Catalyst composition, polylactide and methods of making and using the same

By combining rare earth metal complexes with hydroxyl-containing catalysts, the problems of low catalytic activity and uncontrollable molecular weight were solved, achieving efficient and controllable synthesis of polylactide with high catalytic efficiency and narrow molecular weight distribution.

CN121005877BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410638602.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2026-11-20
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Existing catalysts exhibit low catalytic activity during the polymerization of lactide monomers, have uncontrollable molecular weights, and the addition of hydroxyl-containing compounds leads to catalyst deactivation and termination of the polymerization chain growth reaction.

Method used

Polylactide is prepared by solution polymerization using a rare earth metal complex with a specific structure and a catalyst containing a hydroxyl compound, with the rare earth metal complex acting as the catalyst and the hydroxyl compound acting as the chain transfer agent, while controlling the molecular weight distribution.

Benefits of technology

It achieves highly efficient catalytic ring-opening polymerization of lactide with high polymerization conversion rate, controllable molecular weight, narrow molecular weight distribution, and exhibits 'unkillable' polymerization characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121005877B_ABST
    Figure CN121005877B_ABST
Patent Text Reader

Abstract

The application relates to the technical field of polymers, and discloses a catalyst composition, polylactide and a preparation method and application thereof. The catalyst composition of the application contains a rare earth metal complex with a structure shown in formula (I) and a hydroxyl-containing compound, in formula (I), Ln is a rare earth metal, R1-R6 are independently selected from hydrogen or C1-C3 alkyl; R7 is selected from hydrogen or C1-C3 alkyl or halogen; and R8 is a silicon-containing group. When the catalyst composition provided by the application is used for preparing polylactide through ring-opening polymerization of lactide, the catalyst has high catalytic activity, the obtained polymer has high molecular weight, the molecular weight can be controlled, and the molecular weight distribution is narrow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer technology, specifically to a catalyst composition, polylactide, its preparation method, and its application. Background Technology

[0002] Polylactic acid (PLA) is a polyester-based biodegradable material with excellent biodegradability, making it widely used in the manufacture of tableware, films, fibers, clothing, automotive parts, and disposable containers. This helps address the environmental pollution problems caused by petrochemical resources. Furthermore, PLA possesses good biocompatibility, non-toxicity, and adjustable degradation characteristics, meeting the requirements for pharmaceutical polymer materials. It shows broad application prospects in fracture internal and external fixation materials, surgical sutures, tissue engineering scaffold materials, and drug sustained-release and controlled-release carrier materials.

[0003] Early methods for synthesizing polyesters primarily involved condensation reactions of acidic and alcoholic compounds. However, the resulting polymers exhibited uncontrollable structures, potentially being linear, branched, or cyclic, with excessively wide molecular weight distributions, low molecular weights, and difficulty in controlling molecular weight, ultimately leading to poor mechanical properties. To improve the overall performance of polymers, recent research on polyester synthesis has focused on developing catalysts for coordination polymerization to initiate ring-opening polymerization of cyclic esters to prepare polyester polymers. Compared to the aforementioned condensation reaction methods, ring-opening polymerization offers the following advantages: First, the molecular weight of the polyester can be precisely controlled, and the molecular weight distribution is narrower; second, no water is generated during ring-opening polymerization, resulting in polymers with higher molecular weights; and third, selective polymerization of chiral monomers can be achieved through catalyst selection.

[0004] Catalyst systems used in the coordination ring-opening polymerization of lactones mainly include complexes of stannous octoate, aluminum, calcium, magnesium, zinc, titanium, and Group IIIB metal complexes. Stannous octoate is currently recognized as a relatively effective catalyst, exhibiting high catalytic activity, requiring only a small amount of catalyst, and capable of producing high molecular weight polymers. Its drawback is that it can only undergo high-temperature bulk polymerization, and its conversion rate is only around 50% at the highest molecular weight. To improve the conversion rate, it is necessary to reduce the molecular weight. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of low catalytic activity and uncontrollable molecular weight in existing technologies, and to provide a catalyst composition, polylactide, its preparation method, and its applications. When the catalyst composition provided by this invention is used in the ring-opening polymerization of lactide to prepare polylactide, it not only exhibits high catalytic activity, but also produces a polymer with a high molecular weight, adjustable molecular weight, and a narrow molecular weight distribution.

[0006] In conventional technologies, the addition of hydroxyl-containing compounds to conventional catalysts during the polymerization of lactide monomers often leads to catalyst deactivation, thereby terminating the polymerization chain growth reaction. However, the inventors of this invention, through in-depth research, have discovered that the addition of hydroxyl-containing compounds to the rare earth metal complexes of this invention can still catalyze polymer chain growth normally without terminating polymerization. In the polymerization of lactide monomers, the rare earth metal complexes act as catalysts, while the hydroxyl-containing compounds act as chain transfer agents. That is, active chain transfer can occur between the hydroxyl-containing compounds and the initiation center, resulting in continuous chain growth. The apparent effect is that one complex molecule can initiate the growth of a 1-1000 times larger molecular chain. Therefore, the catalytic efficiency is very high, the conversion rate of the polymerization reaction is high, and it exhibits "undying" polymerization characteristics. Utilizing this, the molecular weight of the polymer can be adjusted within a wide range by controlling the amount of hydroxyl-containing compounds added. Simultaneously, the addition of hydroxyl-containing compounds also results in an ideal molecular weight distribution for the polymer.

