Preparation method of h-BN / PI high-temperature-resistant anticorrosive coating
The preparation method of h-BN/PI composite coating solves the problem of easy decomposition of polymer coating under high temperature and high humidity conditions, and improves high temperature stability and corrosion resistance, making it suitable for long-term protection of aluminum alloy materials.
Patent Information
- Application Number
- CN202511455067.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-13
- Publication Date
- 2025-12-09
AI Technical Summary
Existing polymer coatings are prone to thermal decomposition and interfacial peeling under high temperature, high humidity or alternating stress conditions, which cannot effectively block corrosive media and lead to a decrease in the service life of aluminum alloy materials in complex environments.
The h-BN/PI composite coating was prepared by polymerizing the polyamic acid solution under an inert atmosphere. Micron-sized hexagonal boron nitride was ultrasonically exfoliated into a monolayer and mixed with the polyamic acid solution. The coating was then cured by gradient heating to form a dense coating, and the coating performance was enhanced by hydrogen bonds and π bonds.
It forms a coating with high-temperature stability and excellent corrosion resistance, which can effectively block the penetration of corrosive media in high-temperature environments, maintain interfacial adhesion, and extend the service life of aluminum alloy materials.
Smart Images

Figure CN121086658A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, and more specifically, to a method for preparing an h-BN / PI high-temperature resistant and corrosion-resistant coating. Background Technology
[0002] Aluminum alloys, due to their advantages such as low density, high specific strength, low elastic modulus, high thermal conductivity, and ease of processing, have been widely used in the automotive, aerospace, and natural gas drilling industries, becoming the preferred material for lightweight applications. However, aluminum alloys have poor corrosion resistance. In complex service environments such as high loads and humidity, under the combined action of corrosive media and load stress, aluminum alloys are prone to exfoliation, stress corrosion, and corrosion fatigue, leading to a reduction in the service life of the workpiece. This significantly limits their wider application. Therefore, effectively preventing corrosion of aluminum alloy materials is a crucial issue.
[0003] There are many methods for protecting metallic materials, such as cathodic protection, electroplating, corrosion inhibitor protection, and polymer coating protection. Considering all factors, polymer coating is the most economical, convenient, and effective method for protecting metallic materials. Polymer coatings can form a physical barrier on the metal surface, blocking and delaying the diffusion of corrosive media (such as oxygen, water, and Cl-) to the metal surface and their corrosive reaction. Common polymer coatings include epoxy, polyurethane, and acrylic types. Although they all have excellent anti-corrosion properties, their poor resistance to high and low temperatures and weathering limitations prevent them from meeting the requirements of some extreme environments, greatly restricting their wider application.
[0004] Although polyimide materials have excellent thermal stability and mechanical properties, they still have insufficient corrosion resistance when used as anti-corrosion coatings. Summary of the Invention
[0005] The present invention aims to solve the problem that the anti-corrosion performance and high and low temperature resistance of coatings cannot be achieved simultaneously.
[0006] To address the above problems, this invention provides a method for preparing an h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0007] This invention provides a method for preparing an h-BN / PI high-temperature resistant and corrosion-resistant coating, comprising the following steps: Under an inert atmosphere, an aromatic diamine containing a five-membered ring of heterogeneous elements and an aromatic dianhydride containing an ether bond are polymerized in a polar aprotic solvent to obtain a polyamic acid solution. Micron-sized hexagonal boron nitride was subjected to ultrasonic-assisted liquid-phase exfoliation to obtain a single layer of hexagonal boron nitride. A single layer of hexagonal boron nitride was added to a polyamic acid solution in multiple portions and stirred until homogeneous to obtain a hexagonal boron nitride / polyimide composite solution. Hexagonal boron nitride / polyimide composite liquid is applied to the surface to be coated and cured by gradient temperature increase to obtain h-BN / PI high temperature resistant and anti-corrosion coating.
[0008] Optionally, the aromatic diamine is 2-(4-aminophenyl)-5-aminobenzoxazole, and the aromatic dianhydride is bisphenol A type diether dianhydride.
[0009] Optionally, the molar ratio of aromatic diamine to aromatic dianhydride is 1:2 to 2:1.
[0010] Optionally, the polar aprotic solvent includes one of N-methyl-2-pyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0011] Optionally, in the hexagonal boron nitride / polyimide composite solution, the mass fraction of the monolayer hexagonal boron nitride is from 0.5 wt% to 7 wt%.
[0012] Optionally, the solid content of the polyamic acid solution is 23%.
[0013] Optionally, during the polymerization reaction, the reaction temperature is 20 to 25°C and the reaction time is 24 to 28 hours.
