一种轧制钛钢复合板的生产方法
By optimizing the dynamic gap design and the staged rolling process, the problem of poor interface bonding in titanium-steel composite plates was solved, achieving stable bonding and improved yield in large-area plates, and making it suitable for the production of titanium-steel composite plates of different specifications.
Patent Information
- Application Number
- CN202511194025.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-08-25
AI Technical Summary
In the rolling process for producing titanium-steel composite plates, the difference in high-temperature deformation characteristics between titanium and steel leads to poor interfacial bonding. This is especially true in the production of large-area plates, where it is difficult to achieve effective bonding across the entire size, resulting in increased cutting losses and reduced yield.
Through dynamic gap design and rolling process optimization, a gap design of G=min(50, max(25, 0.0072L+8.4)) mm is adopted, and a small reduction is controlled when the cumulative deformation is ≤30%. Combined with the welding of positioning blocks between the titanium middle plate and the frame, the extension buffer and position stability of the titanium layer are ensured, and the titanium-steel interface bonding is controlled by staged rolling.
It achieves consistent interface bonding in large-area composite panels, improves yield and product quality, adapts to production needs of different panel lengths, and reduces production costs.
Smart Images

Figure CN120828056B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal composite material manufacturing technology, and in particular to a production method for rolling titanium-steel composite plates. This method solves the problem of poor interfacial bonding caused by the difference in high-temperature deformation characteristics of titanium and steel during the rolling process by using dynamic gap design and rolling process optimization. Background Technology
[0002] Titanium-steel composite plates, possessing the superior properties of both titanium and steel, have been widely used in petroleum, chemical, and marine engineering fields. There are four main production methods for titanium-steel composite plates: explosive bonding, diffusion bonding, explosive-rolling, and rolling bonding. Among these, rolling bonding has become the main development direction for titanium-steel composite plate production due to its advantages of being environmentally friendly, efficient, and low-cost.
[0003] Currently, significant progress has been made in the research on the production of titanium-steel composite plates by rolling. However, in practical industrial applications, the stability of the bonding rate still faces challenges. In particular, when producing larger-sized plates, it is difficult to achieve effective bonding across a large area and full dimensions, leading to increased cutting losses, reduced yield, and inability to meet contract requirements for fixed-length specifications.
[0004] Existing research mainly focuses on improving interfacial shear strength, while paying insufficient attention to the issue of large-area bonding consistency. Besides known factors such as raw material surface condition and heating uniformity, the difference in deformation behavior between titanium and steel during rolling may be one of the key contributing factors: at high temperatures, the flow stress of titanium is significantly lower than that of steel, resulting in a significantly greater longitudinal elongation of the titanium cladding plate than the steel substrate under the same rolling force. Since the titanium-steel interface before compositing is only constrained by friction and lacks a forced deformation coordination mechanism, the excessive elongation of the titanium plate is rigidly bound by the frame within the billet structure, leading to local accumulation and forced formation of wavy, folded stacking (e.g., ...). Figure 2 (As shown). This wrinkling results in a periodic distribution of local contact areas (peaks) and delamination areas (troughs) at the interface—the contact areas can achieve metallurgical bonding under rolling pressure, while the delamination areas have micro-gap gaps that block atomic diffusion. This leads to a decrease in bonding area and bonding force. Existing processes rarely pay attention to the decisive influence of deformation coordination on the consistency of interface contact, which may be an important factor restricting the improvement of yield of large-area plates.
[0005] Therefore, it is urgent to explore an effective method to achieve stable interfacial bonding of titanium-steel composite plates produced by rolling, so as to improve its feasibility and reliability in industrial applications. Summary of the Invention
[0006] To address the deformation compatibility issues mentioned in the background art, this invention provides a method for producing rolled titanium-steel composite plates. The core of this method lies in the synergistic effect of dynamic gap design and optimized rolling process to suppress interfacial contact instability caused by the wrinkled stacking of titanium layers, thereby improving the bonding consistency of large-area composite plates. It should be noted that this solution can be implemented in conjunction with technologies such as raw material surface treatment and heating uniformity control.
