Polymer electrolyte membrane with high ionic conductivity and preparation method thereof

By blending ethoxybisphenol A type diacrylate crosslinking agent with PEO to form a three-dimensional crosslinking network, the problems of low conductivity and narrow electrochemical window of PEO-based polymer electrolytes are solved, and an electrolyte membrane with high ionic conductivity, wide electrochemical window and excellent mechanical strength is realized, which is suitable for the simple preparation of high energy density solid-state lithium batteries.

CN121035327APending Publication Date: 2025-11-28HUANGGANG NORMAL UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510446334.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-10
Publication Date
2025-11-28

AI Technical Summary

Technical Problem

Existing PEO-based polymer electrolytes suffer from low room-temperature ionic conductivity, narrow electrochemical window, and industrialization challenges, making it difficult to simultaneously achieve high ionic conductivity, wide voltage window, and simple preparation process.

Method used

An electrolyte membrane with high ionic conductivity, wide electrochemical window and excellent mechanical strength is formed by blending ethoxybisphenol A type diacrylate crosslinking agent with polyethylene oxide (PEO) and then curing it with ultraviolet light. This avoids the use of plasticizers or inorganic fillers.

Benefits of technology

A polymer electrolyte membrane with high ionic conductivity (>10-4 S/cm), wide electrochemical window (≥4.5V) and excellent mechanical strength has been developed, which is suitable for high energy density solid-state lithium batteries, simplifies the preparation process, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121035327A_ABST
    Figure CN121035327A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer electrolyte membrane materials, and particularly relates to a high-ionic-conductivity polymer electrolyte membrane and a preparation method thereof.The preparation method comprises the steps that 1, PEO and lithium salt are added into a polar aprotic solvent, and the mixture is rapidly and violently stirred to be completely dissolved; (2) adding a cross-linking agent and a photoinitiator into the mixed solution, and violently stirring to obtain a mixed solution; and (3) coating the mixed solution in a polytetrafluoroethylene template, heating to remove the solvent, and performing ultraviolet radiation. According to the invention, a three-dimensional cross-linked network is formed by photocuring of an acrylate group of the cross-linking agent, PEO chain segment crystallization is inhibited, and lithium salt anions (such as TFSI-) are physically embedded. A benzene ring structure in a cross-linked network endows the electrolyte membrane with flexibility, mechanical property deterioration caused by a plasticizer or a diluent is avoided, the compact structure of the electrolyte membrane can inhibit lithium dendrite growth, the ionic conductivity reaches 1.7 * 10 <-4 > S / cm, and the electrochemical window reaches 4.9 V. The method is simple in process and suitable for large-scale preparation of the high-energy-density solid-state lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application belongs to the technical field of polymer electrolyte, and particularly relates to a polymer electrolyte film with high ionic conductivity and a preparation method thereof. BACKGROUND

[0002] With the increasing demand for high energy density and high safety energy storage, solid-state lithium metal batteries have become the core development direction in the field of new energy. Polyethylene oxide (PEO) based polymer electrolyte is considered as one of the important candidate materials for solid-state battery electrolyte due to its excellent flexibility, good interface compatibility with lithium metal negative electrode and simple processing technology. However, the PEO-based electrolyte in the prior art still has defects such as low room temperature ionic conductivity (10 -6 ~ 10 -5 S / cm) and narrow electrochemical window (<4.0V), which seriously restricts its practical application

[0003] The existing modification technology generally faces the problem of performance balance: for example, when the ionic conductivity is improved by plasticizer or inorganic filler composite, it often leads to significant decrease in mechanical strength or deterioration of interface stability. Literature 1 "Cross-linking network based on Poly(ethylene oxide): Solid polymer electrolyte for room temperature lithium battery. 2019, 420: 63-72." and Literature 2 "UV-derived double crosslinked PEO-based solid polymer electrolyte for room temperature. Journal of Colloid and Interface Science, 2023, 629: 492-500." both use plasticizers such as TEGDME to soften the polymer, but the polymer shrinkage rate of the system is easy to increase, which is not conducive to mass production; Literature 3 "Ultrathin PEO based electrolyte for high voltage lithium metal batteries enabled by polymer host-plasticizer interactions. Journal of Energy Storage, 2023, 68: 107640." uses butanedinitrile as a plasticizer, which can inhibit PEO crystallization and significantly improve ionic conductivity, but it will significantly reduce the mechanical modulus of the electrolyte film and increase the risk of dendrite penetration; In addition, by compounding inorganic fillers (such as LATP, LLZO), the ionic conductivity is significantly improved, but the agglomeration of inorganic fillers easily leads to discontinuous ion transport path, especially the high addition amount (50-80wt%) of inorganic fillers easily causes phase separation, which is difficult to balance high ionic conductivity and interface performance, and increases production cost.

