Flame-retardant modified asphalt waterproofing coiled material and preparation method thereof

By utilizing the synergistic effect of styrene-butadiene-styrene copolymer, carbon nanotubes, and composite flame retardants, the flame-retardant modified bitumen waterproof membrane with a five-layer structure solves the problems of insufficient flame retardant and mechanical properties of modified bitumen waterproof membrane, achieving highly efficient flame retardant, waterproof, and aging-resistant effects.

CN120902385BActive Publication Date: 2026-11-24WEIFANG SHIHUA CHEM BUILDING MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511168433.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-08-20
Publication Date
2026-11-24
Estimated Expiration
2045-08-20

AI Technical Summary

Technical Problem

Existing modified bitumen waterproof membranes have shortcomings in terms of flame retardancy and mechanical properties. In particular, the inorganic flame retardants have poor compatibility and the organic flame retardants are prone to migration, resulting in poor flame retardancy, decreased mechanical properties, and weak aging resistance.

Method used

The flame-retardant modified bitumen waterproof membrane adopts a five-layer structure. By adding styrene-butadiene-styrene copolymer, carbon nanotubes, and composite flame retardants to the bitumen matrix, an interpenetrating network structure is formed. Inorganic flame retardants are treated with bio-based silane coupling agents to improve compatibility and dispersibility. Graphene forms a physical barrier layer, which synergistically enhances flame retardant and mechanical properties.

Benefits of technology

It improves the limiting oxygen index to 33.6-34.1%, tensile strength to 597-606 N/mm, elongation at break to 475-486%, tear strength to 181-187 N/mm, and seam peel strength to 3.76-3.93 N/mm. It also exhibits excellent aging resistance, significantly improved high-temperature stability, and enhanced waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a flame-retardant modified bitumen waterproof membrane and its preparation method, belonging to the technical field of waterproof membranes. The preparation method involves coating flame-retardant modified bitumen material onto both sides of a base layer to obtain an upper flame-retardant modified bitumen layer and a lower flame-retardant modified bitumen layer. The flame-retardant modified bitumen material is prepared by sequentially adding 70# bitumen, styrene-butadiene-styrene copolymer, naphthenic oil, carbon nanotubes, bitumen modifier, and composite flame retardant to a sealed container, stirring, and then adding naphthenic oil and isoflurane diisocyanate to obtain the flame-retardant modified bitumen material. The flame-retardant modified bitumen waterproof membrane obtained by this invention improves flame-retardant performance while ensuring mechanical properties, exhibiting excellent waterproof performance and good aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of waterproof membrane technology, specifically relating to a flame-retardant modified bitumen waterproof membrane and its preparation method. Background Technology

[0002] Waterproof membranes are mainly used in building walls, roofs, tunnels, highways, landfills, etc. They are flexible building materials that can be rolled up to resist external rainwater and groundwater seepage. As a leak-proof connection between the foundation and the building, waterproof membranes are the first line of defense for waterproofing the entire project and play a vital role in the overall project.

[0003] Currently, waterproof membranes mainly include modified bitumen waterproof membranes, self-adhesive waterproof membranes, and polymer waterproof membranes, among which modified bitumen waterproof membranes are widely used due to their good flexibility, weather resistance, and waterproof performance. However, asphalt itself is a flammable material. During combustion, asphalt will first melt, drip, and flow, and then the molten beads will start to burn. The burning molten beads will continue to drip and flow, causing the fire to spread rapidly. In addition, asphalt releases a large amount of toxic gases when burning, which will fuel the fire and produce a lot of smoke, making the fire difficult to extinguish. Therefore, it is of great significance to study modified asphalt waterproof membranes with excellent flame retardant properties.

[0004] Existing technologies for preparing flame-retardant modified bitumen waterproof membranes typically involve adding flame retardants. Common flame retardants include inorganic and organic flame retardants. Inorganic flame retardants include aluminum hydroxide and magnesium hydroxide, while organic flame retardants include halogenated and nitrogen-based flame retardants. However, this approach presents the following problems: Inorganic flame retardants have poor compatibility with asphalt, and phase separation is likely to occur during the preparation and use process, which will reduce the tensile strength and other mechanical properties of the waterproof membrane. Furthermore, the flame retardant effect is limited due to the single flame retardant mechanism. Although organic flame retardants have relatively good compatibility with asphalt matrix, they are prone to migration. Over time, the flame retardants will migrate from the asphalt, thereby reducing the flame retardant performance of the waterproof membrane and failing to meet the requirement of long-term flame retardant effect.

[0005] CN118496779A discloses a flame-retardant asphalt-based waterproof membrane. The preparation steps of the flame-retardant asphalt-based waterproof membrane are as follows: heating asphalt to 190-200℃, adding aromatic oil and stirring evenly, then cooling to 180-190℃, adding styrene-butadiene-styrene block copolymer, heating to 190-200℃ and stirring, adding tackifying resin and waste rubber powder, keeping warm and stirring, then adding modified hexagonal boron nitride, continuing to keep warm and stirring to obtain a mixture; the mixture is melted and extruded, pressed into sheets, and then cooled, trimmed, drawn, and wound to obtain the flame-retardant asphalt-based waterproof membrane; wherein, the modified hexagonal boron nitride is obtained by surface treatment of boron nitride with silane coupling agent kH550 and phytic acid, and then obtaining titanium dioxide by chemical reaction of ammonium hexafluorotitanate and boric acid, which adheres to the surface of boron nitride through chelation, which can improve flame retardant performance and reduce smoke generated during combustion.