[0007] The technical means employed in this invention are as follows: A method for producing rolled titanium-steel composite plates includes the following steps: S1. Raw material preparation: Prepare two titanium plates, two steel billets and frame, all of which are machined and leveled. S2. A release agent is coated on the surface of the titanium plate. S3, Billet Assembly: S31. Stack the steel billet, titanium plate, titanium plate, and steel billet symmetrically in the following order: steel billet-titanium plate-titanium plate-steel billet; S32. A frame is provided around the titanium middle plate, and a gap of Gmm is reserved between the inner side of the frame and the titanium middle plate. S33. Weld at least two titanium positioning blocks to the edges at both ends of the titanium plate. The positioning blocks are in contact with the inner side of the frame, and the welding position is within the cut edge range of the finished product. S34. Set the border width; S4. Heat the assembled billet to 850-950℃; S5. Roll the heated composite billet: When the cumulative deformation is ≤30%, the deformation per pass shall be controlled within 15%; when the cumulative deformation is >30%, the conventional rolling procedure shall be followed.
[0008] Furthermore, in S1, the thickness of the titanium plate and the steel billet is determined according to the compression ratio, the compression ratio is ≥10, and the length of the steel billet = length of the titanium plate + width of the frame × 2 + 2Gmm.
[0009] Furthermore, in S32, the gap G between the titanium plate and the frame satisfies: G=min(50,max(25,0.0072L+8.4)), where L is the length of the titanium plate (in mm).
[0010] Furthermore, when L < 2300 mm, G is taken as 25 mm.
[0011] Furthermore, in S34, the border width is 50mm.
[0012] Furthermore, in S5, when the cumulative deformation is ≤30%, the deformation per pass is within 10%.
[0013] In this invention: 1. Dynamic gap assembly: A gap G = min(50, max(25, 0.0072L + 8.4)) (mm) is set between the titanium middle plate and the frame, where L is the length of the titanium middle plate. This gap design provides buffer space for the extension of the titanium layer and also reduces the constraint stress of the frame.
[0014] Simultaneously, titanium positioning blocks (≥2 at each end) are welded to the beginning and end of the titanium plate. The tight contact between the positioning blocks and the inner side of the frame constrains the longitudinal movement of the titanium plate in the rolling direction, preventing it from sliding and accumulating in the billet cavity due to differences in elongation rates. This ensures that the titanium plate always maintains a preset relative position with the billet, avoiding increased wrinkling and stacking in the beginning and end areas due to displacement. The welding position is within the finished product cutting edge range, without compromising yield.
[0015] 2. Staged rolling control: When the cumulative deformation is ≤30%, a small reduction of 15% or less should be used, preferably not exceeding 10%. At this stage, the titanium steel is not yet composite, and a small reduction can reduce the difference in elongation of the titanium steel and prevent the titanium layer from rapidly extending and impacting the frame. After the cumulative deformation is >30%, the titanium steel has been initially composited, and the conventional rolling procedure should be followed.
[0016] Compared with the prior art, the present invention has the following outstanding effects: 1. Eliminate interface separation caused by wrinkled stacking: By dynamically accommodating the elongation amount and controlling the elongation rate with a small reduction amount, full-size bonding is ensured. Especially for large-size slabs, continuous contact of the entire interface is achieved, which is conducive to stable control of interface bonding.
[0017] 2. Strong engineering compatibility: The gap formula G=0.0072L+8.4 can be adapted to different plate lengths. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 This is a flowchart of the method of the present invention.
[0020] Figure 2 This is a schematic diagram of the rolling process using a symmetrical material assembly method according to the present invention.
[0021] Figure 3 This is a schematic diagram showing that after rolling, the titanium and steel are in both contact and non-contact states.
[0022] Figure 4This is a schematic diagram of the edge welding positioning blocks at both ends of the titanium plate of the present invention.