[0004] In summary, the existing PEO-based polymer electrolyte has advantages in interface compatibility and processability, but its performance bottlenecks (such as low ionic conductivity, narrow electrochemical window) and industrialization problems (such as complex modification process, high cost) have not been effectively solved. Therefore, it is urgent to develop a PEO-based electrolyte system with high ionic conductivity (up to 10 -4 S / cm), wide voltage window (>4.5V) and simple preparation process, to promote the practical breakthrough of solid-state battery technology. SUMMARY

[0005] To solve the above problems, the application provides a preparation method of a PEO-based electrolyte membrane based on bisphenol A type diacrylate crosslinking agent.The application provides the following technical scheme: an ethoxy bisphenol A diacrylate compound is used as a crosslinking agent, and is blended with polyethylene oxide (PEO) and a lithium salt (such as LiTFSI) to form a three-dimensional crosslinking network structure through ultraviolet light curing.The specific steps are as follows: (1) a three-dimensional network formed by a rigid benzene ring and an ether bond in the bisphenol A structure can physically embed lithium salt anions (such as TFSI-), thereby significantly improving lithium ion transference number (verified by experiments );(2) the crosslinking structure effectively inhibits PEO chain segment crystallization, improves the proportion of amorphous regions, and avoids the use of plasticizers or active diluents, so that a homogeneous electrolyte membrane with high ionic conductivity (>10 -4 S / cm), a wide electrochemical window (≥4.5V) and excellent mechanical strength is finally prepared, and the electrolyte membrane is suitable for high-energy-density solid-state lithium batteries.

[0006] According to a first aspect of the application, the application first provides a high-ionic-conductivity polymer electrolyte membrane and a preparation method thereof, which comprises the following steps:

[0007] (1) PEO is dissolved in a polar aprotic solvent, and is rapidly and intensively stirred until completely dissolved to obtain a solution A;

[0008] (2) the crosslinking agent, the lithium salt and the photoinitiator are sequentially added to the solution A, and are intensively stirred until completely dissolved to obtain a mixed solution B.

[0009] (3) photocrosslinking: the mixed solution B is coated on a polytetrafluoroethylene template, is heated to remove the solvent, and is irradiated with ultraviolet light to obtain a solid polymer electrolyte membrane.

[0010] According to an embodiment of the application, the PEO in step (1) has a molecular weight of 30-60w, and the polar aprotic solvent is acetonitrile, wherein the PEO and the acetonitrile need to be dried in advance.

[0011] According to an embodiment of the application, the photocrosslinking agent in step (2) is any one of 3(ethoxy) bisphenol A diacrylate, 4(ethoxy) bisphenol A diacrylate, 10(ethoxy) bisphenol A diacrylate, 20(ethoxy) bisphenol A diacrylate and 30(ethoxy) bisphenol A diacrylate.

[0012] According to an embodiment of the application, the lithium salt in step (2) is one or more of lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium trifluoromethylsulfonate (LiCF3SO3), lithium bis(trifluoromethylsulfonate)imide (LiTFSI) and lithium bisfluorosulfonylimide (LiFSI).

[0013] According to one embodiment of the present invention, the photoinitiator in step (2) is any one of benzophenone, 4-methylbenzophenone, and 2,2-dimethoxy-2-phenylacetophenone (DMPA).

[0014] According to one embodiment of the present invention, the mass ratio of PEO: lithium salt: crosslinking agent: photoinitiator in step (2) is (0.3-0.5):(0.08-0.15):(0.1-0.2):(0.04-0.08), wherein the molar ratio of PEO structural unit to Li is (20-24):1.

[0015] According to one embodiment of the present invention, the mixing process in step (2) is as follows: in a glove box where the water and oxygen content are both less than 0.1 ppm, a crosslinking agent, a lithium salt and an initiator are added to the PEO solution in sequence and stirred vigorously until completely dissolved. The initiator needs to be pre-powdered.