[0006] This waterproof membrane has excellent flame retardant properties, high peel strength, and certain anti-fouling and bactericidal effects. Its oxygen index is 28-31%, and its peel strength is 2.3-2.5 N / mm. However, its oxygen index is still relatively low, and its mechanical properties such as tensile strength are poor, as is its aging resistance. Summary of the Invention

[0007] To address the technical problems existing in the prior art, this invention provides a flame-retardant modified bitumen waterproof membrane that improves flame retardancy while ensuring mechanical properties, enhancing waterproof performance, and improving the aging resistance of the waterproof membrane.

[0008] This invention provides a flame-retardant modified bitumen waterproof membrane and its preparation method, as detailed below: A method for preparing a flame-retardant modified bitumen waterproof membrane is as follows: flame-retardant modified bitumen material is coated on both sides of a base layer to obtain an upper flame-retardant modified bitumen layer and a lower flame-retardant modified bitumen layer; polyethylene film is covered on both sides of the flame-retardant modified bitumen layer to obtain an upper protective layer and a lower protective layer; and the flame-retardant modified bitumen waterproof membrane is obtained by hot pressing and cooling. The flame-retardant modified bitumen waterproof membrane has the following structure from top to bottom: upper protective layer, upper flame-retardant modified bitumen layer, base layer, lower flame-retardant modified bitumen layer, and lower protective layer. The base layer is made of polyester fiber nonwoven fabric with a thickness of 0.20-0.25mm; The coating thickness of the flame-retardant modified asphalt material is 1.2-1.4 mm; The thickness of the polyethylene film is 0.18-0.23 mm.

[0009] The preparation method of the flame-retardant modified asphalt material is as follows: 70# asphalt is added to a sealed container, the temperature is raised to 162-167℃, and the mixture is stirred at 280-310 rpm for 27-32 min. Then, styrene-butadiene-styrene copolymer is added, the temperature is raised to 175-180℃, and the mixture is sheared and dispersed at 2000-2300 rpm for 18-22 min. Naphthenic oil is added for the first time, and shearing and dispersion continues for 23-27 min. Finally, carbon nanotubes are added, and the temperature is lowered to 168℃. Stir at -172℃ and 1100-1300rpm for 37-45min, then lower the temperature to 140-144℃, add asphalt modifier, stir at 610-640rpm for 38-45min, add composite flame retardant, keep warm and stir for 32-40min, add naphthenic oil for the second time, keep warm and stir for 27-32min, and finally add isoflurane diisocyanate, stir at 128-133℃ for 38-43min to obtain flame-retardant modified asphalt material; The carbon nanotubes have a particle size of 80-110 nm; The mass ratio of the 70# asphalt, styrene-butadiene-styrene copolymer, naphthenic oil (first addition), carbon nanotubes, asphalt modifier, composite flame retardant, naphthenic oil (second addition), and isoflurane diisocyanate is 100:4.0-4.5:1.8-2.2:4.8-5.3:8.7-9.2:6.2-6.7:1.8-2.2:2.4-2.6.

[0010] The preparation method of the asphalt modifier is as follows: epoxidized soybean oil is added to a sealed container, followed by methyltetrahydrophthalic anhydride. After stirring evenly, tetrabutylammonium bromide is added under a nitrogen atmosphere while stirring. The stirring speed is 280-310 rpm. After the addition is completed, the temperature is raised to 82-87℃, and the mixture is stirred at 460-510 rpm for 78-83 minutes. After the reaction is completed, the mixture is cooled and filtered to obtain the asphalt modifier. The mass ratio of the epoxidized soybean oil, methyltetrahydrophthalic anhydride, and tetrabutylammonium bromide is 18-23:3.7-4.0:0.10-0.14.

[0011] The preparation method of the composite flame retardant includes mixing and compounding steps; The mixing step is as follows: magnesium hydroxide and ammonium polyphosphate are added to anhydrous ethanol, the temperature is raised to 48-52°C, and the mixture is stirred for 27-32 minutes. Then, a bio-based silane coupling agent is added, and the mixture is kept warm and stirred for 58-65 minutes to obtain a flame retardant. The mass ratio of magnesium hydroxide, ammonium polyphosphate, anhydrous ethanol, and bio-based silane coupling agent is 4.0-4.4:6.0-6.5:100:1.5-1.8.

[0012] The composite step involves adding deionized water to graphene, performing ultrasonic dispersion, controlling the ultrasonic power at 360-380W, the ultrasonic frequency at 27-32kHz, and the ultrasonic time at 25-35min. After ultrasonication, a flame retardant is added, the temperature is raised to 48-52℃, and the mixture is stirred at 670-720rpm for 1.8-2.2h. The temperature is then raised to 70-75℃, and the temperature of the maleic anhydride-grafted polyethylene solution is lowered to 70-75℃. The maleic anhydride-grafted polyethylene solution is then added, and the mixture is stirred at 240-260rpm for 1.0-1.3h to obtain the composite flame retardant. The mass ratio of graphene, deionized water, flame retardant, and maleic anhydride-grafted polyethylene solution is 6.2-6.5:68-75:10.2-10.7:3.0-3.4. The maleic anhydride-grafted polyethylene solution is a mixture of maleic anhydride-grafted polyethylene and xylene at 112-117°C, wherein the mass ratio of maleic anhydride-grafted polyethylene to xylene is 5.5:24.5-28.5. The maleic anhydride-grafted polyethylene has a melt index of 10-13 g / 10 min at 180°C and 2.16 kg.