[0023] In the diagram: 1. Steel billet; 2. Titanium plate; 3. Isolation layer; 4. Frame; 5. Steel pipe; 6. Enclosure; 7. Positioning block. Detailed Implementation
[0024] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0025] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0026] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0027] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values of the components and steps described in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0028] When producing titanium-steel composite plates using the rolling process, to avoid warping caused by incoordination in the deformation of the two materials, a method is typically used... Figure 2The symmetrical assembly method shown is used for rolling. However, at high temperatures, titanium's deformation resistance is much lower than that of steel, and there are no constraints between the steel substrate and the titanium cladding plate other than friction. This results in the titanium plate elongating much more longitudinally than the steel plate under the same conditions in the initial stage of deformation. Furthermore, the titanium plate is constrained by the frame at both ends, preventing the longitudinal elongation from unfolding freely, leading to local accumulation and ultimately forming wavy folds to coordinate the deformation. This results in the simultaneous existence of both contact and non-contact areas between the titanium and steel at the interface (e.g.,...). Figure 3 (As shown). The interface diffusion products of these two states are completely different, which leads to an unstable bonding area in the final product.
[0029] To address the existing problems, this invention provides a method for producing rolled titanium-steel composite plates, which can improve the interfacial bonding rate of titanium-steel composite plates.
[0030] like Figure 1 As shown, the process flow for producing titanium-steel composite plates using the rolling method of this invention is as follows: preparation of raw materials such as composite titanium plates, base steel billets 1 and frame 4 → coating and isolating the composite titanium plates → symmetrical assembly of the base steel billets and composite titanium plates → heating of the composite billet → rolling of the composite billet → unloading. The technology and implementation methods of this invention are described in detail below according to the process flow: S1. Raw material preparation.
[0031] The raw material preparation for titanium-steel composite plates mainly includes titanium plates and steel billets.
[0032] Formula for calculating billet length: L 钢 =L 钛 +2×W 边框 +2G; Where: L 钛 Length of titanium plate (in mm); W 边框 : Frame width (fixed at 50mm to ensure welding strength); G: Dynamic gap value (unit mm), calculated according to the formula G=min(50,max(25,0.0072L+8.4)).
[0033] Among them, while ensuring welding strength, the frame width can also be other width dimensions by adjusting the billet length calculation.
[0034] The steel billet, titanium plate, and frame all need to be machined to level and remove oxide scale and oil stains.
[0035] The thickness of the titanium plate and the steel billet must meet the requirement of a compression ratio ≥10 (to ensure the complete elimination of the non-contact area at the interface). For example, if the finished product thickness is 2mm TA2 + 8mm Q235 and the compression ratio is 15, according to the proportional deformation calculation of titanium steel, the thickness of the titanium plate raw material should be 30mm and the thickness of the Q235 steel billet raw material should be 120mm.
[0036] S2, The surface of the titanium plate is coated with a release agent.
[0037] After wiping the oil stains off the surface of the titanium plate with anhydrous ethanol, apply a release agent and let it dry to form a release layer 3.
[0038] S3, billet assembly.
[0039] use Figure 2 The titanium-steel composite plate is assembled using a symmetrical assembly method, as shown. Specifically, the materials are assembled symmetrically from top to bottom in the following order: steel plate, titanium middle plate, titanium middle plate, and steel plate. A border is provided around the titanium middle plate, with a pre-reserved gap G between the inner side of the border and the titanium middle plate.
[0040] Align the center point of the titanium middle plate with the center point of the steel base plate. Since gaps are reserved between the beginning and end of the titanium middle plate and the frame to accommodate the longitudinal extension of the titanium middle plate, two positioning titanium blocks 7 need to be welded to the edges at both ends of the titanium middle plate (e.g., Figure 4 (As shown). Otherwise, during billet movement or rolling, the titanium plate may shift within the billet cavity, leading to uncontrolled final plate shape and dimensional accuracy. The welding position of the positioning block should be within the finished product's cut edge range; otherwise, it will affect the normal yield.
[0041] After the titanium billet is fixed, the upper steel substrate is placed and overlaps with the lower steel substrate.
[0042] After welding the upper and lower steel substrates to the frame, connect the steel pipe 5 to the frame, and then connect the external vacuum equipment to... Figure 2 The steel pipes are connected in group 5, and internal vacuum treatment (of the frame, titanium plate, and space between the steel billets) is performed. When the vacuum degree is ≤1×10⁻⁶... -2 After Pa, the steel pipe 5 is sealed (forming a sealing area 6) to maintain the internal vacuum.
