High-elastic wear-resistant yarn and hot twist type strip covering spinning method and application thereof
By employing a hot-twisted strip-wrapping spinning method and a three-zone gradient heating process, the problems of low friction coefficient, poor adhesion, and lack of elasticity in high-strength, high-modulus fiber filaments have been solved, resulting in the preparation of high-performance composite yarns suitable for high-performance textiles.
Patent Information
- Application Number
- CN202511145886.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-15
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-08-15
AI Technical Summary
High-strength, high-modulus fiber filaments suffer from problems such as low coefficient of friction, poor adhesion, lack of elasticity, and poor processability during processing, leading to a decline in the performance of composite materials.
A hot-twisted strip-wrapping spinning method is used to prepare high-elasticity and abrasion-resistant yarn by hot-twisting thermoplastic film rolls into strips and high-strength, high-modulus fiber filaments, combined with three-zone gradient heating and precise pressure control.
A composite yarn with high elasticity, high abrasion resistance and high strength was prepared, which improved the overall performance of the yarn and is suitable for high-performance textiles such as outdoor sports footwear and protective equipment. It simplifies the production process and reduces costs.
Smart Images

Figure CN120905820B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of textile processing technology, and in particular to a high-elasticity, abrasion-resistant yarn and its hot-twisted strip-wrapping spinning method and application. Background Technology
[0002] High-strength, high-modulus fiber filaments are widely used in aerospace, defense, building reinforcement, petrochemical, and leisure sports due to their excellent properties such as lightweight, high strength, high modulus, electrical conductivity, thermal conductivity, high temperature resistance, and corrosion resistance. However, these fiber filaments face some technical bottlenecks in practical applications, such as low coefficient of friction, poor adhesion, difficulty in blending with other fiber yarns, and lack of elasticity and poor processability, which limit their application in high-performance textiles.
[0003] Traditional high-strength, high-modulus fiber filaments, due to their high rigidity, are difficult to elasticize and improve abrasion resistance during processing. For example, materials such as carbon fiber and aramid fiber, while possessing extremely high strength and modulus, are prone to breakage during processing due to their lack of elasticity when made into yarns, and the final products lack comfort and abrasion resistance. Furthermore, when these fiber filaments are compounded with other materials, their poor adhesion makes it difficult to form a uniform composite structure, leading to a decline in the overall performance of the composite material.
[0004] To address these issues, various methods have been explored in the prior art, such as coating the fiber surface with an elastic coating or using elastic fibers for composite bonding. However, these methods have some drawbacks. For example, coating methods may cause the coating on the fiber surface to peel off during processing, affecting the performance of the composite material; while simple composite methods struggle to achieve a uniform bond between the fiber and the elastic material, resulting in insufficient elasticity and wear resistance in the composite material.
[0005] Therefore, developing a new method that can effectively solve the technical bottlenecks in elasticity, abrasion resistance and processability of high-strength, high-modulus fiber filaments has important practical significance and application value. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention aims to provide a high-elasticity, abrasion-resistant yarn, its hot-twisted strip-wrapping spinning method, and its application.
[0007] To achieve the above-mentioned objectives, the present invention also provides a method for hot-twisted strip-wrapping spinning of high-elasticity, abrasion-resistant yarn, comprising the following steps:
[0008] S1. Cut the thermoplastic film roll into strips;
[0009] S2. The strip and high-strength, high-modulus fiber filaments are wrapped together by hot twisting to form yarn, resulting in high-elasticity and wear-resistant yarn.
[0010] The hot-twisted strip covering includes a three-zone gradient hot pressing process. The three-zone gradient heating is divided into a front zone, a middle zone, and a back zone from the front roller to the yarn guide hook. The heating temperature of the front zone is 110-120℃ and the contact pressure is 10-30mN. The heating temperature of the middle zone is 120-140℃ and the contact pressure is 20-40mN. The heating temperature of the back zone is 90-110℃ and the contact pressure is 5-25mN.
[0011] Preferably, the hot-twisted strip-wrapping spinning method for the high-elasticity, abrasion-resistant yarn is as follows:
[0012] S1. Place the thermoplastic film roll in a cutting machine and cut it into strips;
[0013] S2. The high-strength, high-modulus fiber filaments and the strip are processed by a ring spinning machine. The high-strength, high-modulus fiber filaments and the strip are respectively passed through guide rollers and converged at the nip of the front roller and the front rubber roller to ensure that the high-strength, high-modulus fiber filaments are located in the middle of the strip. A three-zone gradient hot pressing device is added to the lower part of the yarn between the front roller and the guide hook. The prepolymer, after being heated and bonded, is wound onto the yarn tube after passing through the guide hook and the wire traveler, and finally a high-elasticity and wear-resistant yarn is obtained.
