A method for dynamic gauge change in tandem cold rolling

By controlling the rolling force, additional tension, and bending force of the cold rolling mill, the problems of strip breakage and low yield in the dynamic specification process of strip steel with large differences in rolling characteristics were solved, and stable rolling and efficient production were achieved.

CN120815818BActive Publication Date: 2026-11-20SHOUGANG ZHIXIN QIAN AN ELECTROMAGNETIC MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510906686.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-02
Publication Date
2026-11-20
Estimated Expiration
2045-07-02

AI Technical Summary

Technical Problem

When dealing with two strip steels with significantly different rolling characteristics, existing technologies struggle to achieve dynamic specification changes, which can easily lead to strip breakage and low yield.

Method used

By controlling the rolling force and additional tension of the connecting weld seam through the cold rolling mill, combined with the adjustment of the bending roll force and the roll shifting value, a smooth transition between low-speed rolling and high-speed stable rolling is achieved, ensuring rolling stability and thickness accuracy.

Benefits of technology

It enables dynamic specification changes without stopping the machine, improves rolling stability and yield, avoids edge cracking defects, and ensures the quality and production efficiency of cold-rolled products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120815818B_ABST
    Figure CN120815818B_ABST
Patent Text Reader

Abstract

The application discloses a method for dynamic gauge change in cold continuous rolling, and aims at solving the technical problems of low rolling speed and low yield rate in the gauge change of steel with large difference in rolling characteristics in the prior art. The method comprises the following steps: first strip steel and second strip steel are sequentially rolled by a cold rolling unit, wherein the rolling force of the connecting weld when passing through any rack of the cold rolling unit is 110-130% of the set rolling force of the corresponding rack of the one with low strength in the first strip steel and the second strip steel; the tail of the first strip steel and the head of the second strip steel are low-speed rolled at a speed of 30-80 m / min, and the additional tension of the hot-rolled strip steel in the low-speed rolling process is 105-125% of the set tension. The method provided by the application improves the efficiency of gauge change, guarantees the flatness and thickness precision, and improves the yield rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of cold continuous rolling technology, specifically relating to a method for dynamic specification change in cold continuous rolling. Background Technology

[0002] Cold rolling mills offer high rolling speeds and strong rolling capacity, making them widely used for rolling strips with similar rolling characteristics. However, some strips exhibit significantly different rolling characteristics. For example, due to differences in material properties such as alloy composition and microstructure, the rolling parameters used when rolling different strips vary considerably. Therefore, when switching between different specifications and grades, the dynamic specification change method cannot be directly used, or strip breakage is prone to occur. This necessitates empty rolling of the weld seam to the coiler before starting the rolling mill for the raw material plate. This method wastes the mill's production efficiency and results in a loss of yield. For some grades, starting the rolling mill is very difficult and requires highly skilled operation, making strip breakage during start-up extremely likely.

[0003] Therefore, it is urgent to improve the rolling rate and yield of two strip steels with significantly different rolling characteristics. Summary of the Invention

[0004] To address the technical problems of low rolling speed and low yield for two types of strip steel with significantly different rolling characteristics, this application provides a method for dynamic variable specification cold continuous rolling.

[0005] This application provides a method for dynamic specification change in cold continuous rolling, applicable to a first strip and a second strip connected sequentially by a connecting weld, wherein the first strip and the second strip are made of different materials, and the method includes:

[0006] The first and second strips are sequentially cold rolled on a cold rolling mill, wherein:

[0007] The rolling force when the connecting weld passes through any stand of the cold rolling mill is 110 to 130% of the set rolling force of the lower strength strip of the first and second strips passing through the corresponding stand.

[0008] The tail of the first strip and the head of the second strip are rolled at a low speed of 30 to 80 m / min. During the low-speed rolling process, the additional tension of the hot-rolled strip is 105 to 125% of the set tension.

[0009] In some embodiments, during the low-speed rolling process, the rolling force F of the stand where the hot-rolled strip is located, the bending force V of the work roll, and the width W of the hot-rolled strip meet the following relationship: V=a*W+b*F, where: the value of a ranges from -0.0001 to -0.01; and the value of b ranges from 0.003 to 0.027.