[0007] Therefore, in a first aspect, the present invention provides a catalyst composition comprising a rare earth metal complex of formula (I) and a hydroxyl-containing compound.

[0008]

[0009] In formula (I), Ln is a rare earth metal, R1-R6 are each independently selected from hydrogen or C1-C3 alkyl groups; R7 is selected from hydrogen or C1-C3 alkyl groups or halogens; and R8 is a silicon-containing group.

[0010] In formula (I), THF represents tetrahydrofuran.

[0011] Preferably, Ln is selected from scandium, yttrium, lanthanides or actinides, and more preferably from scandium or yttrium; R1-R5 are hydrogen; R6 is methyl, ethyl or isopropyl; R7 is hydrogen or chlorine; R8 is trimethylsilylmethylene or hexamethyldisilazine.

[0012] Preferably, the rare earth metal complex with the structure shown in formula (I) is selected from at least one of the following complexes:

[0013] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0014] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0015] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazine.

[0016] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane.

[0017] Preferably, the hydroxyl-containing compound is an alcohol and / or a phenolic compound.

[0018] Preferably, the hydroxyl-containing compound is a substituted or unsubstituted C1-C5 straight-chain or branched fatty alcohol, or a C6-C5... 20 At least one of aromatic alcohols, C4-C6 alkanolamines, and phenols, wherein the substituted group is selected from C1-C6 alkyl, C1-C6 alkoxy, or C6-C6 alkyl groups. 10 Aryl.

[0019] Preferably, the hydroxyl-containing compound is at least one selected from methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, triethanolamine, diphenylmethanol, triphenylmethanol, benzyl alcohol, and phenol.

[0020] Preferably, the molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.01-500, more preferably 1:0.1-100, and even more preferably 1:0.1-50.

[0021] According to a second aspect of the present invention, a method for preparing polylactide is provided, wherein the method comprises: a step of solution polymerization of lactide monomers in the presence of a rare earth metal complex of formula (I) and a hydroxyl-containing compound.

[0022]

[0023] In formula (I), Ln is a rare earth metal, R1-R6 are each independently selected from hydrogen or C1-C3 alkyl groups; R7 is selected from hydrogen or C1-C3 alkyl groups or halogens; and R8 is a silicon-containing group.

[0024] Preferably, Ln is selected from scandium, yttrium, lanthanides or actinides, and more preferably from scandium or yttrium; R1-R5 are hydrogen; R6 is methyl, ethyl or isopropyl; R7 is hydrogen or chlorine; R8 is trimethylsilylmethylene or hexamethyldisilazine.

[0025] Preferably, the rare earth metal complex with the structure shown in formula (I) is selected from at least one of the following complexes:

[0026] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0027] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0028] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazine.

[0029] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane.

[0030] Preferably, the hydroxyl-containing compound is an alcohol and / or a phenolic compound.

[0031] Preferably, the hydroxyl-containing compound is a substituted or unsubstituted C1-C5 straight-chain or branched fatty alcohol, or a C6-C5... 20 At least one of aromatic alcohols, C4-C6 alkanolamines, and phenols, wherein the substituted group is selected from C1-C6 alkyl, C1-C6 alkoxy, or C6-C6 alkyl groups. 10 Aryl.

[0032] Preferably, the hydroxyl-containing compound is at least one selected from methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, triethanolamine, diphenylmethanol, triphenylmethanol, benzyl alcohol, and phenol.

[0033] Preferably, the molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.01-500, more preferably 1:0.1-100, and even more preferably 1:0.1-50.

[0034] Preferably, the molar ratio of the hydroxyl-containing compound to the lactide monomer is 1:1-10000, more preferably 1:20-8000, more preferably 1:20-6000, even more preferably 1:20-5000, and even more preferably 1:500-5000.

[0035] Preferably, the molar ratio of the rare earth metal complex to the lactide monomer is 1:10-5000, more preferably 1:50-3000, more preferably 1:100-2500, and even more preferably 1:100-2000.

[0036] Preferably, the conditions for solution polymerization include: a reaction temperature of 10-160℃, more preferably 25-100℃; and a reaction time of 0.02-24h, more preferably 0.1-3h.

[0037] According to a third aspect of the present invention, a polylactide prepared by the method of the present invention is provided.

[0038] According to a fourth aspect of the invention, the use of the catalyst composition of the invention in the preparation of polylactide is provided.

[0039] Through the above technical solutions, the catalyst composition and its application, as well as the polylactide and its preparation method provided by the present invention, achieve the following beneficial effects:

[0040] The catalyst composition comprising a rare earth metal complex with a specific structure and a hydroxyl-containing compound provided by this invention can efficiently catalyze the ring-opening polymerization of lactide at a low metal catalyst concentration, exhibiting high catalytic efficiency and high conversion rate of the polymerization reaction. Simultaneously, during the catalytic process, the hydroxyl-containing compound undergoes active chain transfer with the initiation center, thereby enabling the polylactide chain to continuously grow, exhibiting "undying" polymerization characteristics and a molecular weight distribution close to 1, and obtaining polylactide with controllable molecular weight. Detailed Implementation

[0041] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0042] According to a first aspect of the present invention, a catalyst composition is provided, wherein the catalyst composition comprises a rare earth metal complex with the structure shown in formula (I) and a hydroxyl-containing compound.