[0013] The preparation method of the bio-based silane coupling agent is as follows: ricinoleic acid and γ-aminopropyltriethoxysilane are added to a sealed container, and the mixture is stirred at 330-370 rpm for 13-20 min under nitrogen protection. Then, aminosulfonic acid is added, and the temperature is increased to 78-82℃ at a rate of 1.8-2.2℃ / min. The mixture is stirred at this temperature for 18-25 min, and then the temperature is increased to 102-107℃ at a rate of 0.8-1.2℃ / min. The mixture is kept at this temperature for 1.7-2.2 h. After the reaction is completed, the mixture is filtered, washed, and dried to obtain the bio-based silane coupling agent. The mass ratio of castor oil acid, γ-aminopropyltriethoxysilane, and aminosulfonic acid is 8.2-8.6:3.8-4.2:0.13-0.16.

[0014] A flame-retardant modified bitumen waterproof membrane is prepared by the aforementioned method.

[0015] The flame-retardant modified bitumen waterproof membrane of this invention has a five-layer structure. Through the synergistic effect between the components, it improves flame retardancy while ensuring mechanical properties, enhancing waterproof performance and aging resistance. The main components are the upper and lower flame-retardant modified bitumen layers, formed by flame-retardant modified bitumen material. This material uses 70# bitumen as the matrix, and by adding styrene-butadiene-styrene copolymer, both rigid and flexible structures are introduced. This enhances high-temperature resistance while ensuring low-temperature flexibility. The bitumen modifier has good compatibility with the bitumen system, further optimizing the balance between flexible and rigid segments. The synergistic composite flame retardant ensures its dispersion performance in the bitumen system. The addition of naphthenic oil twice effectively adjusts the viscosity of the system. Isocyanate can firmly bond with bitumen, constructing a cross-linked network, enhancing waterproof performance, and improving both the flame retardant properties and mechanical properties and high-temperature stability of the flame-retardant modified bitumen material.

[0016] Specifically, the asphalt modifier uses epoxidized soybean oil and methyltetrahydrophthalic anhydride, which are combined under the action of tetrabutylammonium bromide to introduce flexible long chains to enhance low-temperature flexibility. Furthermore, the anhydride, as a rigid structure, can improve high-temperature stability. It has good compatibility with styrene-butadiene-styrene copolymer, promotes the formation of interpenetrating network structure, and enhances aging resistance. Specifically, the composite flame retardant uses magnesium hydroxide and ammonium polyphosphate as a blend, treated with a bio-based organosilane coupling agent, and then combined with graphene. In the mixing step, a bio-based silane coupling agent is used to combine with the flame retardant components. The bio-based silane coupling agent is made from aminosilane coupling agent and castor oil acid, which are chemically combined under catalysis. The resulting bio-based silane coupling agent acts as a bridging agent, enhancing the compatibility of magnesium hydroxide, ammonium polyphosphate, etc., with asphalt and improving their dispersibility in the asphalt system. This improves both flame retardant performance and mechanical properties. In the composite step, the layered structure of graphene forms a physical barrier layer, effectively enhancing its flame retardant properties. Combined with maleic anhydride-grafted polyethylene, the maleic anhydride binds to the hydroxyl groups of graphene. The polyethylene segments have good compatibility with asphalt, further enhancing their dispersibility in the asphalt system. The final composite flame retardant forms a multi-layered flame retardant system that not only enhances flame retardant performance but also improves mechanical and stability properties.

[0017] Compared with the prior art, the present invention has achieved the following beneficial effects: 1. The flame-retardant modified bitumen waterproof membrane prepared by this invention has a water-facing pressure controlled at 0.2 MPa for 2 hours, with each additional 0.01 MPa pressurized for 30 minutes. Water permeability occurs at 0.64-0.67 MPa. 2. The flame-retardant modified bitumen waterproof membrane prepared by this invention has a limiting oxygen index of 33.6-34.1%; 3. The flame-retardant modified bitumen waterproof membrane prepared by this invention has a tensile strength of 597-606 N / mm, an elongation at break of 475-486%, a tear strength of 181-187 N, a seam peel strength of 3.76-3.93 N / mm, and does not flow or drip when kept at 118-123℃ for 2.0 h, and shows no cracks at -32.0~-33.4℃. 4. The flame-retardant modified bitumen waterproof membrane prepared by this invention was left to stand for 10 days in an environment with a temperature of 70℃ and a humidity of 65%, and then subjected to ultraviolet irradiation with an intensity of 0.8W / cm2 and a temperature of 40℃ for 10 days. After irradiation, the tensile strength was measured to be 572-584N / mm, the elongation at break was 456-471%, the tear strength was 173-180N, the seam peel strength was 3.58-3.76N / mm, and there were no cracks at -30.3~-31.9℃. Detailed Implementation

[0018] To provide a clearer understanding of the technical features, objectives, and effects of the present invention, specific embodiments of the present invention are now described.