[0010] In some embodiments, the difference between the bending force of the work rolls for rolling the first strip and the bending force of the work rolls for rolling the second strip, ΔV1, and the difference between the rolling force at the tail of the first strip and the rolling force at the head of the second strip, ΔF1, conform to the following relationship: ΔV1=b*ΔF1.

[0011] In some embodiments, the rolling speed of the tail of the first strip and the head of the second strip is 40 to 60 m / min.

[0012] In some embodiments, during the low-speed rolling process, the additional tension of the hot-rolled strip is 110 to 120% of the set tension.

[0013] In some embodiments, the tail of the first strip is within a range of 5 to 15 meters before the connecting weld, and the head of the second strip is within a range of 5 to 15 meters after the connecting weld.

[0014] In some embodiments, when the width of the first strip is greater than the width of the second strip, the tapered section of the work roll is moved toward the rolling centerline after the connecting weld exits the cold rolling mill.

[0015] In some embodiments, when the width of the first strip is less than the width of the second strip, the tapered section of the work roll is moved away from the rolling centerline before the connecting weld enters the cold rolling mill.

[0016] In some embodiments, the thickness of the hot-rolled strip is 1.5 to 3.0 mm, and in the first strip and the second strip, the mass fraction of Si in one strip is ≥2.0%, and the mass fraction of Si in the other strip is <2.0%.

[0017] In some embodiments, the width difference between the first strip and the second strip is ≤240mm.

[0018] According to an embodiment of this application, a method for dynamic variable specification cold rolling is provided, applicable to a first strip and a second strip connected sequentially by a connecting weld, wherein the first strip and the second strip are made of different materials. The method includes: the first strip and the second strip are sequentially cold rolled by a cold rolling mill, wherein: the rolling force when the connecting weld passes through any stand of the cold rolling mill is 110-130% of the set rolling force of the lower strength of the first strip and the second strip passing through the corresponding stand;

[0019] The tail of the first strip and the head of the second strip are rolled at a low speed of 30 to 80 m / min. During the low-speed rolling process, the additional tension of the hot-rolled strip is 105 to 125% of the set tension.

[0020] This application ensures thickness accuracy and improves rolling stability by controlling the rolling force when the connecting weld passes through the stand. By controlling the additional tension at and around the connecting weld, it offsets part of the rolling force during low-speed operation, reduces the difference in rolling force between the low-speed rolling and high-speed stable rolling stages, improves the stability of the cold continuous rolling process, and avoids edge cracking defects in steel grades with high rolling strength and poor plasticity, thereby improving the quality of cold-rolled products.

[0021] The cold rolling dynamic specification change method provided in this application is applicable to two strips of different materials. It enables online dynamic specification change rolling without stopping the machine, resulting in high production efficiency. By controlling the low-speed rolling in the transition zone, combined with the control of rolling force and additional tension, the stability of the rolling process is ensured, and product quality is improved. The strip length is short during the dynamic specification change stage, which increases the yield. Attached Figure Description

[0022] Figure 1 A process flowchart of a method for dynamic specification change in cold continuous rolling according to one or more embodiments of this application is shown. Detailed Implementation

[0023] To enable those skilled in the art to more clearly understand this application, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0024] Connecting multiple strips sequentially and then cold-rolling them on a continuous rolling mill can improve rolling efficiency. Generally, adjacent strips are joined by welding.

[0025] The first aspect of this application provides a method for dynamic specification change in cold continuous rolling, which is applicable to the cold continuous rolling of a first strip and a second strip of different materials connected by a connecting weld. The rolling process is stable and the strip length is short during the dynamic specification change stage.

[0026] Please see Figure 1 The method for dynamic specification change in cold continuous rolling provided in this application includes:

[0027] The first and second strips are sequentially cold rolled on a cold rolling mill, wherein:

[0028] S1. When the connecting weld passes through any stand of the cold rolling mill, the rolling force is 110-130% of the set rolling force of the lower strength strip of the first strip and the second strip passing through the corresponding stand.