[0014] The high-strength, high-modulus fiber filament is at least one of aramid fiber, carbon fiber, para-aramid, polyethylene fiber, polyimide fiber, polyphenylene sulfide fiber, polyarylate fiber, basalt fiber, and silicon carbide fiber.
[0015] The thermoplastic film roll is at least one of thermoplastic styrene elastomer, thermoplastic vulcanized rubber, and thermoplastic polyurethane elastomer.
[0016] The strip has a width of 5-30 mm and a thickness of 0.01-0.05 mm.
[0017] The ring spinning machine has a spindle speed of 1500-3000 r / min and an output speed of 5-20 m / min.
[0018] The arc length of each heating contact surface of the three-zone gradient hot pressing device corresponds to a central angle of 10-60 degrees, the arc length radius is 5-10mm, and the interval between each heating contact surface is 3-20mm.
[0019] The high-elasticity and abrasion-resistant yarn described in this invention can be used in sports footwear, protective equipment, outdoor gear, and smart wearables.
[0020] The improvement and inventiveness of this invention lie in the gradual optimization of the processing method for high-strength, high-modulus fiber filaments. Firstly, to address the problems of low friction coefficient, poor adhesion, lack of elasticity, and poor processability of high-strength, high-modulus fiber filaments, this invention employs a strip-wrapping method for the fiber filaments. This method involves wrapping the outer surface of the fiber filaments with flexible thermoplastic elastomer strips. Utilizing the elasticity and adhesion of the thermoplastic elastomer, the surface properties of the fiber filaments are improved, increasing their elasticity and abrasion resistance. Simultaneously, the processing performance of the fiber filaments is enhanced, providing a foundation for subsequent processing.
[0021] Furthermore, this invention introduces a heating step, which enhances the bonding between the thermoplastic elastomer strip and the fiber filament. This improvement not only strengthens the bond between the strip and the fiber but also improves the overall performance of the yarn, making the composite yarn more stable during processing. The introduction of the heating step is a key step in solving the poor adhesion between the fiber filament and the thermoplastic elastomer strip, enabling the two materials to form a tighter bond at high temperatures, thereby improving the overall performance of the composite yarn.
[0022] Building upon this foundation, the present invention further optimizes the heating process by employing a three-zone gradient heating method. This heating approach achieves precise control of the thermoplastic elastomer strip by setting different temperatures in different zones. The preheating zone ensures the strip reaches the appropriate temperature before entering the bonding zone, softening it and preventing cold-stretch breakage. The middle zone performs precise bonding, while the rear zone provides cooling and shaping transitions, reducing yarn structure loosening or tightening caused by thermal deformation. This zoned heating method not only improves the bonding quality of the yarn but also reduces thermal damage caused by uneven temperature, further enhancing the yarn's performance and quality.
[0023] Finally, this invention further optimizes the composite yarn preparation process by precisely controlling the pressure. By adjusting the pressure, it ensures uniform bonding between the thermoplastic elastomer strip and the fiber filaments, while avoiding yarn damage due to excessive pressure or weak bonding due to insufficient pressure. This precise pressure control, combined with a three-zone gradient heating process, enables the composite yarn to maintain high strength and high modulus while also possessing excellent elasticity and abrasion resistance. Ultimately, it achieves high performance and processability of high-strength, high-modulus fiber filaments, making it possible for applications in outdoor sports footwear and other fields.
[0024] Compared with existing technologies, it has the following advantages:
[0025] 1) This invention successfully produces a composite yarn that combines high elasticity, high abrasion resistance, and high strength by using thermoplastic elastomer flexible strips to wrap high-strength, high-modulus fiber filaments and combining this with a three-zone gradient heating and precise pressure control process. This composite yarn overcomes the technical bottlenecks of traditional high-strength, high-modulus fiber filaments being inelastic and not abrasion-resistant, significantly improving the overall performance of the yarn and enabling it to meet the needs of high-performance textiles such as outdoor sports footwear and protective equipment.
[0026] 2) This invention proposes a hot-twisted strip-wrapping spinning method. Through strip spinning, utilizing the twisting and core-sleeving effect of the spinning frame, the strip-shaped linear composite prepolymer is directly and continuously transformed into a linear cylindrical core-sleeved composite yarn. This method not only simplifies the traditional spinning process, eliminating a series of steps such as drawing and roving, but also improves production efficiency and reduces production costs, exhibiting significant economic advantages and ease of promotion and application.