[0043]

[0044] In formula (I), Ln is a rare earth metal, R1-R6 are each independently selected from hydrogen or C1-C3 alkyl groups; R7 is selected from hydrogen or C1-C3 alkyl groups or halogens; and R8 is a silicon-containing group.

[0045] In this invention, the C1-C3 alkyl groups can be methyl, ethyl, propyl or isopropyl, among which methyl, ethyl or isopropyl are preferred.

[0046] According to the present invention, preferably, the halogen is fluorine, chlorine, bromine or iodine, more preferably chlorine or bromine, and even more preferably chlorine.

[0047] According to the present invention, R8 is a silicon group, preferably, R8 is a trimethylsilylmethylene or hexamethyldisilazine group.

[0048] As a rare earth metal complex with the structure shown in formula (I), it is preferably selected from at least one of the following complexes.

[0049] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0050] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0051] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazine.

[0052] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane.

[0053] According to the present invention, the hydroxyl-containing compound can be an alcohol and / or a phenolic compound. Preferably, the hydroxyl-containing compound is a substituted or unsubstituted C1-C5 straight-chain or branched fatty alcohol, or a C6-C5... 20 At least one of aromatic alcohols, C4-C6 alkanolamines, and phenols, wherein the substituted group is selected from C1-C6 alkyl, C1-C6 alkoxy, or C6-C6 alkyl groups. 10 Aryl; more preferably, the hydroxyl-containing compound is at least one selected from methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, triethanolamine, diphenylmethanol, triphenylmethanol, benzyl alcohol, and phenol; particularly preferably, the hydroxyl-containing compound is at least one selected from isopropanol, benzyl alcohol, diphenylmethanol, triphenylmethanol, and triethanolamine.

[0054] According to the present invention, the contents of the rare earth metal complex and the hydroxyl-containing compound can vary within a wide range. For example, the molar ratio of the rare earth metal complex to the hydroxyl-containing compound can be 1:0.01-500, preferably 1:0.1-100, more preferably 1:0.1-50, and particularly preferably 1:1-10.

[0055] According to the present invention, a catalyst composition comprising a rare earth metal complex with a specific structure and a hydroxyl-containing compound can efficiently catalyze the ring-opening polymerization of lactide at a low metal catalyst concentration, with high catalytic efficiency and high conversion rate of the polymerization reaction. At the same time, during the catalytic process, the hydroxyl-containing compound undergoes active chain transfer with the initiation center, thereby enabling the polylactide chain to grow continuously, exhibiting "undying" polymerization characteristics and a molecular weight distribution close to 1, and obtaining polylactide with controllable molecular weight.

[0056] In this invention, the rare earth metal complex can be synthesized using conventional methods in the art. In a preferred embodiment of this invention, the method includes:

[0057] 1) In the presence of a solvent, in the presence of Na2S2O2, the compound with the structure shown in formula (1) is subjected to a first contact reaction with the compound with the structure shown in formula (2) to obtain the compound with the structure shown in (II) (hereinafter also referred to as the ligand);

[0058] 2) In an organic solvent, the compound with the structure shown in formula (II) undergoes a second contact reaction with an alkyl rare earth metal compound or an amino rare earth metal compound to obtain a rare earth metal complex with the structure shown in formula (I).

[0059] The alkyl rare earth metal compound is selected from Ln[CH2Si(CH3)3]3(THF)2, and the amino rare earth metal compound is selected from Ln{N[Si(CH3)3]2}3(THF)2.

[0060]

[0061] In formulas (1), (2) and (II), for the R1, R2, R3, R4, R5, R6, R7 and R8 groups, as described above, and in addition, the rare earth metals in the alkyl rare earth metal compounds or amino rare earth metal compounds, such as Ln as described above, will not be repeated here.

[0062] Step 1): In the presence of a solvent and Na2S2O2, the compound with the structure shown in formula (1) undergoes a first contact reaction with the compound with the structure shown in formula (2) to obtain the compound with the structure shown in (II).

[0063] The solvent can be a solvent that can dissolve the reactants and is inert to them, such as a mixture of N,N-dimethylformamide (DMF) and water.

[0064] In a preferred embodiment of the present invention, the solvent is a mixed solvent of N,N-dimethylformamide and water, wherein the volume ratio of N,N-dimethylformamide to water is 2-5:1, preferably 3-4:1.

[0065] There is no particular limitation on the amount of solvent used; it can be any amount commonly used in the field.

[0066] The amount of compound with the structure shown in formula (2) can also be selected according to the amount of compound with the structure shown in formula (1). For example, the molar ratio of compound with the structure shown in formula (1) to compound with the structure shown in formula (2) can be 1:1-2, preferably 1:1-1.5, more preferably 1:1-1.2, and even more preferably 1:1-1.1.

[0067] The amount of Na2S2O2 can also be selected according to the amount of the compound with the structure shown in formula (1). For example, the molar ratio of the compound with the structure shown in formula (1) to Na2S2O2 can be 1:2-5, preferably 1:3-4.

[0068] The first contact reaction is preferably carried out at 80-100°C, for example at 100°C.