[0029] When the connecting weld passes through the cold rolling mill, the speed is reduced, and the transition section connecting the first and second strips is rolled at a low speed to improve the stability of the connecting weld as it passes through the cold rolling mill. However, under low-speed continuous cold rolling conditions, a larger rolling force needs to be controlled to ensure the rolling thickness accuracy. But if the rolling force is too large, it will cause ultra-thin slippage or strip breakage. Therefore, the rolling force of the connecting weld when it passes through any stand is 110 to 130% of the set rolling force of the lower strength one of the first and second strips when it passes through the corresponding stand. This can improve rolling stability and ensure rolling thickness accuracy.

[0030] Generally, a cold rolling mill has 5 to 7 stands. Taking a cold rolling mill with 6 stands as an example, the 6 stands along the cold rolling direction are, in sequence, the first stand, the second stand, the third stand, the fourth stand, the fifth stand, and the sixth stand. Assuming that when the connecting weld passes through the third stand, the rolling force applied to the connecting weld by the third stand is 110-130% of the set rolling force for the lower-strength strip between the first and second strips passing through the third stand. The set rolling force for the lower-strength strip passing through the third stand refers to the set rolling force when the lower-strength strip is rolled at a normal (high-speed stable rolling, e.g., a rolling rate of 800-1500 m / min) rate.

[0031] When the strength of the first strip is higher than that of the second strip, the first strip is more difficult to roll. The set rolling force of the first strip when it passes through the mill stand is greater than that of the second strip when it passes through the mill stand. In this case, the connecting weld is based on the set rolling force of the second strip when it passes through the mill stand, and is increased by 10% to 30%. This can ensure the rolling stability of the connecting weld and its vicinity. If the connecting weld is based on the set rolling force of the first strip when it passes through the mill stand, the rolling force at the weld will be too large, which may cause the strip near the connecting weld and the second strip to become too thin and break.

[0032] When the strength of the first strip is lower than that of the second strip, rolling the first strip is easier. The set rolling force for the first strip as it passes through the mill stand is less than that for the second strip. In this case, the connecting weld is based on the set rolling force of the first strip as it passes through the mill stand, with an upward adjustment of 10% to 30%. This ensures the rolling stability of the connecting weld and its vicinity. If the connecting weld is based on the set rolling force of the second strip as it passes through the mill stand, there is a risk that the connecting weld may break due to excessive rolling force and an ultra-thin first strip.

[0033] During low-speed rolling, the rolling force at the tail of the first strip is 110-130% of the set rolling force for the first strip, improving the thickness accuracy and rolling stability of the tail of the first strip. The rolling force at the head of the second strip is 110-130% of the set rolling force for the second strip, improving the thickness accuracy and rolling stability of the tail of the second strip.

[0034] S2. The tail of the first strip and the head of the second strip are rolled at a low speed of 30 to 80 m / min. During the low-speed rolling process, the additional tension of the hot-rolled strip is 105 to 125% of the set tension.

[0035] As mentioned earlier, using low-speed rolling for the tail of the first strip and the head of the second strip ensures the stable passage of the connecting weld and its vicinity through the cold rolling mill, improving the stability of the cold continuous rolling process. If the rolling rate of the tail of the first strip and the head of the second strip is too low, it may reduce production efficiency to some extent and prolong the length of the strip during the dynamic specification change stage; if the rolling rate of the tail of the first strip and the head of the second strip is too high, it may increase the risk of strip breakage to some extent and also affect the thickness accuracy to some extent.

[0036] During the low-speed rolling of the tail of the first strip and the head of the second strip, the additional tension of the hot-rolled strip is increased, which reduces the rolling force of the corresponding stands. During the stable high-speed rolling of the other parts of the first and second strips (excluding the middle sections of the head and tail), no additional tension is applied. This reduces the difference between the stand rolling force during low-speed rolling and the stand rolling force during high-speed stable rolling, thus reducing the difference between the stand rolling force during the rolling of the tail of the first strip and the head of the second strip and the stand rolling force during high-speed stable rolling of the other parts, thereby improving the rolling stability of the first and second strips. When the tail of the first strip passes through the continuous rolling mill, the additional tension applied to the tail of the first strip is 105-125% of the set tension of the first strip. When the head of the second strip passes through the continuous rolling mill, the additional tension applied to the head of the second strip is 105-125% of the set tension of the second strip.