[0043] S4, Heating Because of the limited solid solubility between titanium and steel, brittle intermetallic compounds easily form at the interface, compromising the bond strength. Therefore, the heating temperature is typically controlled between 850℃ and 950℃, preferably 900℃. Above 950℃, diffusion intensifies, and the number of compounds increases dramatically, while below 850℃, the load on the rolling mill increases.
[0044] S5, Rolling When the cumulative deformation is ≤30%, the deformation per pass should be controlled within 15%, ideally below 10%. Once the cumulative deformation exceeds 30%, further consideration is unnecessary. This is because in the early rolling passes, before the titanium and steel have fully bonded, there is no constraint between the titanium and the steel substrate except for friction. Since the deformation resistance of titanium is much lower than that of the steel substrate, a large deformation per pass will cause the titanium to rapidly elongate to the edge, forming a wavy pattern after being constrained and compressed by the edge, resulting in partial contact between the titanium and steel interface. When the cumulative deformation reaches 30% or more, the titanium and steel have formed a preliminary bond, and they will deform together, no longer producing wavy patterns.
[0045] This invention is applicable to the production of titanium-steel composite plates using the direct rolling method. It can be promoted in steel enterprises and can produce products with high bonding strength, showing good prospects for widespread application.
[0046] The production method of titanium-steel composite plate of the present invention can improve the interface bonding rate and achieve an average economic benefit of 0.5 million yuan / ton.
[0047] Example 1 The method of this invention for rolling a 2mm TA2+8mm Q235 composite plate specifically includes the following steps: S1. The design frame width is 50mm, and the compression ratio is 14. Based on the finished product thickness, the titanium medium plate thickness is determined to be 28mm, and the Q235 steel billet thickness is 112mm. The titanium medium plate length is 6000mm, and the reserved gap = min(50, 0.0072×6000+8.4) = min(50, 51.6) = 50mm gap. Therefore, the steel billet raw material length is 6000+50×2+2×50=6200mm. Both the titanium medium plate and the steel billet are machined to ensure straightness.
[0048] S2. After wiping the titanium plate clean with anhydrous ethanol, apply a release agent and let it air dry. The release agent coating thickness is 0.5mm.
[0049] S3, according to Figure 2 As shown, the titanium middle plate is assembled according to the following method: [The text abruptly ends here, likely due to an incomplete sentence or a formatting error.] Figure 4 Four positioning titanium blocks are welded as shown. After the preform assembly is completed, the interior is subjected to vacuum treatment with a vacuum degree of 0.008 Pa.
[0050] S4. Heating temperature is 900℃.
[0051] S5, the reduction amounts for the first four passes are 5%, 8%, 10%, and 12%, respectively. At this point, the cumulative deformation has reached 30%, and subsequent rolling is carried out automatically according to the model settings.
[0052] After rolling, the interface bonding rate was inspected by flaw detection, and no unqualified areas were found.
[0053] Example 2 The method of this invention is used to roll a 1.2mm TA2+10mm Q235 composite plate, which specifically includes the following steps: S1. The design frame width is 50mm, and the compression ratio is 12. Based on the finished product thickness, the titanium plate thickness is determined to be 14.4mm, and the Q235 steel billet thickness is 120mm. The titanium plate length is 4000mm, and the reserved gap = min(50, 0.0072×4000+8.4) = min(50, 37.2)≈37mm. Therefore, the steel billet raw material length is 4000+50×2+2×37=4174mm. Both the titanium plate and the steel billet are machined to ensure straightness.
[0054] S2. After wiping the titanium plate clean with anhydrous ethanol, apply a release agent and let it air dry. The release agent coating thickness is 1.0 mm.
[0055] S3, according to Figure 2 As shown, the titanium plates are assembled according to the following procedure: the head and tail areas are arranged as follows. Figure 4 Four positioning titanium blocks are welded as shown. After the preform assembly is completed, the interior is subjected to vacuum treatment with a vacuum degree of 0.007 Pa.
[0056] S4. Heating temperature is 910℃.
[0057] S5, the reduction amounts for the first four passes are 5%, 5%, 8%, 10%, and 12%, respectively. At this point, the cumulative deformation has reached 30%, and subsequent rolling is carried out automatically according to the model settings.