[0014] Optionally, gradient temperature curing includes: holding at 70-90℃ for 1 to 2 hours, raising the temperature to 110-130℃ and holding for 1 to 2 hours, raising the temperature to 140-160℃ and holding for 1 to 2 hours, raising the temperature to 170-190℃ and holding for 1 to 2 hours, raising the temperature to 200-220℃ and holding for 1 to 2 hours, raising the temperature to 230-250℃ and holding for 1 to 2 hours, and raising the temperature to 270-290℃ and holding for 1 to 2 hours.
[0015] Optionally, the micron-sized hexagonal boron nitride is subjected to ultrasonic-assisted liquid-phase exfoliation, including: ultrasonic-assisted liquid-phase exfoliation of the micron-sized hexagonal boron nitride in a solution of isopropanol and water in a volume ratio of 1:1 for more than 1 hour, followed by vacuum filtration to obtain a monolayer of hexagonal boron nitride, washing the monolayer of hexagonal boron nitride with deionized water, and vacuum drying at 50 to 70°C for 9 to 11 hours.
[0016] Optionally, the monolayer hexagonal boron nitride is added to the polyamic acid solution in multiple portions and stirred until homogeneous, including: adding the monolayer hexagonal boron nitride to the polyamic acid solution in four to six portions and mechanically stirring for more than 12 hours.
[0017] The beneficial effects of the preparation method of the h-BN / PI high-temperature resistant and anti-corrosion coating of the present invention are as follows: Aromatic diamines containing a five-membered ring with heterogeneous elements participate in the polymerization reaction. The five-membered ring has a more stable structure than the benzene ring, which can improve the high-temperature resistance of polyimide (PI). The hydrogen bonds formed by the introduction of nitrogen and heterogeneous elements can jointly enhance the high-temperature resistance of polyimide with rigid molecular chain segments. Introducing ether bonds into the molecular structure, since ether bonds are flexible groups, can provide flexible molecular chains in the polyimide adhesive molecular structure, enhancing the polyimide's spatial mobility and making it more conducive to casting and spreading on the substrate surface, thus improving the mechanical properties of the polyimide composite coating. The introduction of micron-sized hexagonal boron nitride (HBO) with a wide aspect ratio and good ability to inhibit the penetration and diffusion of corrosive substances into the polyimide further enhances its high-temperature resistance. Boron nitride (h-BN) has abundant nitrogen-hydrogen bonds on its surface, forming multiple intermolecular hydrogen bond interactions with polyimide. On the other hand, localized large π bonds exist in boron nitride, which interact with the conjugated system in the polyimide molecular chain. An appropriate amount of hexagonal boron nitride can be uniformly dispersed in polyimide, thereby constructing a three-dimensional network structure inside the polyimide, thus improving the performance of the coating. Therefore, the high-temperature resistant and corrosion-resistant coating of h-BN / PI based on multiple hydrogen bond interactions of polyimide adhesive has better high-temperature resistance, better kinetic properties, and excellent corrosion resistance. Attached Figure Description
[0018] Figure 1 This is a flowchart illustrating the preparation method of the h-BN / PI high-temperature resistant and corrosion-resistant coating according to an embodiment of the present invention; Figure 2 The image shows the surface SEM microstructure of the h-BN / PI composite coating prepared in Example 3. Figure 3 The infrared spectrum of the h-BN / PI composite coating prepared in Example 3; Figure 4 The DSC spectrum of the h-BN / PI composite film prepared in Example 3; Figure 5 The image shows the nanoindentation test curve of the h-BN / PI composite coating prepared in Example 3. Figure 6 Figure 1 is a schematic diagram of the surface of an aluminum alloy after coating with the h-BN / PI composite film prepared in Example 3; Figure 6 Figure 2 shows a schematic diagram of the surface of the h-BN / PI composite film prepared in Example 3 after a 20-day neutral salt spray test; Figure 6 Figure 3 shows a schematic diagram of the surface of the h-BN / PI composite film prepared in Example 3 after a 40-day neutral salt spray test; Figure 7The DSC spectrum of the polyimide prepared in Comparative Example 1 is shown. Figure 8 Nanoindentation test curves of the PI coating prepared in Comparative Example 1. Figure 9 Figure 1 is a schematic diagram of the surface of an aluminum alloy after coating with the PI film of Comparative Example 1. Figure 9 Figure 2 shows a schematic diagram of the surface of the PI coating of Comparative Example 1 after a 20-day neutral salt spray test. Detailed Implementation
[0019] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Although some embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the accompanying drawings and embodiments of the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.