[0037] The rolling force during low-speed rolling of strip steel is higher than that during high-speed stable rolling. If the additional tension of hot-rolled strip steel is too small, it will cause the rolling force to be too large to a certain extent, which can easily overload the rolling mill and cause equipment damage. For strip steel with high strength, such as electrical steel with Si mass fraction ≥2.0%, the material itself is hard and strong but has poor plasticity. Under such high rolling force, it is very easy to develop edge crack defects.

[0038] As the above analysis shows, this application achieves online specification changes without stopping the mill by controlling the rolling force and additional tension of the connecting weld as it passes through the stand, thus shortening the length of the variable specification strip. Controlling the rolling force of the connecting weld as it passes through any stand of the cold rolling mill improves rolling stability; controlling the additional tension of the connecting weld and its vicinity reduces the rolling force during low-speed rolling, decreasing the difference in rolling force between the low-speed and high-speed stable rolling stages, thereby improving the stability of the cold continuous rolling process and avoiding edge cracking defects caused by rolling high-strength, low-plasticity steel grades, thus improving the quality of cold-rolled products.

[0039] In addition to the aforementioned control of rolling force and additional tension, to further improve the dynamic shape effect of cold continuous rolling and enhance the stability of the rolling process, it is also necessary to control the rolling force F of the mill stand, the bending force V of the work rolls, and the width W of the hot-rolled strip. Specifically, in some embodiments, during the low-speed rolling process, the rolling force F of the mill stand containing the hot-rolled strip, the bending force V of the work rolls, and the width W of the hot-rolled strip conform to the following relationship:

[0040] V = a * W + b * F

[0041] In the formula: V is the bending force of the work roll, in tons or kN; W is the width of the hot-rolled strip, in mm. When rolling the tail of the first strip, the width at this point is the width of the first strip. When rolling the head of the second strip, the width at this point is the width of the second strip; F is the actual rolling force of any stand in the continuous rolling mill. The weld length angle is not considered. The unit is tons or kN; a is the coefficient of variation of the bending force of the work roll with the width of the hot-rolled strip. The value of a ranges from -0.0001 to -0.01; b is the coefficient of variation of the bending force of the work roll with the rolling force. The value of b ranges from 0.003 to 0.027.

[0042] Controlling the bending roll force can control the crown of hot-rolled strip after cold continuous rolling. As shown in the formula above, the bending roll force, rolling force, and width of the hot-rolled strip are matched. When the rolling force of the stand is large, the bending roll force of the work rolls of that stand is also large to ensure that the strip does not have edge waviness after cold rolling, thus improving the strip shape accuracy. When the width of the hot-rolled strip is wide, the bending roll force of the work rolls is small; when the width of the hot-rolled strip is narrow, the bending roll force of the work rolls is large to ensure the strip shape.

[0043] In some embodiments, the difference ΔV1 between the bending force of the work rolls rolling the first strip and the bending force of the work rolls rolling the second strip, and the difference ΔF1 between the rolling force at the tail of the first strip and the rolling force at the head of the second strip, conform to the following relationship: ΔV1=b*ΔF1. The bending force of the work rolls remains constant throughout the entire strip rolling process; therefore, the bending force of the work rolls is the same during high-speed rolling and low-speed rolling. Controlling ΔV1=b*ΔF1 can ensure the shape accuracy of the first strip after rolling, thereby improving the stability of the rolling process.

[0044] In this application, the units for rolling force and bending force are both kN, which can also be converted to tons, 10 kN ≈ 1 ton.

[0045] The rolling force for the first strip and the second strip during high-speed and stable rolling is the aforementioned set rolling force for each.

[0046] In some embodiments, the low-speed rolling speed of the tail of the first strip and the head of the second strip is 40 to 60 m / min.