[0058] After rolling, the interface bonding rate was inspected by flaw detection, and no unqualified areas were found.
[0059] Example 3 The rolling process for producing a 1.0mm TA2+6mm Q345 composite plate (minimum specification boundary) includes the following steps: S1. The design frame width is 50mm, and the compression ratio is 12. Based on the finished product thickness, the titanium plate thickness is determined to be 12mm, and the Q235 steel billet thickness is 72mm. The titanium plate length is 2300mm, and the reserved gap = min(50, 0.0072×2300+8.4)=max(25, 24.96)=25mm. Therefore, the steel billet raw material length is 2300+50×2+2×25=2450mm. Both the titanium plate and the steel billet are machined to ensure straightness.
[0060] S2. After wiping the titanium plate clean with anhydrous ethanol, apply a release agent and let it air dry. The release agent coating thickness is 0.5mm.
[0061] S3, according to Figure 2 As shown, the titanium middle plate is aligned with the center point of the Q235 steel base plate, and a 25mm gap is reserved between it and the frame. After the assembly is completed, the interior is vacuum treated with a vacuum degree of 0.008Pa.
[0062] S4. Heating temperature is 900℃.
[0063] S5, the reduction amounts for the first four passes are 6%, 8%, 10%, and 10%, respectively. At this point, the cumulative deformation has reached 30%. Subsequent rolling is carried out according to the automatic settings of the model, and no side pressure is used throughout the rolling process.
[0064] After rolling, the plates were separated, and no non-bonding areas were found during flaw detection.
[0065] Comparative Example 1 (Insufficient gap, failure) The rolling process for producing a 2mm TA2+8mm Q235 composite plate includes the following steps: S1. The design frame width is 50mm, and the compression ratio is 14. Based on the finished product thickness, the titanium plate thickness is determined to be 28mm, and the Q235 steel billet thickness is 112mm. The titanium plate length is 6000mm, and the steel billet raw material length is 6100mm. Both the titanium plate and the steel billet are machined to ensure straightness.
[0066] S2. After wiping the titanium plate clean with anhydrous ethanol, apply a release agent and let it air dry. The release agent coating thickness is 0.5mm.
[0067] S3, according to Figure 2 As shown, the titanium middle plate is aligned with the center point of the Q235 steel base plate, with no gap between it and the frame. After the assembly is completed, the interior is subjected to vacuum treatment with a vacuum degree of 0.008 Pa.
[0068] S4. Heating temperature is 900℃.
[0069] S5, the reduction amounts for the first four passes are 5%, 8%, 10%, and 12%, respectively. At this point, the cumulative deformation has reached 30%. Subsequent rolling is carried out automatically according to the model settings, and no side pressure is used throughout the rolling process.
[0070] After rolling, the plates were separated, and multiple flaw detection results in the head and tail 15m area showed unbonded areas.
[0071] Comparative Example 2 (Inappropriate pressure settings, failed) The rolling process for producing a 1.2mm TA2+10mm Q235 composite plate includes the following steps: S1. The design frame width is 50mm, and the compression ratio is 12. Based on the finished product thickness, the titanium plate thickness is determined to be 14.4mm, and the Q235 steel billet thickness is 120mm. The titanium plate length is 5500mm, and the reserved gap = min(50, 0.0072×5500+8.4) = min(50, 48)≈48mm. Therefore, the steel billet raw material length is 5500+50×2+2×48=5696mm. Both the titanium plate and the steel billet are machined to ensure straightness.
[0072] S2. After wiping the titanium plate clean with anhydrous ethanol, apply a release agent and let it air dry. The release agent coating thickness is 1.0 mm.
[0073] S3, according to Figure 2 As shown, the titanium middle plate is assembled according to the corner area. Figure 4 Four positioning titanium blocks are welded as shown. After the preform assembly is completed, the interior is subjected to vacuum treatment with a vacuum degree of 0.007 Pa.
[0074] S4. Heating temperature is 910℃.
[0075] S5, the reduction amounts for the first three passes are 16%, 20%, and 20%, respectively.
