditions, and improving the thermal and electrochemical stability of the modified cathode material.

[0118] A comparison of Examples 1 and 4 shows that if the coating material is FeOF, the Fe-O bond energy is lower than that of the Al-O bond, making it susceptible to corrosion by HF in the electrolyte under high temperature or high pressure, which may lead to Fe... 2+ Dissolves and catalyzes electrolyte decomposition, while Fe 2+ Easily oxidized to Fe 3+ This causes lattice distortion in FeOF, leading to cracking of the cladding layer and loss of protection for the LMFP core.

[0119] As can be seen from the comparison between Example 1 and Examples 5-6, if the thickness of the coating layer is too small, the thin coating layer is prone to damage due to stress during cycling and cannot maintain its protective function for a long time, thus affecting the cycling stability of the material; if the thickness of the coating layer is too large, the excessively thick coating layer may generate interfacial stress due to the decreased matching with the core lattice, and is prone to peeling during charge and discharge volume changes, exacerbating the risk of interfacial failure.

[0120] As can be seen from the comparison between Example 1 and Examples 7-8, if the molar ratio of Ti to S doping is too small, the intrinsic electronic conductivity of lithium manganese iron phosphate will be limited. Even if S doping expands the lithium ion channels, the ion diffusion advantage cannot be fully utilized due to the inefficient conduction of electrons, resulting in limited improvement in the rate performance of the material. At the same time, excessive S may destroy the lattice integrity, increase structural defects, and exacerbate capacity decay during cycling. If the molar ratio of Ti to S doping is too large, the diffusion rate of lithium ions will be limited, lithium ions cannot migrate quickly, and excessive Ti may cause lattice distortion, destroy the structural stability of lithium manganese iron phosphate, and reduce the cycle life of the material.

[0121] As can be seen from the comparison between Example 1 and Example 9, if pre-firing is not performed in step (1), the carbon source reaction is insufficient, the raw material particles lack effective constraint under direct main firing, and over-sintering and grain growth are likely to occur, resulting in poor rate performance of the material. Furthermore, uneven particle size distribution will further reduce cycle stability. The uneven distribution of doped elements makes it difficult to effectively improve the performance of the material.

[0122] As can be seen from the comparison between Example 1 and Comparative Example 1, if Ti and Cl are co-doped in the lithium manganese iron phosphate core, the ionic radius of chloride ions is larger than that of PO4. 3- O in 2- After doping, it is easy to embed into the interstitial space or replace O. 2- The presence of chlorine sites exacerbates lattice distortion, undermines structural stability, and makes the structure prone to collapse during cycling. At the same time, chloride ions readily combine with lithium ions in the electrolyte at high temperatures to form LiCl, which not only consumes active lithium but may also form a loose LiCl layer at the interface, hindering lithium ion migration. Furthermore, the electron holes introduced by Ti may be neutralized due to the electron affinity of chlorine, weakening its effect on improving electronic conductivity.

[0123] As can be seen from the comparison between Example 1 and Comparative Example 2, if the coating layer is an alumina layer, its insulating oxide properties will significantly increase the interfacial impedance, hinder electron transport, and lead to a decrease in the material's rate performance. Simultaneously, alumina has a low lithium-ion diffusion coefficient, which prolongs the lithium-ion migration path. Furthermore, the lattice matching between alumina and lithium manganese iron phosphate is poor, making it prone to cracking due to stress concentration during volume changes in charge-discharge cycles. This makes it unable to provide long-term protection against HF corrosion in the electrolyte, ultimately leading to accelerated dissolution of transition metal ions and poor cycle stability.

[0124] It should be noted that the technical solution of the present invention is illustrated through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A modified cathode material, characterized in that, The modified cathode material includes a lithium manganese iron phosphate core and a coating layer covering the surface of the lithium manganese iron phosphate core, wherein the coating layer is made of a metal fluoride oxide; the lithium manganese iron phosphate core is co-doped with Ti and S; the molar ratio of Ti to S is 1:(0.04-0.4); A carbon layer is also present between the lithium manganese iron phosphate core and the coating layer; The general chemical formula of the lithium manganese iron phosphate core is LiMn. 1-x-y Fe x Ti y PO 4-z S z Where 0.2≤x≤0.8, 0<y<0.05, 0<z<0.02; The modified cathode material is prepared by the following method, which includes the following steps: A lithium source, a manganese source, an iron source, a phosphorus source, a sulfur source, a titanium source, and a carbon source are mixed and sintered to obtain a sintered product; the sintering process includes a pre-firing and a main firing performed sequentially; the pre-firing temperature is 300-500℃; A coating layer is deposited on the surface of the sintered product to obtain the modified cathode material; wherein the material of the coating layer includes fluorine oxide; The deposition method for the coating layer is a co-precipitation method, and the specific steps include: (a) The metal fluorine mixture and the sintering product are mixed to obtain a suspension; (b) Adjust the pH of the suspension to carry out a co-precipitation reaction so that the surface of the sintered product is coated with metal hydroxy fluoride, and then perform a calcination treatment to convert the metal hydroxy fluoride into metal fluoride oxide.