[0016] According to one embodiment of the present invention, the photocrosslinking process in step (3) is as follows: the mixed solution is coated onto a polytetrafluoroethylene template at room temperature, then degassed and kept at 60°C for 2-4 hours to remove the solvent, and then irradiated with ultraviolet light for 5-15 minutes while hot to obtain a polymer electrolyte membrane.

[0017] According to one embodiment of the present invention, the polymer electrolyte membrane prepared by the preparation method according to any one of claims 1-8 has a membrane thickness of 50-150 μm and an ionic conductivity of 0.05-1.7 × 10⁻⁶. -4 S / cm, electrochemical window >4.5V.

[0018] According to another aspect of the present invention, the present invention also provides a solid electrolyte membrane prepared by the above method, wherein the lithium ion transference number of the solid electrolyte membrane reaches 0.58.

[0019] According to another aspect of the present invention, the present invention also provides the application of the above-described solid electrolyte membrane in lithium-ion batteries.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) Synergistic improvement of ionic conductivity and mechanical strength: The three-dimensional cross-linking network constructed by ethoxybisphenol A diacrylate cross-linking agent destroys the PEO crystalline region to increase the proportion of amorphous phase, which is beneficial to improve the room temperature ionic conductivity; at the same time, it overcomes the strength loss problem caused by traditional plasticizers or inorganic fillers, and utilizes the synergistic effect of benzene ring rigid skeleton and cross-linking structure to make the electrolyte membrane flexible.

[0022] (2) Wide electrochemical window and enhanced interfacial stability: The cross-linked network restricts anion migration through physical embedding, thereby improving ionic conductivity. Its dense structure can suppress lithium dendrite growth and improve the electrochemical window.

[0023] (3) Advantages of simplified process and homogeneous structure: The photocuring crosslinking process is formed in one step, avoiding the phase separation problem that is easily caused by the traditional blending method, and is suitable for large-scale production. Attached Figure Description

[0024] Figure 1 An optical photograph of the PEO-based polymer electrolyte prepared in Example 1.

[0025] Figure 2 The flexibility of the PEO-based polymer electrolyte prepared in Example 1.

[0026] Figure 3 The results show the ionic conductivity of the PEO-based polymer electrolyte prepared in Example 2.

[0027] Figure 4 The results are the electrochemical stability window test results for Example 2 and Comparative Example 1.

[0028] Figure 5 The lithium-ion transference number is the PEO-based polymer electrolyte prepared in Example 3. Detailed Implementation

[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0030] This invention provides a polymer electrolyte membrane with high ionic conductivity and a method for preparing the same, comprising the following steps:

[0031] (1) Dissolve PEO in a polar aprotic solvent and stir rapidly and vigorously until completely dissolved to obtain solution A;

[0032] (2) The crosslinking agent, lithium salt and photoinitiator are added to the above solution A in sequence and stirred vigorously until completely dissolved to obtain mixed solution B.

[0033] (3) Photocrosslinking: The above mixed solution B is coated on a polytetrafluoroethylene template, heated to remove the solvent, and then irradiated with ultraviolet light to obtain a solid polymer electrolyte membrane.

[0034] In some embodiments, the molecular weight of PEO in step (1) is 30-60w, and the polar aprotic solvent is acetonitrile. PEO and acetonitrile need to be pre-dried.

[0035] It should be noted that after PEO is dissolved in acetonitrile, it needs to be stirred rapidly at a speed of up to 30,000 rpm, thereby effectively shortening the stirring time to within half an hour.

[0036] In some embodiments, the photocrosslinking agent in step (2) is any one of 3(ethoxy)bisphenol A diacrylate, 4(ethoxy)bisphenol A diacrylate, 10(ethoxy)bisphenol A diacrylate, 20(ethoxy)bisphenol A diacrylate, and 30(ethoxy)bisphenol A diacrylate.

[0037] In some embodiments, the lithium salt in step (2) is one or more of lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonate)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI).

[0038] It should be noted that, in specific implementations, lithium salt LiTFSI is preferred.

[0039] In some embodiments, the photoinitiator in step (2) is any one of benzophenone, 4-methylbenzophenone, and 2,2-dimethoxy-2-phenylacetophenone (DMPA).

[0040] In some embodiments, the mass ratio of PEO: lithium salt: crosslinking agent: photoinitiator in step (2) is (0.3-0.5): (0.08-0.15): (0.1-0.2): (0.04-0.08), wherein the molar ratio of PEO structural units to Li is (20-24):1.