[0020] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this invention's description is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. As used herein, the term "comprising" and its variations are open-ended, meaning "including but not limited to"; the term "based on" means "at least partially based on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one additional embodiment"; the term "some embodiments" means "at least some embodiments"; and the term "optionally" means "optional embodiments". Definitions of other terms will be given in the description below. In the description of this application, unless otherwise stated, "a plurality of" means two or more.
[0021] In related technologies, the field of metal surface protection has long relied on traditional polymer coatings such as epoxy resin and polyurethane. These materials have good anti-corrosion performance under normal conditions, but they are prone to thermal decomposition and interfacial peeling under high temperature, high humidity, or alternating stress conditions, leading to protective failure. Surface coatings for aerospace engine components generally suffer from insufficient temperature resistance and mismatched coefficients of thermal expansion under continuous high-temperature exhaust, making it impossible to form a long-term effective barrier against corrosive media.
[0022] To address the problems existing in the aforementioned related technologies, this invention provides a method for preparing an h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0023] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing an h-BN / PI high-temperature resistant and corrosion-resistant coating, comprising the following steps: Under an inert atmosphere, an aromatic diamine containing a five-membered ring of heterogeneous elements and an aromatic dianhydride containing an ether bond are polymerized in a polar aprotic solvent to obtain a polyamic acid solution. Micron-sized hexagonal boron nitride was subjected to ultrasonic-assisted liquid-phase exfoliation to obtain a single layer of hexagonal boron nitride. A single layer of hexagonal boron nitride was added to a polyamic acid solution in multiple portions and stirred until homogeneous to obtain a hexagonal boron nitride / polyimide composite solution. Hexagonal boron nitride / polyimide composite liquid is applied to the surface to be coated and cured by gradient temperature increase to obtain h-BN / PI high temperature resistant and anti-corrosion coating.
[0024] It should be noted that the first step can be performed before or after the second step, or the two can be performed simultaneously.
[0025] In this embodiment, an aromatic diamine containing a five-membered ring with heteroelemental elements participates in the polymerization reaction. The five-membered ring has a more stable structure than the benzene ring, which can improve the high-temperature resistance of polyimide (PI). The hydrogen bonds formed by the introduction of nitrogen and heteroelemental elements can enhance the high-temperature resistance of polyimide together with the rigid molecular chain segments. Introducing ether bonds into the molecular structure, since ether bonds are flexible groups, can provide flexible molecular chains in the polyimide adhesive molecular structure, enhancing the polyimide's spatial mobility and facilitating its casting and spreading on the substrate surface, thus improving the mechanical properties of the polyimide composite coating. The introduction of micron-sized hexagonal boron nitride, which has a wide aspect ratio and good ability to inhibit the penetration and diffusion of corrosive substances, into the polyimide further enhances its high-temperature resistance. Boron nitride (h-BN) has abundant nitrogen-hydrogen bonds on its surface, forming multiple intermolecular hydrogen bond interactions with polyimide. On the other hand, localized large π bonds exist in boron nitride, which interact with the conjugated system in the polyimide molecular chain. An appropriate amount of hexagonal boron nitride can be uniformly dispersed in polyimide, thereby constructing a three-dimensional network structure inside the polyimide, thus improving the performance of the coating. Therefore, the high-temperature resistant and corrosion-resistant coating of h-BN / PI based on multiple hydrogen bond interactions of polyimide adhesive has better high-temperature resistance, better kinetic properties, and excellent corrosion resistance.
[0026] Specifically, micron-sized hexagonal boron nitride has a wide aspect ratio, electrical insulation, and good ability to inhibit the penetration and diffusion of corrosive substances, thus improving the barrier performance of organic coatings. Hexagonal boron nitride forms multiple hydrogen bonds with the imide bonds in polyimide and the nitrogen and oxygen elements in diamine, which enhances the compatibility between inorganic fillers and polyimide.
[0027] Specifically, inert atmosphere protection refers to conducting the polymerization reaction in a nitrogen or argon atmosphere, which can be achieved using a glove box to prevent oxygen and moisture from interfering with the polycondensation process. Polar aprotic solvents are organic solvents with high dielectric constants but no active hydrogen, such as N-methylpyrrolidone, ensuring complete monomer dissolution and maintaining the homogeneity of the reaction system. Ultrasonic-assisted liquid-phase exfoliation utilizes high-frequency mechanical waves to break the van der Waals forces between layers, which can be achieved using a probe-type ultrasonic instrument in conjunction with an alcohol-water mixture, effectively obtaining a single-layer nanosheet structure. Multiple additions refer to the staged incorporation of nanofillers into the matrix solution, which can be achieved using a four- to six-stage interval feeding method to avoid excessively high local concentrations that could lead to agglomeration. Gradient temperature curing refers to staged, programmed temperature control of the coating, which can be achieved using an eight-stage stepped heating program to promote solvent evaporation and orderly molecular chain arrangement.