[0047] In some embodiments, during the low-speed rolling process, the additional tension of the hot-rolled strip is 110 to 120% of the set tension.

[0048] In some embodiments, the tail of the first strip is within a range of 5 to 15 meters before the connecting weld, and the head of the second strip is within a range of 5 to 15 meters after the connecting weld.

[0049] In some embodiments, when the width of the first strip is greater than the width of the second strip, the tapered section of the work roll is moved towards the rolling centerline after the connecting weld exits the cold rolling mill. The work roll includes tapered and straight sections connected sequentially along the axial direction, with the cross-sectional diameter of the tapered section increasing sequentially from the tapered section to the straight section. The thickness of the strip can be adjusted by adjusting the work roll with the tapered section. Each stand includes two work rolls, arranged vertically opposite each other. The two tapered sections are located on the operating side and drive side of the continuous rolling mill, respectively, meaning the tapered sections of the two work rolls are arranged in opposite directions. After the connecting weld exits the cold rolling mill, the tapered section of the work roll is moved towards the rolling centerline, that is, the tapered section of the work roll moves towards the axial center section of the work roll. During this movement, the two oppositely arranged work rolls move in opposite directions. The wider strip is rolled first, followed by the narrower strip, meaning the rolling width gradually decreases. After the connecting weld has passed, the tapered section is moved towards the rolling centerline. This ensures the shape accuracy and stability of the wider first strip during size changes. The movement of the two work rolls on each stand is (W2-W1) / 2, where W1 is the width of the first strip and W2 is the width of the second strip.

[0050] In some embodiments, when the width of the first strip is lower than the width of the second strip, the tapered section of the work roll is moved away from the rolling centerline before the connecting weld enters the cold rolling mill, and the amount of movement is (W2-W1) / 2, where W1 is the width of the first strip and W2 is the width of the second strip.

[0051] The narrower strip is rolled first, followed by the wider strip, meaning the strip width gradually increases. Before the weld is connected, the tapered sections of both work rolls on the stand are moved outwards to ensure the shape accuracy of the second strip at the head. If the work roll position is adjusted after the weld is connected and the strip exits the cold rolling mill, the head of the second strip is prone to large or medium waviness or even undercut defects, affecting the strip shape and potentially causing strip breakage and damaging the rolls.

[0052] In some embodiments, the thickness of the hot-rolled strip is 1.5 to 3.0 mm, the width difference between the first strip and the second strip is ≤240 mm, and the difference in raw material thickness meets the welding requirements of the welding machine.

[0053] In some embodiments, of the first strip and the second strip, one strip has a Si mass fraction ≥ 2.0%, and the other strip has a Si mass fraction < 2.0%. Strips with a Si mass fraction ≥ 2.0% have high strength, high brittleness, and are difficult to roll; strips with a Si mass fraction < 2.0% have low strength, good plasticity, and are easy to roll.

[0054] For two strips with completely different rolling characteristics, the strip with a Si mass fraction ≥ 2.0% may be rolled first and the strip with a Si mass fraction < 2.0% may be rolled second; or the strip with a Si mass fraction < 2.0% may be rolled first and the strip with a Si mass fraction ≥ 2.0% may be rolled second. The cold continuous rolling dynamic specification change method provided in this application is applicable to either of the above situations.

[0055] The following specific embodiments further illustrate the cold continuous rolling dynamic specification method provided in this application:

[0056] Taking two adjacent strips of steel, silicon steel and carbon steel, as examples, the silicon steel has a width of 1150 mm, a silicon content of 2.2%, and a finished thickness of 0.35 mm. The carbon steel has a width of 1200 mm, a silicon content of 0.2%, and a finished thickness of 0.3 mm. The strength of silicon steel is greater than that of carbon steel. Tables 1 and 2 show the rolling process parameters for silicon steel and carbon steel, respectively. The set rolling force can also be the actual rolling force. S1 to S6 are the stand numbers sequentially arranged along the rolling direction of the strip in the continuous rolling mill.