[0019] Example 1 A method for preparing a flame-retardant modified bitumen waterproof membrane is as follows: flame-retardant modified bitumen material is coated on both sides of a base layer to obtain an upper flame-retardant modified bitumen layer and a lower flame-retardant modified bitumen layer; polyethylene film is covered on both sides of the flame-retardant modified bitumen layer to obtain an upper protective layer and a lower protective layer; and the flame-retardant modified bitumen waterproof membrane is obtained by hot pressing and cooling. The flame-retardant modified bitumen waterproof membrane has the following structure from top to bottom: upper protective layer, upper flame-retardant modified bitumen layer, base layer, lower flame-retardant modified bitumen layer, and lower protective layer. The base layer is made of polyester fiber nonwoven fabric with a thickness of 0.20 mm; The coating thickness of the flame-retardant modified asphalt material is 1.2 mm; The polyethylene film has a thickness of 0.18 mm.

[0020] The method for preparing the flame-retardant modified asphalt is as follows: 100g of 70# asphalt is added to a sealed container, the temperature is raised to 162℃, and the mixture is stirred at 280rpm for 27min. Then, 4.0g of styrene-butadiene-styrene copolymer is added, the temperature is raised to 175℃, and the mixture is sheared and dispersed at 2000rpm for 22min. Then, 1.8g of naphthenic oil is added, and the mixture is sheared and dispersed for another 23min. Then, 4.8g of carbon nanotubes is added, the temperature is lowered to 168℃, and the mixture is stirred at 1100rpm for 45min. Then, the temperature is lowered to 140℃, 8.7g of asphalt modifier is added, and the mixture is stirred at 610rpm for 45min. Then, 6.2g of composite flame retardant is added, and the mixture is kept warm and stirred for 40min. Then, 1.8g of naphthenic oil is added, and the mixture is kept warm and stirred for 32min. Finally, 2.4g of isoflurane diisocyanate is added, and the mixture is stirred at 128℃ for 43min to obtain the flame-retardant modified asphalt. The carbon nanotubes have a particle size of 80 nm.

[0021] The preparation method of the asphalt modifier is as follows: 18g of epoxidized soybean oil is added to a sealed container, followed by 3.7g of methyltetrahydrophthalic anhydride. After stirring evenly, 0.10g of tetrabutylammonium bromide is added under a nitrogen atmosphere while stirring. The stirring speed is 280rpm. After the addition is completed, the temperature is raised to 82℃, and the mixture is stirred at 460rpm for 78min. After the reaction is completed, the mixture is cooled and filtered to obtain the asphalt modifier.

[0022] The preparation method of the composite flame retardant includes mixing and compounding steps; The mixing step is as follows: 4.0g magnesium hydroxide and 6.0g ammonium polyphosphate are added to 100g anhydrous ethanol, the temperature is raised to 48°C, and the mixture is stirred for 32 minutes. Then, 1.5g bio-based silane coupling agent is added, and the mixture is kept warm and stirred for 65 minutes to obtain the flame retardant. The composite step is as follows: 68g of deionized water is added to 6.2g of graphene, and ultrasonic dispersion is performed. The ultrasonic power is controlled at 360W, the ultrasonic frequency at 32kHz, and the ultrasonic time at 35min. After ultrasonication, 10.2g of flame retardant is added, the temperature is raised to 48℃, and the mixture is stirred at 670rpm for 2.2h. The temperature is then raised to 70℃, and the temperature of the maleic anhydride-grafted polyethylene solution is lowered to 70℃. 3.0g of maleic anhydride-grafted polyethylene solution is added, and the mixture is stirred at 240rpm for 1.3h to obtain the composite flame retardant. The maleic anhydride-grafted polyethylene solution is a mixture of maleic anhydride-grafted polyethylene and xylene at 112°C, wherein the mass ratio of maleic anhydride-grafted polyethylene to xylene is 5.5:24.5. The maleic anhydride-grafted polyethylene has a melt index of 10 g / 10 min at 180°C and 2.16 kg. The preparation method of the bio-based silane coupling agent is as follows: 8.2g of castor oil acid and 3.8g of γ-aminopropyltriethoxysilane are added to a sealed container. Under nitrogen protection, the mixture is stirred at 330rpm for 20min. Then, 0.13g of aminosulfonic acid is added, and the temperature is increased to 78℃ at a rate of 1.8℃ / min. The mixture is stirred at this temperature for 25min. Then, the temperature is increased to 102℃ at a rate of 0.8℃ / min. The mixture is stirred at this temperature for 2.2h. After the reaction is completed, the mixture is filtered, washed, and dried to obtain the bio-based silane coupling agent.

[0023] Example 2 A method for preparing a flame-retardant modified bitumen waterproof membrane is as follows: flame-retardant modified bitumen material is coated on both sides of a base layer to obtain an upper flame-retardant modified bitumen layer and a lower flame-retardant modified bitumen layer; polyethylene film is covered on both sides of the flame-retardant modified bitumen layer to obtain an upper protective layer and a lower protective layer; and the flame-retardant modified bitumen waterproof membrane is obtained by hot pressing and cooling. The flame-retardant modified bitumen waterproof membrane has the following structure from top to bottom: upper protective layer, upper flame-retardant modified bitumen layer, base layer, lower flame-retardant modified bitumen layer, and lower protective layer. The base layer is made of polyester fiber nonwoven fabric with a thickness of 0.22mm; The coating thickness of the flame-retardant modified asphalt material is 1.3 mm; The polyethylene film has a thickness of 0.20 mm.