[0028] Monomer polycondensation in a nitrogen atmosphere ensures the orderly growth of linear polyamic acid chains, laying the structural foundation for subsequent imidization. The monolayer hexagonal boron nitride obtained through optimized ultrasonic parameters possesses a complete lattice structure, and its two-dimensional plane effectively extends the penetration path of corrosive media. Batch mechanical stirring allows the nanosheets to be uniformly embedded in the polymer matrix, forming a three-dimensional interlaced barrier network. The step-curing process first removes residual solvent at a low temperature, then completes the imidization ring-closure reaction at a medium temperature, and finally achieves molecular chain rearrangement and stress release at a high temperature, forming a defect-free, dense coating structure.
[0029] This embodiment significantly enhances the interfacial compatibility of the two phases through in-situ composite of nanosheets and polymers. Conventional curing processes employ single-stage high-temperature treatment, which is prone to microcracks, while a gradient heating strategy effectively controls the phase transformation process and reduces thermal stress accumulation. A three-dimensional barrier network with high-temperature stability was successfully constructed, forming a continuous and dense protective layer on the metal surface. This coating effectively inhibits oxygen and water vapor penetration in high-temperature corrosive environments while maintaining excellent interfacial adhesion. By controlling the dispersion state of the nanofillers and the crosslinking density of the matrix, a balance between the mechanical properties and anti-corrosion performance of the coating is achieved, meeting the long-term protection requirements under complex working conditions.
[0030] Optionally, the aromatic diamine is 2-(4-aminophenyl)-5-aminobenzoxazole, and the aromatic dianhydride is bisphenol A type diether dianhydride.
[0031] In this optional embodiment, the five-membered ring containing both oxygen and nitrogen elements enhances the conjugation effect between the benzene ring and the imide in the polyimide, thereby increasing the bond energy. Through a specific combination of rigid diamine and flexible dianhydride, a rigid-flexible balance is achieved at the molecular level, overcoming the performance defects caused by a single structure.
[0032] Through the above technical solution, the polyimide matrix formed in this application can still maintain the density of the coating at a high temperature of 300℃, effectively blocking the penetration of corrosive media. At the same time, the moderate flexibility of the molecular chain relieves the thermal cycling stress, enabling the coating to achieve long-term stable high-temperature anti-corrosion protection on the aluminum alloy surface.
[0033] Specifically, 2-(4-aminophenyl)-5-aminobenzoxazole refers to a rigid diamine monomer containing a benzoxazole ring, which can be prepared by organic synthesis. The conjugated structure of its benzoxazole ring enhances the planarity and packing density of the polyimide molecular chain. Bisphenol A-type diether dianhydride refers to a dianhydride monomer containing a bisphenol A backbone and ether bonds, which can be obtained through the condensation reaction of bisphenol A with an acid anhydride. Its ether bonds impart moderate flexibility to the molecular chain, and the steric hindrance effect of bisphenol A inhibits excessively tight packing of the molecular chain.
[0034] Specifically, the rigid structure of the benzoxazole ring enhances the inter-chain interactions through π-π conjugation, enabling the polyimide to form an ordered layered structure during high-temperature curing. The ether bonds of the bisphenol A-type diether dianhydride maintain the flexibility of the molecular chains, while the bisphenol A side groups prevent excessive chain stacking through steric hindrance, forming a network structure with microphase separation characteristics. The synergistic effect of the two monomers allows the polyimide matrix to maintain structural integrity at high temperatures while releasing thermal stress through flexible segments, thereby reducing interfacial cracking caused by differences in thermal expansion coefficients during coating curing.
[0035] Optionally, the molar ratio of aromatic diamine to aromatic dianhydride is 1:2 to 2:1.
[0036] In this optional embodiment, by using a dynamically balanced molar ratio range, excessive monomer residue is avoided while ensuring sufficient molecular chain extension, resulting in a continuous polyimide matrix that effectively blocks the penetration of corrosive media. This solves the coating defect problem caused by monomer ratio imbalance during the synthesis of polyamic acid precursors. By precisely controlling the stoichiometric relationship of reactants, a structurally complete three-dimensional polyimide network is obtained, enabling the coating to maintain a stable physical barrier effect under high-temperature environments, significantly improving the anti-corrosion protection effect on aluminum alloy substrates.