[0027] 3) The high-elasticity and abrasion-resistant yarn prepared by this invention maintains high strength and high modulus while also possessing excellent elasticity and abrasion resistance, greatly expanding its application range. This material is not only suitable for the preparation of high-performance textiles such as outdoor sports footwear and protective equipment, but can also be used in fields such as smart wearable devices, providing new possibilities for the application of high-performance fiber composite materials in more fields. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the ring spinning machine used in the hot twisting strip covering spinning method for high elastic abrasion-resistant yarn in Embodiment 1 of the present invention.
[0029] 1. Strip; 2. High-strength, high-modulus fiber filaments; 3-1. Guide roller; 3-2. Guide roller; 4. Front roller; 5. Front rubber roller; 6. Three-zone gradient hot pressing device; 7. Yarn guide hook; 8. Traveling wire; 9. Yarn tube;
[0030] Figure 2 This is a schematic diagram of the hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn according to Embodiment 1 of the present invention;
[0031] Figure 3 This is a digital photograph of the actual object of the hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn in Embodiment 1 of the present invention;
[0032] Figure 4 Images of fabrics prepared from the high-elasticity, abrasion-resistant yarn prepared in Example 1 of this invention;
[0033] Figure 5 Microscopic images of the fabric prepared from the high-elasticity and abrasion-resistant yarn in Example 1 of this invention, displayed under a 3D microscope. Detailed Implementation
[0034] Polyethylene fiber, denier: 100D, number of monofilaments: 82, function: high modulus, tensile strength: 345.20 (N / tex), Dongguan Suoweite Special Wire & Tape Co., Ltd.
[0035] Thermoplastic polyurethane elastomer (TPU), thickness 0.015mm, model: Hydro10, Sichuan Youborui New Material Co., Ltd.
[0036] The raw materials used in the embodiments and comparative examples of this invention are all commercially available products.
[0037] Example 1
[0038] A hot-twisted strip-wrapping spinning method for high-elasticity, abrasion-resistant yarn is as follows:
[0039] S1. Place the thermoplastic polyurethane elastomer film roll into a cutting machine and cut it into strips 1 with a width of 15mm and a thickness of 0.015mm;
[0040] S2. A ring spinning machine is used to process the polyethylene fiber 2 and the strip 1, which are respectively passed through guide rollers 3-1 and 3-2 and converged at the nip of the front roller 4 and the front rubber roller 5, ensuring that the polyethylene fiber 2 is located in the middle of the strip 1. A three-zone gradient hot pressing device 6 is added to the lower part of the yarn between the front roller 4 and the guide hook 7. The prepolymer, after being heated and bonded, passes through the guide hook 7 and the traveler 8 and is then wound onto the yarn tube 9. The spindle speed of the ring spinning machine is 1800 r / min, and the output speed is 12 m / min. The arc length of each heating contact surface of the three-zone gradient hot pressing device 6 corresponds to a central angle of 30 degrees and an arc radius of 8mm. The interval between each heating contact surface is 10mm. The three-zone gradient hot pressing device 6 is divided into a front zone, a middle zone, and a rear zone from the front roller 4 to the yarn guide hook 7. The heating temperature of the front zone is 115℃ and the contact pressure is 20mN. The heating temperature of the middle zone is 130℃ and the contact pressure is 30mN. The heating temperature of the rear zone is 100℃ and the contact pressure is 15mN. Finally, a high-elasticity and wear-resistant yarn is obtained.
[0041] Example 2
[0042] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the heating temperature in the middle zone is 135°C.
[0043] Example 3
[0044] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the heating temperature in the middle zone is 125°C.
[0045] Example 4
[0046] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the pressure in the middle zone is set to 45mN.
[0047] Example 5
[0048] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the pressure in the middle zone is set to 15mN.
[0049] Example 6
[0050] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the heating temperature of the back zone is 120°C.
[0051] Example 7
[0052] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the back zone pressure is set to 25mN.
[0053] Comparative Example 1
[0054] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the front and back zones are not set.
[0055] Comparative Example 2
[0056] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that the front zone, middle zone and back zone are all at room temperature.
[0057] Comparative Example 3
[0058] A hot-twisted strip-wrapping spinning method for high-elasticity and wear-resistant yarn is basically the same as that in Example 1, except that the heating and pressurizing device 6 is not provided.
[0059] Comparative Example 4
[0060] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that only polyethylene fiber 2 is used and strip 1 is not used.