[0057] Table 1. Process parameters for stabilized (high-speed) rolling of silicon steel Rack number S1 entrance S1 S2 S3 S4 S5 S6 Set rolling force - high speed (tons) / 903 894 766 663 661 582 Set tension (tons) 14.7 28.9 19.8 13.3 10.2 8 2.5 Compression ratio (%) / 38 36.5 31.3 28 22.9 11 Work roll misalignment value (mm) / -70 -50 -30 0 0 -20 Intermediate roll slippage value (mm) / 0 0 0 0 0 0 Work roll bending force (tons) / 5 6 7 4 3 2 Intermediate roll bending force (tons) / 14 15 16 16 16 8

[0058] Table 2. Process parameters for stabilized rolling of carbon steel Rack number S1 entrance S1 S2 S3 S4 S5 S6 Set rolling force - high speed (tons) / 765 774 666 637 561 491 Set tension (tons) 13.1 23.3 15.8 12 8.2 6.3 2.5 Compression ratio (%) / 35 37 31.2 26 24 12 Work roll misalignment value (mm) / -70 -50 -30 0 0 -20 Intermediate roll slippage value (mm) / 0 0 0 0 0 0 Work roll bending force (tons) / 2.5 3.5 3.6 3.5 2.5 1.5 Intermediate roll bending force (tons) / 14 15 16 16 16 8

[0059] Example 1

[0060] The first coil of strip steel is silicon steel, and the second coil of strip steel is carbon steel. The first coil of strip steel is rolled in the cold rolling mill first, and the second coil of strip steel is rolled in the cold rolling mill afterward. The second strip steel has lower strength.

[0061] Rolling of the tail section of the first coil of strip and the head section of the second coil of strip:

[0062] When rolling the first coil of silicon steel to the tail end, before the connecting weld enters the first stand (S1 stand) 10 meters, the cold rolling mill reduces its speed to 50 m / min, executes the steel grade change procedure, shuts down all automatic thickness control functions, and enters manual roll gap adjustment mode. After the connecting weld of the first coil of silicon steel and the second coil of carbon steel passes the last stand (S6 stand), the cold rolling mill begins to increase its speed and performs normal rolling of the second coil of carbon steel.

[0063] The rolling force of the silicon steel strip tail passing through stands S1 to S6 is 110 to 130% of the set rolling force of silicon steel. The rolling force of each stand can be found in Table 3.

[0064] The rolling force of the connecting weld seam through stands S1 to S6 is 110 to 130% of the set rolling force for carbon steel. Please refer to Table 3 for the specific rolling force of each stand.

[0065] The rolling force of the carbon steel strip passing through stands S1 to S6 is 110 to 130% of the set rolling force for carbon steel. Please refer to Table 3 for the rolling force of each stand.

[0066] The difference ΔF1 between the rolling force when rolling the tail of the first strip and the rolling force when rolling the head of the second strip can be found in Table 3.

[0067] During the low-speed rolling process, the additional tension of the hot-rolled strip is 115% of the set tension.

[0068] Table 3 Rack number S1 S2 S3 S4 S5 S6 Rolling force (tons) for silicon steel strip tail. 1042 1090 961 843 812 698 Carbon steel strip rolling force - low speed (tons) 865 875 763 732 656 588 Rolling force of the weld (tons) 865 875 763 732 656 588 Rolling force difference △F1 (tons) 177 215 198 111 156 110 The difference in bending force between silicon steel and carbon steel is ΔV1 (tons). 2.5 2.5 3.4 0.5 0.5 0.5

[0069] When the strip deformation zone of the first stand enters the last stand and the deviation between the actual strip thickness and the set thickness of each stand is less than 50 micrometers, the automatic thickness control function of the continuous rolling mill is activated, enabling the continuous rolling mill to precisely adjust the thickness of each stand and gradually increase the speed to a stable rolling speed. During low-speed rolling, the additional tension for silicon steel and carbon steel is 110% of their respective set tensions.

[0070] Before the dynamic specification change (before the connecting weld reaches the S1 stand), the tapered sections of the work rolls and intermediate rolls from the S1 stand to the S6 stand are moved 25mm away from the rolling centerline in advance, according to the width of the carbon steel.