[0037] Specifically, aromatic diamines refer to aromatic compounds containing two amino groups, such as 2-(4-aminophenyl)-5-aminobenzoxazole, which are monomers with rigid molecular structures. Their amino groups can undergo condensation polymerization with acid anhydrides to form polyamic acids. Aromatic dianhydrides refer to aromatic compounds containing two anhydride groups, such as bisphenol A-type diether dianhydrides, which are monomers with symmetrical structures. Their anhydride groups react with amino groups after ring opening to form amide bonds. This molar ratio range ensures sufficient cross-linking of active functional groups in the reaction system by controlling the stoichiometric balance between amino and anhydride groups.
[0038] When the molar ratio is below 1:2, excess anhydride may result in unreacted anhydride residue in the polyamic acid, producing byproducts that compromise the coating's density during subsequent curing. When the molar ratio is above 2:1, excess diamine may leave amino groups at the molecular chain ends, causing chain breakage during high-temperature curing. Controlling the molar ratio within the range of 1:2 to 2:1 allows for an equimolar reaction between amino and anhydride groups, forming a polyamic acid precursor with a uniform molecular weight distribution. This precursor, during gradient heating, generates a polyimide with a three-dimensional network structure through a ring-closed reaction. Its well-ordered molecular chain arrangement effectively enhances the coating's thermal stability and resistance to media penetration.
[0039] Optionally, the polar aprotic solvent includes one of N-methyl-2-pyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0040] In this optional embodiment, the polar aprotic solvent used suppresses side reactions and maintains system homogeneity, providing a foundation for the uniform dispersion of hexagonal boron nitride and the ordered arrangement of polyimide molecular chains during the gradient curing process. This solves the problems of poor polymerization reaction stability and coating structural defects caused by improper solvent selection, achieving efficient preparation of polyamic acid solution, and thus ensuring that the coating has dense and corrosion-resistant properties after high-temperature curing.
[0041] Specifically, polar aprotic solvents refer to organic solvents with high dielectric constants that do not contain dissociable protons. These can be achieved using N-methyl-2-pyrrolidone, N,N-dimethylformamide, or N,N-dimethylacetamide. Such solvents can dissolve aromatic diamines and aromatic dianhydrides and maintain the stability of the polymerization reaction system. N-methyl-2-pyrrolidone, with its high boiling point and strong polarity, can prevent premature solvent evaporation that could lead to an inhomogeneous reaction system. The strong solubility of N,N-dimethylformamide promotes thorough monomer dispersion. The thermal stability of N,N-dimethylacetamide reduces the interference of solvent decomposition at high temperatures on the polymerization reaction.
[0042] In the preparation of polyamic acid solutions, selecting one of the three solvents mentioned above can effectively dissolve aromatic diamines and aromatic dianhydride monomers, avoiding monomer aggregation or incomplete reactions due to insufficient solvent polarity. The aprotic nature of these solvents prevents proton exchange side reactions with the monomers, ensuring the polycondensation reaction proceeds along the intended path. Simultaneously, the high boiling point of the solvent maintains a liquid phase environment during the polymerization reaction, preventing sudden changes in system viscosity due to solvent evaporation, thereby ensuring the linear growth and uniform dispersion of the polyamic acid molecular chains.
[0043] Optionally, in the hexagonal boron nitride / polyimide composite solution, the mass fraction of the monolayer hexagonal boron nitride is from 0.5 wt% to 7 wt%.
[0044] In this optional embodiment, the problem of synergistic optimization of filler dispersion and interfacial bonding is solved by precisely controlling the mass fraction range. Uniform dispersion of hexagonal boron nitride in the polyimide matrix is achieved, forming a dense lamellar barrier structure that effectively delays the penetration of corrosive media to the metal substrate surface. Simultaneously, the interfacial interaction enhances the internal adhesion of the coating, thereby significantly improving the long-term stability of the composite coating in high-temperature corrosive environments.
[0045] Specifically, the hexagonal boron nitride / polyimide composite solution refers to a mixed system formed by uniformly dispersing monolayer hexagonal boron nitride nanosheets in a polyimide precursor polyamic acid solution. Dispersion can be achieved through mechanical stirring and phased feeding. This mass fraction range is used to balance the filler reinforcement effect and dispersion stability, avoiding discontinuous barrier networks due to excessively low content or agglomeration of the sheets due to excessively high content.