[0061] Comparative Example 5
[0062] A hot-twisted strip-wrapping spinning method for high-elasticity and abrasion-resistant yarn is basically the same as that in Example 1, except that only the cut strip 1 is used, and polyethylene fiber 2 is not used.
[0063] Test Example 1
[0064] Abrasion resistance test:
[0065] According to the national textile industry standard JJ / F050-2015 "Calibration Specification for Yarn Abrasion Resistance Tester", the abrasion resistance of the high-elasticity abrasion-resistant yarns prepared in the embodiments and comparative examples of this invention were tested. The testing instrument was an FFZ622 yarn abrasion resistance tester. Each group of tests was repeated 10 times at a speed of 60 times / min. The friction medium was 400-mesh sandpaper, and the weight was 40g. The number of abrasion tests was recorded, and the average value of the results was taken.
[0066] The test results are shown in Table 1.
[0067] Table 1
[0068] Experimental protocol Average number of wear cycles Example 1 4752 Example 2 4271 Example 3 4325 Example 4 4456 Example 5 4295 Example 6 4501 Example 7 4630 Comparative Example 1 3963 Comparative Example 2 3862 Comparative Example 3 3695 Comparative Example 4 2759 Comparative Example 5 1996
[0069] Test Example 2
[0070] Elastic recovery rate test:
[0071] Referring to the textile industry standard FZ / T50007-2012 "Test Method for Elasticity of Spandex Yarn", the elastic recovery performance of the high-elasticity abrasion-resistant yarns prepared in the embodiments and comparative examples of this invention was evaluated using a YG061F electronic single yarn tensile testing machine. The test parameters were: pretension: 0.5 cN / dtex; stretching rate: 500 mm / min; cycle mode: 3 cycles of constant elongation stretching (30% elongation); hold time: 30 seconds (constant length relaxation after each stretching), relaxation time: 180 seconds (free recovery after the final stretching). Ten samples were tested in each group, and the elastic recovery rate after the last cycle was recorded. The calculation formula is as follows:
[0072] εr=(L1−L2) / (L1−L0)×100%
[0073] Where: L0: Original length of the sample (mm);
[0074] L1: Length (mm) when stretched to a fixed length;
[0075] L2: Final length after relaxation (mm);
[0076] The results are represented by the arithmetic mean of the material's elastic recovery performance, and the test results are shown in Table 2.
[0077] Table 2
[0078] Experimental protocol Elastic recovery rate (%) Example 1 91.5 Example 2 85.2 Example 3 82.4 Example 4 87.5 Example 5 86.0 Example 6 82.6 Example 7 90.1 Comparative Example 1 70.6 Comparative Example 2 48.3 Comparative Example 3 45.5 Comparative Example 4 Unable to achieve 30% elongation Comparative Example 5 95.1
[0079] Example 1 precisely matched the viscoelastic transition window of TPU in temperature control. The temperature of 130°C allowed the strip to reach an equilibrium between the molten viscous flow state and the highly elastic state, with moderate molecular chain segment mobility, complete coverage of polyethylene filaments, sufficient adhesion, and structural stability. There was no excessive flow or thermal degradation, and the abrasion resistance reached 4752 cycles with an elastic recovery rate of 91.5%. In terms of microstructure, TPU completely wetted the fiber, with no air gaps or pores, and the stress was evenly distributed. In contrast, Example 2 (135°C) exceeded the thermal stability critical point of TPU, resulting in molecular chain breakage, local overheating leading to TPU decomposition, increased yarn unevenness, a decrease in elastic recovery rate to 85.2%, the formation of stress concentration points, and a 10.1% decrease in abrasion resistance. Example 3 (125°C) was below the viscoelastic transition temperature, resulting in insufficient strip diffusion, weak interfacial bonding, increased risk of core leakage, and a 9.0% decrease in abrasion resistance due to weak adhesion.
[0080] Example 1 (mid-zone pressure 30mN) achieved an optimal balance between high abrasion resistance (4752 cycles) and high resilience (91.5%) by precisely controlling the thermal resistance-temperature coupling relationship. In terms of heat conduction mechanism, the 30mN pressure just eliminates micro-air gaps, maximizing heat conduction efficiency, and the actual temperature is stabilized at 130℃, matching the viscoelastic state of TPU. However, Example 4 (45mN) has too high tension and too low thermal resistance, resulting in local overheating, TPU molecular chain breakage, and more likely to produce uneven yarn formation, forming stress concentration points, and reducing both abrasion resistance and elastic recovery rate. Example 5 (15mN) has too low tension and too high thermal resistance, and the actual temperature is lower than the viscoelastic state window. The TPU and fiber are loosely bonded, and it is easy to delaminate during friction, resulting in significant performance degradation.