[0071] When the weld seam connecting the first coil of silicon steel and the second coil of carbon steel arrives at the coiler, the weld seam shearing procedure is not executed. After the dynamic specification change is successful, the shearing procedure is executed to shear the strip steel with unqualified thickness.

[0072] Example 2

[0073] In Example 2, the first coil of strip steel is carbon steel, and the second coil of strip steel is silicon steel. During the low-speed rolling (70m / min) process of the first and second coils of strip steel:

[0074] The rolling forces for the carbon steel strip tail passing through stands S1 to S6 are shown in Table 4. The rolling forces for the connecting welds passing through stands S1 to S6 are 110–130% of the set rolling forces for carbon steel; the specific rolling forces for each stand are shown in Table 4. The rolling forces for the silicon steel strip head passing through stands S1 to S6 are 110–130% of the set rolling forces for carbon steel; the rolling forces for each stand are shown in Table 4. The difference ΔF1 between the rolling forces for the carbon steel strip tail and the silicon steel strip head is shown in Table 4.

[0075] During the low-speed rolling process, the additional tension of the hot-rolled strip is 110% of the set tension.

[0076] After connecting the weld seam to the corresponding frame, move the tapered section of the work roll 25mm toward the rolling centerline.

[0077] Table 4 Rack number S1 S2 S3 S4 S5 S6 Carbon steel rolling force - low speed (tons) 880 890 766 733 645 565 Silicon steel strip rolling force - low speed (tons) 1038 1028 881 762 760 669 Rolling force of the weld (tons) 880 890 766 733 645 565 Rolling force difference △F1 (tons) 158 138 115 29 115 104 The difference in bending force between silicon steel and carbon steel is ΔV1 (tons). 2.5 2.5 3.4 0.5 0.5 0.5

[0078] Example 3

[0079] In Example 3, the first strip coil is silicon steel, and the second strip coil is carbon steel. During the low-speed rolling (40 m / min) of the first and second strip coils, the rolling force of the silicon steel strip tail passing through stands S1 to S6 is 110-130% of the set rolling force for silicon steel. The rolling forces for each stand are shown in Table 5. The rolling force of the connecting weld seam passing through stands S1 to S6 is 110-130% of the set rolling force for carbon steel. The specific rolling forces for each stand are shown in Table 5. The rolling force of the carbon steel strip head passing through stands S1 to S6 is 110-130% of the set rolling force for carbon steel. The rolling forces for each stand are shown in Table 5. The difference ΔF1 between the rolling force when rolling the tail of the first strip and the rolling force when rolling the head of the second strip is shown in Table 5.

[0080] During the low-speed rolling process, the additional tension of the hot-rolled strip is 110% of the set tension.

[0081] After connecting the weld seam to the corresponding stand, move the tapered section of the work roll 25mm away from the rolling centerline, and increase the roll shifting value of the work roll and intermediate roll of that stand.

[0082] Table 5

[0083] Table 6 shows the quality of the tail position of the first strip and the head position of the second strip.

[0084] The cold continuous rolling dynamic specification method provided in Examples 1 to 3 did not result in strip breakage, improved rolling stability, no waviness, good strip shape, no edge cracks, and good appearance quality. The strip length of the dynamically specified strip is short, and the loss of hot-rolled coil length does not exceed 30m. Compared with the 100m loss of changing specifications when stopping, this application saves about 70 meters and further improves the yield.

[0085] The cold continuous rolling dynamic specification change method provided in this application has at least the following advantages:

[0086] (1) Controlling the rolling force of the connecting weld seam when it passes through any stand of the cold rolling mill to be 110-130% of the set rolling force of the strip on the lower strength side when it passes through the corresponding stand can ensure rolling stability and shorten the rolling length of the strip in the variable specification range.

[0087] (2) Controlling the additional tension of the connecting weld and its vicinity further reduces the rolling force at low speed, reduces the difference in rolling force between the two stages of low-speed rolling and high-speed stable rolling, improves the stability of the cold continuous rolling process, avoids the edge cracking defect caused by steel with high rolling strength and poor plasticity, and thus improves the quality of cold-rolled products.