[0069] The duration of the first contact reaction can be, for example, 0.5 hours or more, preferably 1-10 hours, more preferably 3-8 hours, and even more preferably 4-6 hours.

[0070] After the first contact reaction is completed, the reaction product can be cooled to room temperature and neutralized with ammonia to obtain the ligand (the compound with the structure shown in formula (II)).

[0071] Step 2: In an organic solvent, the compound with the structure shown in formula (II) undergoes a second contact reaction with an alkyl rare earth metal compound or an amino rare earth metal compound to obtain a rare earth metal complex with the structure shown in formula (I).

[0072] As alkyl rare earth metal compounds or amino rare earth metal compounds, they can be prepared according to conventional synthetic methods in the art, for example, by the methods described in the preparation examples below.

[0073] As Ln[R8]3(THF)2, it can be obtained, for example, by reacting R8Li with LnCl3(THF)2.

[0074] The conditions for the above-mentioned contact reaction can be carried out using conventional conditions in this field.

[0075] As the organic solvent, n-hexane, for example, can be used.

[0076] In a preferred embodiment of the present invention, an alkyl rare earth metal compound or an amino rare earth metal compound is dissolved in the organic solvent and then subjected to a second contact reaction with a compound having the structure shown in formula (II).

[0077] The second contact reaction is preferably carried out at room temperature, for example, at 10-40°C.

[0078] The second contact reaction time can be, for example, 0.5 hours or more, preferably 1-24 hours, more preferably 8-15 hours, and even more preferably 8-12 hours.

[0079] After the second contact reaction is completed, the reaction product can be filtered, washed 2-3 times with frozen n-hexane, and dried under vacuum to obtain rare earth metal complex A with the structure shown in formula (I).

[0080] According to a second aspect of the present invention, a method for preparing polylactide is provided, wherein the method comprises: a step of solution polymerization of lactide monomers in the presence of a rare earth metal complex of formula (I) and a hydroxyl-containing compound.

[0081]

[0082] In formula (I), Ln is a rare earth metal, R1-R6 are each independently selected from hydrogen or C1-C3 alkyl groups; R7 is selected from hydrogen or C1-C3 alkyl groups or halogens; and R8 is a silicon-containing group.

[0083] In this invention, the combined use of rare earth metal complexes and hydroxyl-containing compounds reduces the amount of rare earth metal complexes required. A small amount of rare earth metal complexes can catalyze the production of high molecular weight polylactide with high catalytic efficiency. Simultaneously, during the catalytic process, the hydroxyl-containing compounds undergo active chain transfer with the initiation center, thereby enabling the polylactide chains to continuously grow, exhibiting "undying" polymerization characteristics and a molecular weight distribution close to 1, thus obtaining polylactide with controllable molecular weight.

[0084] In this invention, "lactide monomer" refers to L-lactide, D-lactide, and L,D-lactide.

[0085] Furthermore, the Ln group and the R1, R2, R3, R4, R5, R6, R7 and R8 groups are as described above and will not be repeated here.

[0086] As a rare earth metal complex with the structure shown in formula (I), it is preferably selected from at least one of the following complexes.

[0087] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0088] In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene.

[0089] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazine.

[0090] In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane.

[0091] The preparation method of the polylactide of the present invention using rare earth metal complexes and hydroxyl-containing compounds (i.e., the catalyst composition of the present invention) will be described in detail below.

[0092] According to the present invention, the amounts of the rare earth metal complex and the hydroxyl-containing compound can vary within a wide range. For example, the molar ratio of the rare earth metal complex to the hydroxyl-containing compound can be 1:0.01-500. To further improve the catalytic efficiency, preferably, the molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.1-100; more preferably, the molar ratio is 1:0.1-50; and even more preferably, the molar ratio is 1:1-10.

[0093] To further improve catalytic efficiency, preferably, the molar ratio of the hydroxyl-containing compound to the lactide monomer is 1:1-10000, more preferably 1:20-8000, more preferably 1:20-6000, even more preferably 1:20-5000, and even more preferably 1:500-5000.

[0094] To further improve catalytic efficiency, preferably, the molar ratio of the rare earth metal complex to the lactide monomer is 1:10-5000, more preferably 1:50-3000, more preferably 1:100-2500, and even more preferably 1:100-2000.

[0095] In this invention, there is no particular limitation on the way the rare earth metal complex and the hydroxyl-containing compound are added. They can be added separately during the reaction, or they can be added simultaneously, or they can be prepared in advance and added simultaneously by the following method: Under dry and rapid stirring conditions, the organic solvent containing the rare earth metal complex is slowly added dropwise to the organic solvent containing the hydroxyl-containing compound, and the resulting mixture is vacuum filtered to obtain the catalyst composition.

[0096] The organic solvent containing the aforementioned rare earth metal complex can be the same as or different from the organic solvent containing the hydroxyl-containing compound, but preferably both are the same. Furthermore, the solvent used in solution polymerization can also be used as the organic solvent.

[0097] According to the present invention, the solvent used in the solution polymerization can be an organic solvent, preferably at least one of substituted or unsubstituted alkanes, substituted or unsubstituted benzenes and substituted or unsubstituted ethers.