[0046] The mass fraction of monolayer hexagonal boron nitride is limited to 0.5 wt% to 7 wt%. Within this range, hexagonal boron nitride nanosheets can form a uniformly distributed and overlapping physical barrier structure in the polyimide matrix. When the mass fraction is below 0.5 wt%, the nanosheet spacing is too large, failing to effectively block the penetration path of corrosive media; when the mass fraction exceeds 7 wt%, the nanosheets stack due to van der Waals forces, leading to stress concentration defects within the coating. By adding the nanosheets in batches and extending the stirring time, a stable interface can be formed between the nanosheets and the polyamic acid molecular chains through π-π interactions, thereby improving the density and bonding strength of the coating.
[0047] Optionally, the solid content of the polyamic acid solution is 23%.
[0048] In this optional embodiment, by limiting the solid content to 23%, the problems of large coating thickness fluctuations and uneven distribution of curing shrinkage stress caused by a wide concentration range are solved, reducing the internal porosity of the coating to below 0.5%. This achieves a balance between the leveling properties and film strength of the polyamic acid solution during the coating stage, controlling the surface roughness of the cured coating to within 50 nm, while ensuring that the orientation degree of the hexagonal boron nitride layers in the substrate reaches over 85%. This concentration parameter effectively avoids the decrease in coating mechanical strength caused by excessively dilute solutions and the cracking defects caused by excessively concentrated solutions, allowing the coating to maintain its intact interface structure even under thermal shock at 500°C.
[0049] Specifically, solid content refers to the percentage of solid matter in the solution by mass. This can be achieved by controlling the solvent evaporation rate or adjusting the reactant ratio. Precise control of the solution concentration allows the polyamic acid molecular chains to form a moderately entangled state. Experimentally verified, a solid content range of 23% balances the conflicting relationship between solution viscosity and flowability, ensuring sufficient spreadability during coating while avoiding uneven dispersion of the dispersed phase due to excessive concentration.
[0050] During the preparation of the polyamic acid solution, the polymerization reaction conditions of the aromatic diamine and aromatic dianhydride were controlled to maintain a stable solid content of 23% in the final solution. The viscosity of the solution at this concentration was controlled within the range of 2000-3000 mPa·s, satisfying both the process requirements for mechanically dispersing hexagonal boron nitride and ensuring the formation of a uniform liquid film with a thickness deviation of less than 5% on the substrate surface during coating. During the gradient temperature curing stage, the molecular chain spacing corresponding to this concentration is conducive to orderly arrangement, forming a three-dimensional cross-linked network structure, while simultaneously providing uniformly distributed anchoring points for the hexagonal boron nitride sheets.
[0051] Optionally, during the polymerization reaction, the reaction temperature is 20 to 25°C and the reaction time is 24 to 28 hours.
[0052] In this optional embodiment, a combination of low-temperature, long-duration reaction parameters achieves precise control of molecular weight distribution while maintaining production efficiency. This effectively solves the problem of excessively wide molecular weight distribution caused by improper control of reaction conditions during the preparation of polyamic acid solutions. The low-temperature environment suppresses side reactions, and the long reaction time ensures complete monomer conversion. The resulting polyamic acid solution exhibits uniform molecular chain length and stable solution viscosity. During subsequent gradient curing, this solution forms a dense three-dimensional cross-linked network, allowing hexagonal boron nitride to be uniformly dispersed within the polyimide matrix, thereby significantly improving the coating's high-temperature resistance and resistance to permeation corrosion.
[0053] Specifically, controlling the reaction temperature between 20 and 25°C means maintaining the temperature of the polymerization reaction system within this range. This can be achieved in real-time control using a water bath circulation device combined with a temperature sensor. This temperature range effectively suppresses random chain breakage and the formation of by-products, ensuring the orderly polycondensation of monomers to form a linear polymer chain structure. Controlling the reaction time between 24 and 28 hours means setting the polymerization reaction duration within this range, which can be controlled by a timer. This duration ensures that the molar ratio of aromatic diamine to aromatic dianhydride reaches the theoretical equilibrium point, bringing the polycondensation reaction close to complete conversion and preventing unreacted monomer residues from affecting solution stability.
[0054] At a low temperature of 20-25°C, the condensation reaction rate of aromatic diamines and aromatic dianhydrides is controlled at kinetic equilibrium, with monomers gradually losing water molecules to form amide bonds. A continuous reaction time of 24-28 hours results in a monomer conversion rate exceeding 95%, while the molecular weight distribution index (PDI) remains below 1.3. These mild reaction conditions avoid high-temperature-induced branching or cyclization side reactions of the molecular chains, ensuring that the polyamic acid molecular chains possess a regular linear structure. When the reaction temperature is below 20°C, the molecular chain growth rate decreases significantly, leading to incomplete reaction; while temperatures above 25°C cause accelerated solvent evaporation, disrupting the homogeneity of the reaction system. A reaction time of less than 24 hours results in an excessively high proportion of oligomers, while a reaction time exceeding 28 hours may trigger oxidative degradation of the molecular chains.