[0041] In some embodiments, the mixing process in step (2) is as follows: in a glove box where the water and oxygen content are both less than 0.1 ppm, a crosslinking agent, a lithium salt and an initiator are added to the PEO solution in sequence and stirred vigorously until completely dissolved. The initiator needs to be pre-powdered.

[0042] In some embodiments, the photocrosslinking process in step (3) is as follows: the mixed solution is coated onto a polytetrafluoroethylene template at room temperature, then degassing is performed and the solution is kept at 60°C for 2 to 4 hours to remove the solvent. After being heated and irradiated with ultraviolet light for 5 to 15 minutes, the polymer electrolyte membrane is obtained.

[0043] In some embodiments, the polymer electrolyte membrane prepared by the preparation method according to any one of claims 1-8 has a membrane thickness of 50-150 μm and an ionic conductivity as high as 1.7 × 10⁻⁶. -4 S / cm, the electrochemical window can be extended to 5V.

[0044] The following are specific examples:

[0045] Example 1

[0046] A polymer electrolyte membrane with high ionic conductivity and its preparation method are disclosed, which are prepared by the following steps:

[0047] (1) Dissolve 0.3g PEO (molecular weight 300,000) in 6ml acetonitrile and stir rapidly and vigorously for 30min to obtain PEO solution;

[0048] (2) In a glove box where the water and oxygen content are both less than 0.1 ppm, 0.1 g of 10 (ethoxy) bisphenol A diacrylate, 0.08 g of LiTFSI and 0.04 g of benzophenone are added to the PEO solution in sequence and stirred vigorously until completely dissolved to obtain mixed solution B.

[0049] (3) Photocrosslinking: The above mixed solution B was coated onto a polytetrafluoroethylene template, degassed, and kept at 60°C for 2 hours to remove the solvent. After being heated and irradiated with ultraviolet light for 15 minutes, the polymer electrolyte membrane was obtained. Its optical photographs and tensile diagrams are shown below. Figure 1 and Figure 2 As shown, a flexible polymer electrolyte film was successfully prepared with a tensile strain exceeding 70%. The film thickness was 50 μm.

[0050] Example 2

[0051] (1) Dissolve 0.3g PEO (molecular weight 300,000) in 6ml acetonitrile and stir rapidly and vigorously for 30min to obtain PEO solution;

[0052] (2) In a glove box where the water and oxygen content are both less than 0.1 ppm, 0.1 g of 4-(ethoxy)bisphenol A diacrylate, 0.08 g of LiTFSI and 0.04 g of benzophenone were added to the PEO solution in sequence and stirred vigorously until completely dissolved to obtain mixed solution B.

[0053] (3) Photocrosslinking: The above mixed solution B was coated onto a polytetrafluoroethylene template, degassed, and kept at 60℃ for 2 hours to remove the solvent. After being heated and irradiated with ultraviolet light for 15 minutes, the polymer electrolyte membrane was obtained. Its ionic conductivity test results and electrochemical window analysis are as follows: Figure 3 and Figure 4As shown, a polymer electrolyte membrane with high ionic conductivity was successfully prepared, with a film thickness of 150 μm and a room temperature ionic conductivity as high as 1.7 × 10⁻⁶. -4 S / cm, electrochemical window >4.9V.

[0054] Example 3

[0055] (1) Dissolve 0.3g PEO (molecular weight of 600,000) in 6ml acetonitrile and stir rapidly and vigorously for 30min to obtain PEO solution;

[0056] (2) In a glove box where the water and oxygen content are both less than 0.1 ppm, 0.1 g of 4-(ethoxy)bisphenol A diacrylate, 0.08 g of LiTFSI and 0.04 g of benzophenone were added to the PEO solution in sequence and stirred vigorously until completely dissolved to obtain mixed solution B.

[0057] (3) Photocrosslinking: The above mixed solution B was coated onto a polytetrafluoroethylene template, degassed, and kept at 60°C for 2 hours to remove the solvent. After being heated and irradiated with ultraviolet light for 15 minutes, the polymer electrolyte membrane was obtained. Its lithium-ion transport number is as follows: Figure 5 As shown, the polymer electrolyte membrane has a thickness of 93 μm and a significantly increased lithium-ion transference number of 0.47.

[0058] Comparative Example 1

[0059] (1) Dissolve 0.3g PEO (molecular weight of 600,000) in 6ml acetonitrile and stir rapidly and vigorously for 30min to obtain PEO solution;

[0060] (2) In a glove box where the water and oxygen content are both less than 0.1 ppm, add 0.1 g LiTFSI to the PEO solution, where [EO]:Li = 24:1, and stir vigorously until completely dissolved to obtain mixed solution B.