2. The modified cathode material according to claim 1, characterized in that, The metal fluoride oxide includes AlOF.

3. The modified cathode material according to claim 1, characterized in that, The thickness of the coating layer is 5-50 nm.

4. The modified cathode material according to claim 1, characterized in that, The thickness of the carbon layer is 1-10 nm.

5. The modified cathode material according to claim 1, characterized in that, The particle size D50 of the lithium manganese iron phosphate core is 100-800nm.

6. A method for preparing the modified cathode material according to any one of claims 1-5, characterized in that, The preparation method includes the following steps: A lithium source, a manganese source, an iron source, a phosphorus source, a sulfur source, a titanium source, and a carbon source are mixed and sintered to obtain a sintered product; the sintering process includes a pre-firing and a main firing performed sequentially; the pre-firing temperature is 300-500℃; A coating layer is deposited on the surface of the sintered product to obtain the modified cathode material; wherein the coating layer material includes fluorine oxide; the coating layer is deposited by a co-precipitation method, and the specific steps include: (a) The metal fluorine mixture and the sintering product are mixed to obtain a suspension; (b) Adjust the pH of the suspension to carry out a co-precipitation reaction so that the surface of the sintered product is coated with metal hydroxy fluoride, and then perform a calcination treatment to convert the metal hydroxy fluoride into metal fluoride oxide.

7. The preparation method according to claim 6, characterized in that, The sulfur source includes ammonium sulfide and / or thiourea.

8. The preparation method according to claim 6, characterized in that, The titanium source includes titanium dioxide and / or tetrabutyl titanate.

9. The preparation method according to claim 6, characterized in that, The lithium source includes any one or a combination of at least two of lithium hydroxide monohydrate, lithium carbonate, lithium nitrate, or lithium chloride.

10. The preparation method according to claim 6, characterized in that, The manganese source includes any one or a combination of at least two of manganese carbonate, manganese acetate, manganese dioxide, manganese tetroxide, or manganese nitrate.

11. The preparation method according to claim 6, characterized in that, The iron source includes any one or a combination of at least two of the following: ferrous oxalate dihydrate, ferric oxide, ferric oxide, ferrous chloride, or ferrous nitrate.

12. The preparation method according to claim 6, characterized in that, The phosphorus source includes any one or a combination of at least two of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, or phosphoric acid.

13. The preparation method according to claim 6, characterized in that, The preheating time is 2-6 hours.

14. The preparation method according to claim 6, characterized in that, The pre-burning atmosphere is an inert atmosphere.

15. The preparation method according to claim 6, characterized in that, The main firing temperature is 650-800℃, and the time is 5-15 hours.

16. The preparation method according to claim 6, characterized in that, The atmosphere for the main firing is an inert atmosphere.

17. The preparation method according to claim 6, characterized in that, In step (a), the total concentration of metal ions and fluoride ions in the metal-fluorine mixture is 300-5000 mg / L.

18. The preparation method according to claim 6, characterized in that, The coprecipitation reaction in step (b) is carried out at a temperature of 70-90°C for 1-5 hours.

19. The preparation method according to claim 6, characterized in that, The roasting process in step (b) is carried out at a temperature of 400-600℃ for 2-6 hours.

20. The preparation method according to claim 6, characterized in that, The preparation method includes the following steps: (1) After mixing lithium source, manganese source, iron source, phosphorus source, sulfur source, titanium source and carbon source, add alcohol solvent, perform wet ball milling, then perform pre-calcination for 2-6 hours in an inert atmosphere at 300-500℃, and perform main calcination for 5-15 hours in an inert atmosphere at 650-800℃. After completion, grind and sieve to obtain sintered products with a particle size D50 of 100-800nm. (2) The aluminum source, fluorine source and solvent are mixed to obtain an aluminum-fluorine mixture; wherein the total concentration of aluminum ions and fluorine ions in the aluminum-fluorine mixture is 300-5000 mg / L; The sintered product was dispersed in the aluminum-fluorine mixture and ultrasonically treated for 20-40 minutes to obtain a suspension. The pH of the suspension was adjusted to 2-4, and a co-precipitation reaction was carried out at 70-90℃ for 1-5 hours to allow the surface of the sintered product to be coated with aluminum hydroxy fluoride precursor. Then, the product was centrifuged, washed and dried to obtain an intermediate. The intermediate is calcined under an inert atmosphere to convert the aluminum hydroxy fluoride precursor into AlOF, thereby obtaining a modified cathode material; wherein the calcination temperature is 400-600℃ and the time is 2-6h.

21. The application of a modified cathode material as described in any one of claims 1-5 in the field of secondary batteries.

Citation Information

Patent Citations

  • Fluoride / oxide co-coated positive electrode material and preparation method thereof

    CN112151798A

  • Modified positive electrode material and preparation method and application thereof

    CN117878315A