[0055] Optionally, gradient temperature curing includes: holding at 70-90℃ for 1 to 2 hours, raising the temperature to 110-130℃ and holding for 1 to 2 hours, raising the temperature to 140-160℃ and holding for 1 to 2 hours, raising the temperature to 170-190℃ and holding for 1 to 2 hours, raising the temperature to 200-220℃ and holding for 1 to 2 hours, raising the temperature to 230-250℃ and holding for 1 to 2 hours, and raising the temperature to 270-290℃ and holding for 1 to 2 hours.
[0056] In this optional embodiment, eight precisely temperature-controlled stages allow the solvent to escape in stages and the molecular chains to be reconstructed in segments. This ensures the complete completion of the imidization reaction while avoiding structural defects caused by thermal shock. It effectively controls the distribution of thermal stress during the curing process, eliminates microcracks and bubble defects within the coating, and enables the polyimide molecular chains to form a highly ordered and dense structure. This significantly improves the coating's thermal shock resistance and resistance to corrosive media penetration under high-temperature environments.
[0057] Specifically, gradient temperature curing refers to a curing process that controls the rate of temperature change in stages. This can be achieved using a programmable temperature control chamber or a segmented heating device, by setting eight temperature steps to achieve the gradual conversion of the polyimide precursor. The holding time, limited to 1 to 2 hours, refers to the duration of each temperature step, which can be achieved using a timer linked to a temperature sensor to ensure sufficient solvent evaporation and orderly rearrangement of the molecular chains. The temperature step interval, controlled within the range of 20-40℃, refers to the temperature difference between two adjacent curing stages, which can be achieved by setting a stepped temperature rise curve using a temperature controller to avoid sudden thermal stress that could cause coating cracking.
[0058] In the 70-90℃ range, the polar solvent in the polyamic acid solution is slowly evaporated to avoid rapid volatilization and the formation of bubble defects. When the temperature rises to 110-130℃, the polyamic acid molecular chains begin to dehydrate and cyclize to form a primary polyimide structure. In the 140-160℃ range, the orientation of the molecular chains is strengthened, and a preliminary ordered structure is formed inside the coating. After heating to 170-190℃, the polyamic acid completes the main imidization reaction, generating a stable polyimide backbone. In the 200-220℃ range, residual stress generated in the early curing stage is eliminated through thermal relaxation. The high temperature of 230-250℃ promotes further regularization of the molecular chains, and at 270-290℃, complete cross-linking is finally achieved, forming a dense three-dimensional network structure.
[0059] Optionally, the micron-sized hexagonal boron nitride is subjected to ultrasonic-assisted liquid-phase exfoliation, including: ultrasonic-assisted liquid-phase exfoliation of the micron-sized hexagonal boron nitride in a solution of isopropanol and water in a volume ratio of 1:1 for more than 1 hour, followed by vacuum filtration to obtain a monolayer of hexagonal boron nitride, washing the monolayer of hexagonal boron nitride with deionized water, and vacuum drying at 50 to 70°C for 9 to 11 hours.
[0060] In this optional embodiment, by optimizing the synergistic effect of the solvent system and process parameters, the technical bottlenecks such as low nanosheet collection efficiency and numerous impurity residues are solved while ensuring the integrity of the monolayer structure. This achieves efficient exfoliation and purification of micron-sized hexagonal boron nitride, effectively suppressing the aggregation of monolayer materials, eliminating the negative impact of residual organic solvents on the interfacial adhesion of the coating, and providing a uniformly dispersed functional filler for preparing highly dense composite anti-corrosion coatings.
[0061] Specifically, the isopropanol to water 1:1 volume ratio solution refers to the exfoliation medium formed by mixing isopropanol and deionized water in a 1:1 volume ratio. This can be achieved using a graduated cylinder or pipette for precise volume proportioning. The polarity gradient of this mixed solvent promotes the interlayer separation of hexagonal boron nitride. Ultrasonic-assisted liquid-phase exfoliation for more than one hour refers to applying mechanical vibrations at a frequency of 20-40 kHz to the mixed solution using an ultrasonic generator. This can be achieved using a probe-type ultrasonic instrument at a power of 200-400W for continuous processing. This operation time ensures that the micron-sized hexagonal boron nitride is fully exfoliated into a single-layer structure. Reduced-pressure filtration refers to a filtration device using a Buchner funnel connected to a vacuum pump. Solid-liquid separation can be achieved through a 0.22 μm pore size polytetrafluoroethylene (PTFE) filter membrane. This method effectively collects nano-sized single-layer hexagonal boron nitride. Vacuum drying for 9 to 11 hours refers to maintaining a temperature of 50-70°C in a sealed drying oven and evacuating to below 10Pa. This can be achieved by using a system that combines a circulating water vacuum pump with a constant temperature drying oven. This condition can prevent the single-layer material from undergoing structural reorganization due to high temperature.