[0024] The method for preparing the flame-retardant modified asphalt is as follows: 100g of 70# asphalt is added to a sealed container, the temperature is raised to 165℃, and the mixture is stirred at 300rpm for 30min. Then, 4.2g of styrene-butadiene-styrene copolymer is added, the temperature is raised to 178℃, and the mixture is sheared and dispersed at 2200rpm for 20min. Then, 2.0g of naphthenic oil is added, and the mixture is sheared and dispersed for another 25min. Then, 5.0g of carbon nanotubes is added, the temperature is lowered to 170℃, and the mixture is stirred at 1200rpm for 40min. Then, the temperature is lowered to 142℃, 9.0g of asphalt modifier is added, and the mixture is stirred at 620rpm for 40min. Then, 6.5g of composite flame retardant is added, and the mixture is kept warm and stirred for 35min. Then, 2.0g of naphthenic oil is added, and the mixture is kept warm and stirred for 30min. Finally, 2.5g of isoflurane diisocyanate is added, and the mixture is stirred at 132℃ for 40min to obtain the flame-retardant modified asphalt. The carbon nanotubes have a particle size of 100 nm.

[0025] The preparation method of the asphalt modifier is as follows: 20g of epoxidized soybean oil is added to a sealed container, followed by 3.8g of methyltetrahydrophthalic anhydride. After stirring evenly, 0.12g of tetrabutylammonium bromide is added under a nitrogen atmosphere while stirring. The stirring speed is 300rpm. After the addition is completed, the temperature is raised to 85℃, and the mixture is stirred at 500rpm for 80min. After the reaction is completed, the mixture is cooled and filtered to obtain the asphalt modifier.

[0026] The preparation method of the composite flame retardant includes mixing and compounding steps; The mixing step is as follows: 4.1g of magnesium hydroxide and 6.3g of ammonium polyphosphate are added to 100g of anhydrous ethanol, the temperature is raised to 50°C, and the mixture is stirred for 30 minutes. Then, 1.7g of bio-based silane coupling agent is added, and the mixture is kept warm and stirred for 60 minutes to obtain the flame retardant. The composite step is as follows: 70g of deionized water is added to 6.4g of graphene, and ultrasonic dispersion is performed. The ultrasonic power is controlled at 370W, the ultrasonic frequency at 30kHz, and the ultrasonic time at 30min. After ultrasonication, 10.5g of flame retardant is added, the temperature is raised to 50℃, and the mixture is stirred at 700rpm for 2.0h. The temperature is then raised to 72℃, and the temperature of the maleic anhydride-grafted polyethylene solution is lowered to 72℃. 3.3g of maleic anhydride-grafted polyethylene solution is added, and the mixture is stirred at 250rpm for 1.2h to obtain the composite flame retardant. The maleic anhydride-grafted polyethylene solution is a mixture of maleic anhydride-grafted polyethylene and xylene at 115°C, wherein the mass ratio of maleic anhydride-grafted polyethylene to xylene is 5.5:27.5. The maleic anhydride-grafted polyethylene has a melt index of 12 g / 10 min at 180°C and 2.16 kg. The preparation method of the bio-based silane coupling agent is as follows: 8.3g of castor oil acid and 4.0g of γ-aminopropyltriethoxysilane are added to a sealed container. Under nitrogen protection, the mixture is stirred at 350rpm for 15min. Then, 0.15g of aminosulfonic acid is added, and the temperature is increased to 80℃ at 2.0℃ / min. The mixture is stirred at this temperature for 20min. Then, the temperature is increased to 105℃ at a rate of 1.0℃ / min. The mixture is kept at this temperature for 2.0h. After the reaction is completed, the mixture is filtered, washed, and dried to obtain the bio-based silane coupling agent.

[0027] Example 3 A method for preparing a flame-retardant modified bitumen waterproof membrane is as follows: flame-retardant modified bitumen material is coated on both sides of a base layer to obtain an upper flame-retardant modified bitumen layer and a lower flame-retardant modified bitumen layer; polyethylene film is covered on both sides of the flame-retardant modified bitumen layer to obtain an upper protective layer and a lower protective layer; and the flame-retardant modified bitumen waterproof membrane is obtained by hot pressing and cooling. The flame-retardant modified bitumen waterproof membrane has the following structure from top to bottom: upper protective layer, upper flame-retardant modified bitumen layer, base layer, lower flame-retardant modified bitumen layer, and lower protective layer. The base layer is made of polyester fiber nonwoven fabric with a thickness of 0.25mm; The coating thickness of the flame-retardant modified asphalt material is 1.4 mm; The polyethylene film has a thickness of 0.23 mm.

[0028] The method for preparing the flame-retardant modified asphalt is as follows: 100g of 70# asphalt is added to a sealed container, the temperature is raised to 167℃, and the mixture is stirred at 310rpm for 32min. Then, 4.5g of styrene-butadiene-styrene copolymer is added, the temperature is raised to 180℃, and the mixture is sheared and dispersed at 2300rpm for 18min. Then, 2.2g of naphthenic oil is added, and the mixture is sheared and dispersed for another 27min. Then, 5.3g of carbon nanotubes is added, the temperature is lowered to 172℃, and the mixture is stirred at 1300rpm for 37min. Then, the temperature is lowered to 144℃, 9.2g of asphalt modifier is added, and the mixture is stirred at 640rpm for 38min. Then, 6.7g of composite flame retardant is added, and the mixture is kept warm and stirred for 32min. Then, 2.2g of naphthenic oil is added, and the mixture is kept warm and stirred for 27min. Finally, 2.6g of isoflurane diisocyanate is added, and the mixture is stirred at 133℃ for 38min to obtain the flame-retardant modified asphalt. The carbon nanotubes have a particle size of 110 nm.