[0098] In a preferred embodiment of the present invention, the solvent is at least one selected from pentane, hexane, benzene, chlorobenzene, toluene, tetrahydrofuran, diethyl ether, and dichloromethane; more preferably, the solvent is one or more selected from toluene, tetrahydrofuran, and dichloromethane.

[0099] According to the present invention, preferably, the solution polymerization conditions include a reaction temperature of 10-160°C and a reaction time of 0.02-24 h; more preferably, the solution polymerization conditions include a reaction temperature of 25-100°C and a reaction time of 0.1-3 h. Furthermore, to avoid the influence of water and oxygen on the catalytic activity of the catalyst, the reaction of the present invention is preferably carried out under anhydrous and oxygen-free conditions.

[0100] After the reaction is complete, post-treatment is performed to obtain polylactide. The post-treatment may include adding the mixed liquid after the reaction to an ethanol solution of hydrochloric acid with a volume concentration of 5-20 v% (preferably 8-12 v%) to terminate the reaction, then precipitating it in ethanol, filtering to obtain a white solid, and drying the white solid at 30-50℃ for 36-60 h to obtain polylactide.

[0101] According to a third aspect of the present invention, a polylactide prepared by the method of the second method of the present invention is provided.

[0102] In the preparation method of this invention, the combined use of rare earth metal complexes and hydroxyl-containing compounds reduces the amount of rare earth metal complexes required. A small amount of rare earth metal complexes can catalyze the production of high molecular weight polylactide with high catalytic efficiency. Simultaneously, during the catalytic process, the hydroxyl-containing compounds undergo active chain transfer with the initiation center, thereby enabling the polylactide chains to continuously grow, exhibiting "undying" polymerization characteristics and a molecular weight distribution close to 1, thus obtaining polylactide with controllable molecular weight.

[0103] Specifically, the number-average molecular weight of the polylactide can be 0.1 million to 200,000, preferably 0.35 million to 170,000; the molecular weight distribution is 1 to 1.5, preferably 1 to 1.3.

[0104] According to a fourth aspect of the invention, the use of the catalyst composition of the first aspect of the invention in the preparation of polylactide is provided.

[0105] The present invention will be described in detail below through embodiments, but the present invention is not limited to the following embodiments.

[0106] In the following examples, the room temperature is approximately "25°C";

[0107] (1) Polymer conversion rate: The conversion rate was measured using a Swiss Bruker Avance 400 nuclear magnetic resonance spectrometer. The test conditions were: the solvent was deuterated chloroform and the test temperature was room temperature.

[0108] (2) Molecular weight and distribution of polymer: The molecular weight was determined by a Shimadzu LC-20A liquid gel permeation chromatograph (GPC); the test conditions were: chloroform solvent, test temperature 25℃, and flow rate 1mL / min.

[0109] (3) Elemental analysis of metal complexes: Elemental analysis was performed using an Elementar Vario EL elemental analyzer;

[0110] The ligand structure used in the embodiments of the present invention is shown in formula (II), and the preparation method is as follows:

[0111]

[0112] The compounds with the structure shown in formula (1) and the compound with the structure shown in formula (2) with a molar ratio of 1:1 were weighed and dissolved in a solution of DMF / H2O (volume ratio of 3:1). Three times the molar amount of Na2S2O2 was added, and the mixture was stirred at 100℃ for 5 h. After cooling, the mixture was neutralized with ammonia water to obtain the desired ligand (the compound with the structure shown in formula (II)). The mixture was then filtered, dried under vacuum, and stored for later use.

[0113] in,

[0114] Ligand A (in formula (II), R1-R5 are hydrogen, R6 is methyl, and R7 is hydrogen), its molecular formula is C 17 H 13 N3O (measured values): C, 74.17 (74.16); H, 4.76 (4.78); N, 15.26 (15.25); O, 5.81 (5.81).

[0115] Ligand B (in formula (II), R1-R5 are hydrogen, R6 is ethyl, and R7 is hydrogen), has the molecular formula C 18 H 15 N3O (measured values): C, 74.72 (74.71); H, 5.23 (5.25); N, 14.52 (14.52); O, 5.53 (5.52).

[0116] Ligand C (in formula (II), R1-R5 are hydrogen, R6 is isopropyl, and R7 is hydrogen), its molecular formula is C 19 H 17 N3O (measured values): C, 75.23 (75.21); H, 5.65 (5.66); N, 13.85 (13.85); O, 5.27 (5.28).

[0117] Ligand D (in formula (II), R1-R5 are hydrogen, R6 is methyl, and R7 is chlorine), has the molecular formula C 17 H 12 ClN3O (measured values): C, 65.92 (65.91); H, 3.90 (3.92); N, 13.57 (13.56); O, 5.17 (5.17).