[0088] (3) The bending roll force is compensated according to the strip width, and the bending roll force, rolling force and strip width are controlled to improve the strip shape accuracy.

[0089] (4) The roll shifting value in the transition zone was set according to the roll shifting value of the wider strip to ensure the stability of the variable specification in cold continuous rolling. The roll shifting values ​​of the work roll and intermediate roll when the connecting weld passes through the stand were controlled to ensure the strip shape.

[0090] (4) The method for dynamic specification change in cold continuous rolling provided in this application can ensure that the cold rolling mill does not experience drastic changes in roll gap during dynamic specification change, and realize dynamic adjustment between two strips of different materials. Compared with the traditional rolling method that uses raw material plate start-up method due to the large difference in rolling characteristics between the first and second strips, this application does not require the cold rolling mill to be stopped, thus improving production efficiency and yield.

[0091] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature being directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0092] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", and "counterclockwise" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0093] In this application, unless otherwise expressly specified and limited, the terms "connection," "fixed," etc., should be interpreted broadly. For example, "fixed" can mean a fixed connection, a detachable connection, or an integral part; it can mean a mechanical connection or an electrical connection; it can mean a direct connection or an indirect connection through an intermediate medium; it can mean the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0094] Furthermore, the use of terms such as "first" and "second" in this application is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, features defined with "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0095] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.

Claims

1. A method for dynamic specification change in cold continuous rolling, applicable to a first strip and a second strip connected sequentially by a connecting weld, wherein the first strip and the second strip are made of different materials, characterized in that... The method includes: The first and second strips are sequentially cold rolled on a cold rolling mill, wherein: The rolling force when the connecting weld passes through any stand of the cold rolling mill is 110-130% of the set rolling force of the lower strength strip between the first and second strips when passing through the corresponding stand; The tail of the first strip and the head of the second strip are rolled at a low speed of 30-80 m / min. The difference between the bending force of the work rolls rolling the first strip and the bending force of the work rolls rolling the second strip is... V1. The difference between the rolling force when rolling the tail of the first strip and the rolling force when rolling the head of the second strip. F1 satisfies the following relationship: V1=b F1; During the low-speed rolling process, the additional tension of the hot-rolled strip is 110-120% of the set tension. The rolling force F, the bending force V of the work rolls, and the width W of the hot-rolled strip on the stand meet the following relationship: The value of a ranges from -0.0001 to -0.01; the value of b ranges from 0.003 to 0.

027.

2. The method for dynamic specification change in cold continuous rolling according to claim 1, characterized in that, The rolling speed of the tail of the first strip and the head of the second strip is 40~60m / min.

3. The method for dynamic specification change in cold continuous rolling according to claim 1, characterized in that, The tail of the first strip is within a range of 5 to 15 meters before the connecting weld, and the head of the second strip is within a range of 5 to 15 meters after the connecting weld.

4. The method for dynamic specification change in cold continuous rolling according to claim 1, characterized in that, When the width of the first strip is greater than the width of the second strip, the tapered section of the work roll is moved toward the rolling centerline after the connecting weld exits the cold rolling mill.

5. The method for dynamic specification change in cold continuous rolling according to claim 1, characterized in that, When the width of the first strip is less than the width of the second strip, the tapered section of the work roll is moved away from the rolling centerline before the connecting weld enters the cold rolling mill.

6. The method for dynamic specification change in cold continuous rolling according to claim 1, characterized in that, The thickness of the hot-rolled strip is 1.5~3.0mm. In the first strip and the second strip, the mass fraction of Si in one strip is ≥2.0%, and the mass fraction of Si in the other strip is <2.0%.

7. The method for dynamic specification change in cold continuous rolling according to claim 1, characterized in that, The width difference between the first strip and the second strip is ≤240mm.

Citation Information

Patent Citations

  • Control method for tandem cold mill

    CN105251781A

  • Method for preventing strip deformation zone from being broken in cold rolling dynamic variable specification process

    CN108856304A