[0029] The preparation method of the asphalt modifier is as follows: 23g of epoxidized soybean oil is added to a sealed container, followed by 4.0g of methyltetrahydrophthalic anhydride. After stirring evenly, 0.14g of tetrabutylammonium bromide is added under a nitrogen atmosphere while stirring. The stirring speed is 310rpm. After the addition is completed, the temperature is raised to 87℃, and the mixture is stirred at 510rpm for 83min. After the reaction is completed, the mixture is cooled and filtered to obtain the asphalt modifier.

[0030] The preparation method of the composite flame retardant includes mixing and compounding steps; The mixing step is as follows: 4.4g of magnesium hydroxide and 6.5g of ammonium polyphosphate are added to 100g of anhydrous ethanol, the temperature is raised to 52°C, and the mixture is stirred for 27 minutes. Then, 1.8g of bio-based silane coupling agent is added, and the mixture is kept warm and stirred for 58 minutes to obtain the flame retardant. The composite step is as follows: 74g of deionized water is added to 6.5g of graphene, and ultrasonic dispersion is performed. The ultrasonic power is controlled at 380W, the ultrasonic frequency at 27kHz, and the ultrasonic time at 25min. After ultrasonication, 10.7g of flame retardant is added, the temperature is raised to 52℃, and the mixture is stirred at 720rpm for 1.8h. The temperature is then raised to 75℃, and the temperature of the maleic anhydride-grafted polyethylene solution is lowered to 75℃. 3.4g of maleic anhydride-grafted polyethylene solution is added, and the mixture is stirred at 260rpm for 1.0h to obtain the composite flame retardant. The maleic anhydride-grafted polyethylene solution is a mixture of maleic anhydride-grafted polyethylene and xylene at 117°C, wherein the mass ratio of maleic anhydride-grafted polyethylene to xylene is 5.5:28.5. The maleic anhydride-grafted polyethylene has a melt index of 13 g / 10 min at 180°C and 2.16 kg. The preparation method of the bio-based silane coupling agent is as follows: 8.6g of castor oil acid and 4.2g of γ-aminopropyltriethoxysilane are added to a sealed container. Under nitrogen protection, the mixture is stirred at 370rpm for 13min. Then, 0.16g of aminosulfonic acid is added, and the temperature is increased to 82℃ at a rate of 2.2℃ / min. The mixture is stirred at this temperature for 25min. Then, the temperature is increased to 107℃ at a rate of 1.2℃ / min. The mixture is stirred at this temperature for 1.7h. After the reaction is completed, the mixture is filtered, washed, and dried to obtain the bio-based silane coupling agent.

[0031] Comparative Example 2-1 Based on Example 2, the following changes were made: 1. In the preparation method of the composite flame retardant, the preparation of the bio-based silane coupling agent is omitted, and the bio-based silane coupling agent is replaced by an equal amount of γ-aminopropyltriethoxysilane; 2. The preparation method of the asphalt modifier is omitted, and the asphalt modifier is replaced with an equal amount of epoxidized soybean oil; The rest of the operations are exactly the same.

[0032] Comparative Example 2-2 Based on Example 2, the following changes were made: 1. In the preparation method of flame-retardant modified asphalt, the operation step of "adding 2.5g of isoflurane diisocyanate and stirring at 132℃ for 40min" is omitted; and the operation step of "adding 2.0g of naphthenic oil and stirring at the temperature for 30min" is omitted, and the amount of naphthenic oil added for the first time is modified to 4.0g. 2. In the composite step of the preparation method of composite flame retardant, the operation step of "then add 3.3g of maleic anhydride grafted polyethylene solution, raise the temperature to 75℃, and stir at 250rpm for 1.2h" is omitted. The rest of the operations are exactly the same.

[0033] Test 1. Waterproof performance The flame-retardant modified bitumen waterproof membranes prepared in Examples 1-3, Comparative Examples 2-1, and 2-2 were tested for waterproof performance according to the method in GB / T23457-2009. The pressure on the water-facing side of the waterproof membrane was controlled at 0.2 MPa and maintained for 2 hours. The pressure was increased by 0.01 MPa and maintained for 30 minutes at a time until water permeation occurred. The pressure at the time of water permeation was recorded. The results are as follows:

[0034] 2. Flame retardant properties The flame-retardant modified bitumen waterproof membranes prepared in Examples 1-3, Comparative Example 2-1, and Comparative Example 2-2 were tested for their limiting oxygen index according to the methods in GB18242-2008 "Elastomer Modified Bitumen Waterproof Membranes" and GB / T2408-2021 "Determination of Burning Performance of Plastics - Horizontal and Vertical Methods". The test results are as follows:

[0035] 3. Physical properties The flame-retardant modified bitumen waterproof membranes prepared in Examples 1-3, Comparative Examples 2-1, and Comparative Examples 2-2 were tested for tensile properties, tear strength, seam peel strength, heat resistance, and low-temperature flexibility according to GB / T328-2007 "Test Methods for Building Waterproof Membranes". The test results are as follows:

[0036] 4. Aging resistance The flame-retardant modified bitumen waterproof membranes prepared in Examples 1-3, Comparative Examples 2-1, and Comparative Examples 2-2 were placed in an environment with a temperature of 70°C and a humidity of 65% for 10 days, and then subjected to ultraviolet irradiation at an intensity of 0.8 W / cm² and a temperature of 40°C for 10 days. After irradiation, the tensile properties, tear strength, seam peel strength, and low-temperature flexibility were tested according to GB / T 328-2007 "Test Methods for Waterproof Membranes for Buildings". The test results are as follows:

[0037] The flame-retardant modified bitumen waterproof membrane of this invention has a five-layer structure. Through the synergistic effect between the components, it improves flame retardancy while ensuring mechanical properties, enhancing waterproof performance and aging resistance. The main components are the upper and lower flame-retardant modified bitumen layers, formed by flame-retardant modified bitumen material. This material uses 70# bitumen as the matrix, and by adding styrene-butadiene-styrene copolymer, both rigid and flexible structures are introduced. This enhances high-temperature resistance while ensuring low-temperature flexibility. The bitumen modifier has good compatibility with the bitumen system, further optimizing the balance between flexible and rigid segments. The synergistic composite flame retardant ensures its dispersion performance in the bitumen system. The addition of naphthenic oil twice effectively adjusts the viscosity of the system. Isocyanate can firmly bond with bitumen, constructing a cross-linked network, enhancing waterproof performance, and improving both the flame retardant properties and mechanical properties and high-temperature stability of the flame-retardant modified bitumen material.

[0038] Specifically, the asphalt modifier uses epoxidized soybean oil and methyltetrahydrophthalic anhydride, which are combined under the action of tetrabutylammonium bromide to introduce flexible long chains to enhance low-temperature flexibility. Furthermore, the anhydride, as a rigid structure, can improve high-temperature stability. It has good compatibility with styrene-butadiene-styrene copolymer, promotes the formation of interpenetrating network structure, and enhances aging resistance. Specifically, the composite flame retardant uses magnesium hydroxide and ammonium polyphosphate as a blend, treated with a bio-based organosilane coupling agent, and then combined with graphene. In the mixing step, a bio-based silane coupling agent is used to combine with the flame retardant components. The bio-based silane coupling agent is made from aminosilane coupling agent and castor oil acid, which are chemically combined under catalysis. The resulting bio-based silane coupling agent acts as a bridging agent, enhancing the compatibility of magnesium hydroxide, ammonium polyphosphate, etc., with asphalt and improving their dispersibility in the asphalt system. This improves both flame retardant performance and mechanical properties. In the composite step, the layered structure of graphene forms a physical barrier layer, effectively enhancing its flame retardant properties. Combined with maleic anhydride-grafted polyethylene, the maleic anhydride binds to the hydroxyl groups of graphene. The polyethylene segments have good compatibility with asphalt, further enhancing their dispersibility in the asphalt system. The final composite flame retardant forms a multi-layered flame retardant system that not only enhances flame retardant performance but also improves mechanical and stability properties.

[0039] Comparative Example 2-1 directly used γ-aminopropyltriethoxysilane as a silane coupling agent to treat magnesium hydroxide and ammonium polyphosphate. However, when modifying asphalt, only epoxidized soybean oil was used as the asphalt modifier. The silane coupling agent treatment effect was poor, resulting in poor dispersion in the asphalt system, which in turn affected flame retardancy and mechanical properties, and reduced aging resistance. Comparative Example 2-2 omitted isoflurone diisocyanate in the preparation of the flame-retardant modified asphalt material and added naphthenic oil in one step, failing to fully utilize its viscosity adjustment function. This led to uneven dispersion of the asphalt system and the inability to achieve a cross-linked network, reducing the mechanical properties, heat resistance, and aging resistance of the waterproof membrane. Furthermore, the omission of maleic anhydride-grafted polyethylene in the preparation method of the composite flame retardant further reduced the overall performance of the waterproof membrane.

[0040] Unless otherwise specified, all proportions mentioned in this invention are mass proportions, and all percentages are mass percentages.

[0041] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a flame-retardant modified bitumen waterproof membrane, characterized in that, Flame-retardant modified asphalt material is coated on both sides of the base course to obtain an upper flame-retardant modified asphalt layer and a lower flame-retardant modified asphalt layer. The method for preparing the flame-retardant modified asphalt material is as follows: 70# asphalt, styrene-butadiene-styrene copolymer, naphthenic oil, carbon nanotubes, asphalt modifier, and composite flame retardant are added sequentially to a sealed container. After stirring, naphthenic oil and isoflurane diisocyanate are added to obtain the flame-retardant modified asphalt material. The preparation method of the asphalt modifier is as follows: methyltetrahydrophthalic anhydride is added to epoxidized soybean oil, tetrabutylammonium bromide is added under a nitrogen atmosphere, and the mixture is stirred at 82-87℃ and 460-510 rpm for 78-83 min to obtain the asphalt modifier. The preparation method of the composite flame retardant includes mixing and compounding steps; The mixing step involves adding magnesium hydroxide and ammonium polyphosphate to anhydrous ethanol, heating to 48-52°C, and adding a bio-based silane coupling agent to obtain a flame retardant. The preparation method of the bio-based silane coupling agent is as follows: ricinoleic acid and γ-aminopropyltriethoxysilane are mixed, aminosulfonic acid is added under nitrogen protection, the mixture is stirred at 78-82℃ for 18-25 min, and kept at 102-107℃ for 1.7-2.2 h to obtain the bio-based silane coupling agent. The composite step is as follows: deionized water is added to graphene, ultrasonic dispersion is performed, flame retardant is added, and stirring is carried out at 48-52℃ and 670-720rpm for 1.8-2.2h. The temperature is raised to 70-75℃, maleic anhydride-grafted polyethylene solution is added, and stirring is carried out at 240-260rpm for 1.0-1.3h to obtain composite flame retardant.