[0118] Preparation of alkyl yttrium:

[0119] Li+(CH3)3SiCH2Cl→(CH3)3SiCH2Li

[0120] (CH3)3SiCH2Li+YCl3(THF)2→Y[CH2Si(CH3)3]3(THF)2

[0121] In a glove box, 1.0 g of yttrium trichloride and 40 ml of tetrahydrofuran (THF) were added to a 100 ml single-necked flask and stirred overnight at room temperature. 1.4 g of alkyllithium was added to a 50 ml Erlenmeyer flask, followed by 20 ml of tetrahydrofuran (THF) to dissolve it. While stirring, the tetrahydrofuran solution of alkyllithium was slowly added dropwise to the tetrahydrofuran mixture of yttrium trichloride. After the addition was complete, the reaction was allowed to proceed at room temperature for 3 hours. After the reaction was complete, the tetrahydrofuran was dried under vacuum to obtain a grayish-white solid. The solid was washed with 10 ml × 8 ml of n-hexane and transferred to a clean flask. Approximately one-third of the solvent was removed under vacuum, and the flask was frozen at -30°C. After 1 hour, the flask was removed, and a yellow oily substance adhered to the flask wall. The supernatant was transferred out, and the above operation was repeated until no more yellow oily substance precipitated. The supernatant was then dried under vacuum to obtain a white crystalline solid, i.e., alkyl yttrium, with a yield of 74%.

[0122] Preparation of alkyl scandium:

[0123] The preparation method for alkyl yttrium described above is followed, except that YCl3(THF)2 is replaced with ScCl3(THF)2.

[0124] Preparation of aminoyttrium:

[0125] [(CH3)3Si]2NLi+YCl3(THF)2→Y{N[Si(CH3)3]2}3(THF)2

[0126] In a glove box, 0.77 g of yttrium trichloride and 20 ml of tetrahydrofuran (THF) were added to a 50 ml single-necked flask and stirred overnight at room temperature. Then, the tetrahydrofuran was dried under vacuum, and 20 ml of n-hexane was added and stirred. While stirring, 1.6 g of lithium amino group powder was slowly added to the above n-hexane mixture. After the addition was complete, the mixture was reacted at room temperature for 15 hours. After the reaction was complete, the mixture was filtered, and the filter cake was washed with a small amount of frozen n-hexane. The filter cake was then frozen in a refrigerator, and white crystals precipitated. The supernatant was dried under vacuum to obtain a white solid; both were aminoyttrium, with a yield of 64%.

[0127] Preparation of aminoscandium:

[0128] The preparation method of aminoyttrium described above is followed, except that YCl3(THF)2 is replaced with ScCl3(THF)2.

[0129] Preparation Example 1

[0130] Preparation of rare earth metal complex A (in formula (I), Ln is scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene)

[0131] Ligand A has the structure shown in formula (II), where R1-R5 are hydrogen, R6 is methyl, and R7 is hydrogen. 1.0 mmol of alkyl scandium was weighed, dissolved in n-hexane, and placed in a refrigerator for half an hour. Then, while stirring, an equimolar amount of ligand A powder was slowly added. After the addition was complete, the mixture was reacted at room temperature for 12 hours. The mixture was filtered, washed 2-3 times with frozen n-hexane, and dried under vacuum to obtain rare earth metal complex A in 58% yield.

[0132] The elemental analysis data of the product are: C 24 H 29 N3O2ScSi (measured values): C, 62.05 (62.04); H, 6.29 (6.30); N, 9.05 (9.04); O, 6.89 (6.89).

[0133] Preparation Example 2

[0134] Preparation of rare earth metal complex B (in formula (I), Ln is scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene)

[0135] Ligand B has the structure shown in formula (II), where R1-R5 are hydrogen, R6 is ethyl, and R7 is hydrogen. 1.0 mmol of alkyl scandium was weighed, dissolved in n-hexane, and placed in a refrigerator for half an hour. Then, while stirring, an equimolar amount of ligand A powder was slowly added. After the addition was complete, the mixture was reacted at room temperature for 12 hours. The mixture was filtered, washed 2-3 times with frozen n-hexane, and dried under vacuum to obtain rare earth metal complex A in 60% yield.

[0136] The elemental analysis data of the product are: C 25 H 31 N3O2ScSi (measured values): C, 62.74 (62.75); H, 6.53 (6.55); N, 8.78 (8.76); O, 6.69 (6.70).

[0137] Preparation Example 3

[0138] Preparation of rare earth metal complex C (in formula (I), Ln is yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazino)

[0139] Ligand C has the structure shown in formula (II), where R1-R5 are hydrogen, R6 is isopropyl, and R7 is hydrogen. 1.0 mmol of aminoyttrium was weighed, dissolved in n-hexane, and frozen for half an hour. Then, while stirring, an equimolar amount of ligand A powder was slowly added. After the addition was complete, the mixture was reacted at room temperature for 12 hours. The mixture was filtered, washed 2-3 times with frozen n-hexane, and dried under vacuum to obtain rare earth metal complex A in 56% yield.

[0140] The elemental analysis data of the product are: C 27 H 38 N4O2Si2Y (measured values): C, 54.44 (54.43); H, 6.43 (6.44); N, 9.41 (9.41); O, 5.37 (5.38).

[0141] Preparation Example 4

[0142] Preparation of rare earth metal complex D (in formula (I), Ln is yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane)

[0143] Ligand D has the structure shown in formula (II), where R1-R5 are hydrogen, R6 is methyl, and R7 is chlorine. 1.0 mmol of aminoyttrium was weighed, dissolved in n-hexane, and frozen for half an hour. Then, while stirring, an equimolar amount of ligand A powder was slowly added. After the addition was complete, the mixture was reacted at room temperature for 12 hours. The mixture was filtered, washed 2-3 times with frozen n-hexane, and dried under vacuum to obtain rare earth metal complex A in 54% yield.