[0076] After rolling, the plates were separated, and multiple flaw detection results within a 30m range at the beginning and end showed that they were not bonded.
[0077] Comparative Example 3 (Location block missing, failure) The rolling process for producing a 1.2mm TA2+10mm Q235 composite plate includes the following steps: S1. The design frame width is 50mm, and the compression ratio is 12. Based on the finished product thickness, the titanium plate thickness is determined to be 14.4mm, and the Q235 steel billet thickness is 120mm. The titanium plate length is 5500mm, and the reserved gap = min(50, 0.0072×5500+8.4) = min(50, 48)≈48mm. Therefore, the steel billet raw material length is 5500+50×2+2×48=5696mm. Both the titanium plate and the steel billet are machined to ensure straightness.
[0078] S2. After wiping the titanium plate clean with anhydrous ethanol, apply a release agent and let it air dry. The release agent coating thickness is 1.0 mm.
[0079] S3, according to Figure 2 The assembly process was carried out as shown, but positioning of the titanium blocks was not prevented. After the assembly was completed, the interior was subjected to vacuum treatment with a vacuum degree of 0.007 Pa.
[0080] S4. Heating temperature is 910℃.
[0081] S5, the reduction amounts for the first three passes are 10%, 10%, and 12%, respectively.
[0082] After rolling, the plates were separated, and multiple flaw detection results within a 30m range at the tail end showed that they were not bonded.
[0083] like Figure 3 The diagram illustrates the simultaneous presence of a titanium-steel contact area and a non-contact area after rolling according to the present invention. This diagram is intended to explain that due to the differences in properties between titanium and steel, their elongation is inconsistent in the early stages of rolling. When the gap and reduction settings are not properly configured, the titanium plate deforms significantly but is constrained by the frame, resulting in… Figure 3 The stacking shown results in poor interface integration.
[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for producing rolled titanium-steel composite plates, characterized in that, Includes the following steps: S1. Raw material preparation: Prepare two titanium plates, two steel billets and frame, all of which are machined and leveled. S2. A release agent is coated on the surface of the titanium plate. S3, Billet Assembly: S31. Stack the steel billet, titanium plate, titanium plate, and steel billet symmetrically in the following order: steel billet-titanium plate-titanium plate-steel billet; S32. A frame is provided around the titanium middle plate, and a gap of Gmm is reserved between the inner side of the frame and the titanium middle plate. S33. Weld at least two titanium positioning blocks to the edges of both ends of the titanium plate. The positioning blocks are in contact with the inner side of the frame, and the welding position is within the finished product cutting edge range. Through the close contact between the positioning blocks and the inner side of the frame, the longitudinal movement of the titanium plate in the rolling direction is constrained, preventing it from sliding and accumulating in the billet cavity due to the difference in elongation rate. Ensure that the titanium plate always maintains a preset relative position with the billet, and avoid the exacerbation of wrinkled stacking in the head and tail areas due to displacement. S34. Set the border width; S4. Heat the assembled billet to 850-950℃; S5. Roll the heated composite billet: When the cumulative deformation is ≤30%, the deformation per pass shall be controlled within 15%; when the cumulative deformation is >30%, the conventional rolling procedure shall be followed. In S1, the thickness of the titanium plate and the steel billet is determined according to the compression ratio. The compression ratio is ≥10, and the length of the steel billet = the length of the titanium plate + the width of the frame × 2 + 2Gmm. In S32, the gap G between the titanium middle plate and the frame satisfies: G=min(50,max(25,0.0072L+8.4)), where L is the length of the titanium middle plate in mm; this gap design provides buffer space for the extension of the titanium layer and also reduces the constraint stress of the frame. In S34, the border width is 50mm.
2. The method for producing rolled titanium-steel composite plates according to claim 1, characterized in that, When L < 2300mm, G is taken as 25mm.
3. The method for producing rolled titanium-steel composite plates according to claim 1, characterized in that, In S5, when the cumulative deformation is ≤30%, the deformation per pass is within 10%.
Citation Information
Patent Citations
Production method of titanium-steel composite plate
CN109465309A
Assembly method of raw material blank of titanium steel composite plate
CN113020295A