2. The method for preparing a flame-retardant modified bitumen waterproof membrane according to claim 1, characterized in that, The preparation method of the flame-retardant modified asphalt material is as follows: 70# asphalt is added to a sealed container, the temperature is raised to 162-167℃, and the mixture is stirred at 280-310 rpm for 27-32 min. Then, styrene-butadiene-styrene copolymer is added, the temperature is raised to 175-180℃, and the mixture is sheared and dispersed at 2000-2300 rpm for 18-22 min. Naphthenic oil is added for the first time, and shearing and dispersion continues for 23-27 min. Finally, carbon nanotubes are added, and the temperature is lowered to 168℃. Stir at -172℃ and 1100-1300rpm for 37-45min, then lower the temperature to 140-144℃, add asphalt modifier, stir at 610-640rpm for 38-45min, add composite flame retardant, keep warm and stir for 32-40min, add naphthenic oil for the second time, keep warm and stir for 27-32min, and finally add isoflurane diisocyanate, stir at 128-133℃ for 38-43min to obtain flame-retardant modified asphalt material; The carbon nanotubes have a particle size of 80-110 nm; The mass ratio of the 70# asphalt, styrene-butadiene-styrene copolymer, naphthenic oil (first addition), carbon nanotubes, asphalt modifier, composite flame retardant, naphthenic oil (second addition), and isoflurane diisocyanate is 100:4.0-4.5:1.8-2.2:4.8-5.3:8.7-9.2:6.2-6.7:1.8-2.2:2.4-2.

6.

3. The method for preparing a flame-retardant modified bitumen waterproof membrane according to claim 1, characterized in that, In the preparation method of the asphalt modifier, the mass ratio of epoxidized soybean oil, methyltetrahydrophthalic anhydride, and tetrabutylammonium bromide is 18-23:3.7-4.0:0.10-0.

14.

4. The method for preparing a flame-retardant modified bitumen waterproof membrane according to claim 1, characterized in that, In the mixing step, the mass ratio of magnesium hydroxide, ammonium polyphosphate, anhydrous ethanol and bio-based silane coupling agent is 4.0-4.4:6.0-6.5:100:1.5-1.

8.

5. The method for preparing a flame-retardant modified bitumen waterproof membrane according to claim 1, characterized in that, In the composite step, the ultrasonic dispersion has an ultrasonic power of 360-380W, an ultrasonic frequency of 27-32kHz, and an ultrasonic time of 25-35min. The mass ratio of graphene, deionized water, flame retardant, and maleic anhydride-grafted polyethylene solution is 6.2-6.5:68-75:10.2-10.7:3.0-3.

4. The maleic anhydride-grafted polyethylene solution is a mixture of maleic anhydride-grafted polyethylene and xylene at 112-117°C, wherein the mass ratio of maleic anhydride-grafted polyethylene to xylene is 5.5:24.5-28.

5. The maleic anhydride-grafted polyethylene has a melt index of 10-13 g / 10 min at 180°C and 2.16 kg.

6. The method for preparing a flame-retardant modified bitumen waterproof membrane according to claim 1, characterized in that, In the preparation method of the bio-based silane coupling agent, the mass ratio of castor oil acid, γ-aminopropyltriethoxysilane, and aminosulfonic acid is 8.2-8.6:3.8-4.2:0.13-0.

16.

7. The method for preparing a flame-retardant modified bitumen waterproof membrane according to claim 1, characterized in that, The method for preparing the flame-retardant modified bitumen waterproof membrane is as follows: flame-retardant modified bitumen material is coated on both sides of the base layer to obtain an upper flame-retardant modified bitumen layer and a lower flame-retardant modified bitumen layer; polyethylene film is covered on both sides of the flame-retardant modified bitumen layer to obtain an upper protective layer and a lower protective layer; and flame-retardant modified bitumen waterproof membrane is obtained by hot pressing and cooling. The flame-retardant modified bitumen waterproof membrane has the following structure from top to bottom: upper protective layer, upper flame-retardant modified bitumen layer, base layer, lower flame-retardant modified bitumen layer, and lower protective layer. The base layer is made of polyester fiber nonwoven fabric with a thickness of 0.20-0.25mm; The coating thickness of the flame-retardant modified asphalt material is 1.2-1.4 mm; The thickness of the polyethylene film is 0.18-0.23 mm.

8. The flame-retardant modified bitumen waterproof membrane prepared by the preparation method according to any one of claims 1-7.

Citation Information

Patent Citations

  • Water-based asphalt coating, preparation method thereof and composite waterproof structure

    CN119979007A

  • Modified asphalt waterproof coiled material and preparation method thereof

    CN120206948A