[0144] The elemental analysis data of the product are: C 25 H 33 ClN4O2Si2Y (measured values): C, 49.87 (49.87); H, 5.52 (5.53); N, 9.31 (9.31); O, 5.31 (5.32).

[0145] Example 1

[0146] At room temperature, 10 μmol of rare earth metal complex A, 10 μmol of benzyl alcohol and 10 mL of toluene solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 20 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0147] The conversion rate of nuclear magnetic resonance testing was 89%.

[0148] GPC analysis determined the number-average molecular weight M of polylactide.n It is 121,000, and the molecular weight distribution is M. w / M n It is 1.38.

[0149] Example 2

[0150] At room temperature, 10 μmol of rare earth metal complex A, 10 μmol of benzyl alcohol and 10 mL of dichloromethane solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free conditions. 20 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle, filtered, and a white solid was obtained. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0151] The conversion rate of nuclear magnetic resonance testing was 97%.

[0152] GPC analysis determined the number-average molecular weight M of polylactide. n It is 148,000, and the molecular weight distribution is M. w / M n It is 1.13.

[0153] Example 3

[0154] At room temperature, 10 μmol of rare earth metal complex A, 10 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 20 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle, filtered, and a white solid was obtained. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0155] The conversion rate of nuclear magnetic resonance testing was 98%.

[0156] GPC analysis determined the number-average molecular weight M of polylactide. n It is 161,000, and the molecular weight distribution is M. w / M n It is 1.14.

[0157] Example 4

[0158] At room temperature, 10 μmol of rare earth metal complex B, 10 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 10 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0159] The conversion rate of nuclear magnetic resonance testing is 95%.

[0160] GPC analysis determined the number-average molecular weight M of polylactide. n It is 128,000, and the molecular weight distribution is M. w / M n It is 1.15.

[0161] Example 5

[0162] At room temperature, 10 μmol of rare earth metal complex C, 100 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 10 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0163] The conversion rate of nuclear magnetic resonance testing is 95%.

[0164] GPC analysis determined the number-average molecular weight M of polylactide. n It is 82,000, and the molecular weight distribution is M. w / M n It is 1.21.

[0165] Example 6

[0166] At room temperature, 10 μmol of rare earth metal complex D, 10 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 5 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0167] The conversion rate of nuclear magnetic resonance testing is 95%.

[0168] GPC analysis determined the number-average molecular weight M of polylactide. n It is 92,000, and the molecular weight distribution is M.w / M n It is 1.23.

[0169] Example 7

[0170] At room temperature, 10 μmol of rare earth metal complex C, 200 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 10 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution with a volume concentration of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0171] The conversion rate of nuclear magnetic resonance testing was 93%.

[0172] GPC analysis determined the number-average molecular weight M of polylactide. n It is 28,000, and the molecular weight distribution is M. w / M n It is 1.14.

[0173] Example 8

[0174] At room temperature, 10 μmol of rare earth metal complex A, 500 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 10 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution with a volume concentration of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0175] The conversion rate of nuclear magnetic resonance testing was 88%.

[0176] GPC analysis determined the number-average molecular weight M of polylactide. n It is 0.83 million, and the molecular weight distribution is M. w / M n It is 1.13.

[0177] Example 9

[0178] At room temperature, 10 μmol of rare earth metal complex C, 10 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 1 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0179] The conversion rate of nuclear magnetic resonance testing was 92%.

[0180] GPC analysis determined the number-average molecular weight M of polylactide. n It is 74,200, and the molecular weight distribution is M. w / M n It is 1.22.

[0181] Example 10

[0182] At room temperature, 10 μmol of rare earth metal complex A, 10 μmol of isopropanol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 10 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0183] The conversion rate of nuclear magnetic resonance testing is 95%.

[0184] GPC analysis determined the number-average molecular weight M of polylactide. n It is 141,000, and the molecular weight distribution is M. w / M n It is 1.18.

[0185] Example 11

[0186] At room temperature, 10 μmol of rare earth metal complex B, 0.5 μmol of benzyl alcohol, 0.5 μmol of diphenylmethanol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free methods. 5 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 48 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0187] The conversion rate of nuclear magnetic resonance testing was 91%.

[0188] GPC analysis determined the number-average molecular weight M of polylactide. n It is 68,000, and the molecular weight distribution is M. w / M n It is 1.23.

[0189] Example 12

[0190] At room temperature, 10 μmol of rare earth metal complex A, 10 μmol of benzyl alcohol and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free solvent. 1 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0191] The conversion rate of nuclear magnetic resonance testing was 85%.

[0192] GPC analysis determined the number-average molecular weight M of polylactide. n It is 32,000, and the molecular weight distribution is M. w / M n It is 1.22.

[0193] Comparative Example 1

[0194] At room temperature, 10 μmol of rare earth metal complex A and 10 mL of tetrahydrofuran solvent were added to a 20 mL polymerization flask that had been treated with anhydrous and oxygen-free conditions. 1 mmol of L,D-lactide monomer was added, and the mixture was stirred at room temperature for 1 h. Then, an ethanol solution of 10 v% hydrochloric acid was added to terminate the reaction. The reaction solution was poured into ethanol to settle and filtered to obtain a white solid. The white solid was dried in a vacuum drying oven at 40 °C for 48 h to obtain polylactide solid.