[0081] The 100℃ / 15mN back-zone process of Example 1 outperforms Examples 6 and 7 in three dimensions: temperature-phase transition control, pressure-molecular chain relaxation, and microstructure verification. Regarding temperature, Example 1 precisely matches the glass transition temperature of TPU, placing it in the transition zone from a highly elastic state to a glassy state, achieving slow, ordered crystallization and forming fine spherulites, ensuring a high elastic recovery rate (91.5%) and good wear resistance (4752 cycles). In contrast, Example 6's over-temperature process breaks through the viscous flow state, forming coarse spherulites, leading to performance degradation. Regarding pressure, the 15mN pressure of Example 1 allows the molecular chains to relax freely, forming a moderately ordered crystallinity, primarily based on entropy elasticity, achieving high elastic recovery. The high pressure of Example 7 forces the molecular chains to orient, increasing crystallinity, primarily based on energy elasticity, sacrificing elasticity and wear resistance.
Claims
1. A method for hot-twisted strip-wrapping spinning of high-elasticity, abrasion-resistant yarn, characterized in that, Includes the following steps: S1. Place the thermoplastic film roll in a cutting machine and cut it into strips (1). S2. Using a ring spinning machine, the high-strength, high-modulus fiber filament (2) and the strip (1) are respectively passed through guide rollers and converged at the nip of the front roller (4) and the front rubber roller (5) to ensure that the high-strength, high-modulus fiber filament (2) is located in the middle of the strip (1). A three-zone gradient hot pressing device (6) is added to the lower part of the yarn between the front roller (4) and the guide hook (7). The prepolymer, which is heated and bonded, is wound onto the yarn tube (9) after passing through the guide hook (7) and the wire ring (8), and finally a high-elasticity and wear-resistant yarn is obtained. The thermoplastic film roll is a thermoplastic polyurethane elastomer; The hot-twisted strip covering includes three-zone gradient hot pressing, which is divided into a front zone, a middle zone, and a back zone from the front roller (4) to the yarn guide hook (7); the heating temperature of the front zone is 110-120℃ and the contact pressure is 10-30mN; the heating temperature of the middle zone is 125-135℃ and the contact pressure is 20-40mN; the heating temperature of the back zone is 90-110℃ and the contact pressure is 5-25mN.
2. The hot-twisted strip-wrapping spinning method for high-elasticity, abrasion-resistant yarn as described in claim 1, characterized in that, The high-strength, high-modulus fiber filament (2) is at least one of aramid fiber, carbon fiber, polyethylene fiber, polyimide fiber, polyphenylene sulfide fiber, polyarylate fiber, basalt fiber, and silicon carbide fiber.
3. The hot-twisted strip-wrapping spinning method for high-elasticity, abrasion-resistant yarn as described in claim 1, characterized in that, The strip (1) has a width of 5-30 mm and a thickness of 0.01-0.05 mm.
4. The hot-twisted strip-wrapping spinning method for high-elasticity, abrasion-resistant yarn as described in claim 1, characterized in that, The ring spinning machine has a spindle speed of 1500-3000 r / min and an output speed of 5-20 m / min.
5. The hot-twisted strip-wrapping spinning method for high-elasticity, abrasion-resistant yarn as described in claim 1, characterized in that, The arc length of each heating contact surface of the three-zone gradient hot pressing device (6) corresponds to a central angle of 10-60 degrees, the arc length radius is 5-10 mm, and the interval between each heating contact surface is 3-20 mm.
6. A high-elasticity, abrasion-resistant yarn, characterized in that, It is prepared by the spinning method described in any one of claims 1-5. Its structure is a core-sheath composite adhesive structure, with high-strength, high-modulus fiber filaments (2) as the core layer and thermoplastic film roll strips (1) as the sheath layer. A molecular-level interpenetrating interface is formed by three-zone gradient hot pressing to achieve efficient bonding between the core layer and the sheath layer.
7. The application of the high-elasticity, abrasion-resistant yarn as described in claim 6, characterized in that, The high-elasticity and abrasion-resistant yarn is used in sports footwear, protective equipment, and outdoor gear.
Citation Information
Patent Citations
Spinning fiber bundle ironing device
CN103255517A
Three-roller superlarge-drafting ironed yarn production method
CN103361789A