[0061] (3) Photocrosslinking: The above mixed solution B was coated onto a polytetrafluoroethylene template, degassed, and kept at 60°C for 2 hours to remove the solvent. After being heated and irradiated with ultraviolet light for 15 minutes, the polymer electrolyte membrane was obtained. This membrane is extremely easy to break, resulting in difficulty in demolding. The membrane is colorless and transparent, and its thickness is 60 μm.

[0062] Comparative Example 2

[0063] (1) Dissolve 0.3g PEO (molecular weight 300,000) in 6ml acetonitrile and stir rapidly and vigorously for 30min to obtain PEO solution;

[0064] (2) In a glove box where the water and oxygen content are both less than 0.1 ppm, add 0.08 g of LiTFSI to the PEO solution, where [EO]:Li = 15:1, and stir vigorously until completely dissolved to obtain mixed solution B.

[0065] (3) Photocrosslinking: The above mixed solution B was coated onto a polytetrafluoroethylene template, degassed, and kept at 60°C for 2 hours to remove the solvent. After being heated and irradiated with ultraviolet light for 15 minutes, the polymer electrolyte membrane was obtained. The membrane was slightly sticky after drying, which may be due to the presence of excessive lithium salt, resulting in difficulty in demolding.

[0066] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A polymer electrolyte membrane with high ionic conductivity and its preparation method, characterized in that, Includes the following steps: (1) Dissolve PEO in a polar aprotic solvent and stir rapidly and vigorously until completely dissolved to obtain solution A; (2) Add the crosslinking agent, lithium salt and photoinitiator to the above solution A in sequence, and stir vigorously until completely dissolved to obtain mixed solution B. (3) Photocrosslinking: The above mixed solution B is coated on a polytetrafluoroethylene template, heated to remove the solvent, and then irradiated with ultraviolet light to obtain a solid polymer electrolyte membrane.

2. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, The molecular weight of PEO in step (1) is 30-60w, and the polar aprotic solvent is acetonitrile. PEO and acetonitrile need to be dried in advance.

3. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, The photocrosslinking agent in step (2) is any one of 3(ethoxy)bisphenol A diacrylate, 4(ethoxy)bisphenol A diacrylate, 10(ethoxy)bisphenol A diacrylate, 20(ethoxy)bisphenol A diacrylate, and 30(ethoxy)bisphenol A diacrylate.

4. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, The lithium salt mentioned in step (2) is one or more of lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalate-borate) (LiBOB), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonate)imide (LiTFSI), and lithium bis(fluorosulfonylimide) (LiFSI).

5. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, The photoinitiator in step (2) is any one of benzophenone, 4-methylbenzophenone, or 2,2-dimethoxy-2-phenylacetophenone (DMPA).

6. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, In step (2), the mass ratio of PEO: lithium salt: crosslinking agent: photoinitiator is (0.3~0.5):(0.08~0.15):(0.1~0.2):(0.04~0.08), and the molar ratio of PEO structural unit to Li is (20~24):

1.

7. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, The mixing process in step (2) is as follows: In a glove box where the water and oxygen content are both less than 0.1 ppm, a crosslinking agent, lithium salt and initiator are added to the PEO solution in sequence and stirred vigorously until completely dissolved. The initiator needs to be powdered beforehand.

8. The method for producing a polymer electrolyte membrane with high ionic conductivity according to claim 1, characterized in that, The photocrosslinking process in step (3) is as follows: the mixed solution is coated onto the polytetrafluoroethylene template at room temperature, then degassed and kept at 60°C for 2-4 hours to remove the solvent, and then irradiated with ultraviolet light for 5-15 minutes while hot to obtain the polymer electrolyte membrane.

9. A polymer electrolyte, characterized in that, The polymer electrolyte is prepared according to any one of claims 1-8, wherein the polymer electrolyte membrane has a thickness of 50–150 μm and an ionic conductivity of 0.05–1.7 × 10⁻⁶. -4 S / cm, electrochemical window >4.5V.

10. The application of a method for a polymer electrolyte membrane with high ionic conductivity as described in claim 9 in a lithium battery.

Citation Information

Cited By

  • Sulfur-containing polymer electrolyte and preparation method thereof

    CN121617833A

  • Sulfur-containing polymer electrolyte and method for preparing the same

    CN121617833B