[0195] The conversion rate of nuclear magnetic resonance testing was 79%.

[0196] GPC analysis determined the number-average molecular weight M of polylactide. n It is 12,000, and the molecular weight distribution is M. w / M n It is 1.35.

[0197] As can be seen from the above embodiments, when the catalyst composition provided by the present invention is used for the ring-opening polymerization of lactide to prepare polylactide, it not only has high catalytic activity, but also produces a polymer with a high molecular weight, adjustable molecular weight, and narrow molecular weight distribution.

[0198] By comparing Example 1 with Comparative Example 1, it can be seen that when the catalyst composition provided by the present invention is used for the ring-opening polymerization of lactide to prepare polylactide, the conversion rate is significantly improved (that is, the catalytic activity is significantly improved) and the number-average molecular weight is significantly improved.

[0199] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A catalyst composition, characterized in that, The catalyst composition contains a rare earth metal complex with the structure shown in formula (I) and a hydroxyl-containing compound. Equation (I) In formula (I), Ln is selected from scandium, yttrium or lanthanide metals, R1-R6 are each independently selected from hydrogen or C1-C3 alkyl groups; R7 is selected from hydrogen or C1-C3 alkyl groups or halogens; R8 is trimethylsilylmethylene or hexamethyldisilazane, and the hydroxyl-containing compound is at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, diphenylmethanol, triphenylmethanol and benzyl alcohol, and the molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.01-500.

2. The catalyst composition according to claim 1, wherein, The Ln is selected from scandium or yttrium; R1-R5 are hydrogen; R6 is methyl, ethyl or isopropyl; R7 is hydrogen or chlorine.

3. The catalyst composition according to claim 1 or 2, wherein, The rare earth metal complex with the structure shown in formula (I) is selected from at least one of the following complexes: In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene; In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene. In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazine. In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane.

4. The catalyst composition according to claim 1 or 2, wherein, The molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.1-100.

5. The catalyst composition according to claim 4, wherein, The molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.1-50.

6. A method for preparing polylactide, characterized in that, The preparation method includes: a step of solution polymerization of lactide monomers in the presence of a rare earth metal complex with the structure shown in formula (I) and a hydroxyl-containing compound. Equation (I) In formula (I), Ln is selected from scandium, yttrium or lanthanide metals, R1-R6 are each independently selected from hydrogen or C1-C3 alkyl groups; R7 is selected from hydrogen or C1-C3 alkyl groups or halogens; R8 is trimethylsilylmethylene or hexamethyldisilazane, and the hydroxyl-containing compound is at least one of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, ethylene glycol, diphenylmethanol, triphenylmethanol and benzyl alcohol, and the molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.01-500.

7. The method according to claim 6, wherein, The Ln is selected from scandium or yttrium.

8. The method according to claim 7, wherein, The Ln is selected from scandium or yttrium; R1-R5 are hydrogen; R6 is methyl, ethyl or isopropyl; R7 is hydrogen or chlorine; R8 is trimethylsilylmethylene or hexamethyldisilazine.

9. The method according to claim 8, wherein, The rare earth metal complex with the structure shown in formula (I) is selected from at least one of the following complexes: In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is methyl, R7 is hydrogen, and R8 is trimethylsilylmethylene; In formula (I), Ln is a complex of scandium, R1-R5 are hydrogen, R6 is ethyl, R7 is hydrogen, and R8 is trimethylsilylmethylene. In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is isopropyl, R7 is hydrogen, and R8 is hexamethyldisilazine. In formula (I), Ln is a complex of yttrium, R1-R5 are hydrogen, R6 is methyl, R7 is chlorine, and R8 is hexamethyldisilazane.

10. The method according to any one of claims 6-9, wherein, The conditions for solution polymerization include: a reaction temperature of 10-160℃ and a reaction time of 0.02-24h.

11. The method according to claim 10, wherein, The conditions for solution polymerization include: a reaction temperature of 25-100℃ and a reaction time of 0.1-3h.

12. The method according to any one of claims 6-9, wherein, The molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.1-100; And / or, the molar ratio of the hydroxyl-containing compound to the lactide monomer is 1:20-8000; And / or, the molar ratio of the rare earth metal complex to the lactide monomer is 1:50-3000.

13. The method according to any one of claims 6-9, wherein, The molar ratio of the rare earth metal complex to the hydroxyl-containing compound is 1:0.1-50; And / or, the molar ratio of the hydroxyl-containing compound to the lactide monomer is 1:20-6000; And / or, the molar ratio of the rare earth metal complex to the lactide monomer is 1:100-2500.

14. The method according to any one of claims 6-9, wherein, The molar ratio of the hydroxyl-containing compound to the lactide monomer is 1:20-5000; And / or, the molar ratio of the rare earth metal complex to the lactide monomer is 1:100-2000.

15. The method according to claim 14, wherein, The molar ratio of the hydroxyl-containing compound to the lactide monomer is 1:500-5000.

16. Use of the catalyst composition according to any one of claims 1-5 in the preparation of polylactide.

Citation Information

Patent Citations

  • Polylactide preparation method regulated and controlled by organic small molecule catalysts

    CN105273175A