[0062] The isopropanol-water mixture creates an intercalation effect through polarity differences, which, under ultrasonic cavitation, disrupts the van der Waals forces between hexagonal boron nitride layers, achieving monolayer exfoliation. Sustained ultrasonic treatment for over one hour overcomes the interlayer bonding energy of micron-sized raw materials, ensuring thorough exfoliation. Reduced-pressure filtration accelerates liquid discharge through negative pressure, retaining the monolayer product while removing unexfoliated particles. Washing with deionized water dissolves residual organic solvent molecules, eliminating the risk of contamination to subsequent composite materials. The vacuum drying stage employs gradient temperature control to maintain the stability of the monolayer structure while removing moisture, preventing secondary agglomeration during drying.
[0063] Optionally, the monolayer hexagonal boron nitride is added to the polyamic acid solution in multiple portions and stirred until homogeneous, including: adding the monolayer hexagonal boron nitride to the polyamic acid solution in four to six portions and mechanically stirring for more than 12 hours.
[0064] In this optional embodiment, the batch addition strategy effectively suppresses van der Waals force-induced agglomeration by gradually reducing the concentration gradient of the system. Conventional stirring time is typically controlled within 6 hours, which cannot completely destroy the weak interactions between nanosheet layers. Continuous stirring for more than 12 hours significantly improves dispersion uniformity by extending the shearing time. This achieves stable dispersion of monolayer hexagonal boron nitride in polyamic acid solution, avoiding stratification of the composite liquid caused by agglomeration. The cured coating forms a continuous and uniform hexagonal boron nitride network structure, thereby improving the coating's impermeability and mechanical property consistency in high-temperature corrosive environments.
[0065] Specifically, adding the boron monolayer in four to six batches refers to dividing the total amount into multiple batches and mixing them into the polyamic acid solution one at a time. This can be achieved by adding the boron monolayer in five batches at 30-minute intervals. This operation avoids agglomeration caused by excessively high local concentrations by controlling the amount added at each batch. Mechanical stirring for more than 12 hours refers to applying continuous shear force to the mixture system with a stirring paddle at a constant speed, specifically at a stirring speed of 500 rpm. This operation breaks down any remaining weak agglomerates through prolonged mechanical action.
[0066] During the batch addition process of monolayer hexagonal boron nitride, each batch was fully contacted with the polyamic acid solution. The polyamic acid molecular chains encapsulated the surface of the nanosheets through hydrogen bonding, forming a stable interfacial bond. When added in five batches, each batch accounted for 20% of the total amount. During the intervals between additions, mechanical stirring was used to ensure the added nanosheets were uniformly dispersed in the solution. Continuous mechanical stirring for 12 hours created a stable shear flow field within the solution. Any incompletely dispersed nanosheets further deagglomerated under the shear force of the fluid, ultimately forming a composite liquid system with a uniform distribution of hexagonal boron nitride.
[0067] The present invention will be further described below with reference to specific embodiments.
[0068] Example 1: Preparation of h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0069] 1. Add 30 ml of N,N-dimethylacetamide as a solvent to a 100 ml three-necked flask equipped with a mechanical stirrer and nitrogen inlet / outlet, and purge with nitrogen. Add the diamine 2-(4-aminophenyl)-5-aminobenzoxazole to the three-necked flask and stir at room temperature until completely dissolved to obtain a diamine solution.
[0070] 2. Weigh the dried dianhydride monomer bisphenol A diether dianhydride and add it to the diamine solution in four portions. The molar ratio of the added dianhydride to the diamine is 1:1. The polymerization reaction is carried out under stirring for 12 hours to obtain a polyamic acid (PAA) solution.
[0071] 3. Hexagonal boron nitride was subjected to ultrasonic-assisted liquid phase stripping in a solution of isopropanol and water at a volume ratio of 1:1 for 1 hour, filtered under reduced pressure, washed with deionized water, and vacuum dried at 60°C for 10 hours.
[0072] 4. The stripped hexagonal boron nitride was added to the PAA solution in four portions and stirred for 12 hours in still water. The mass fraction of the hexagonal boron nitride was set to 0.5% for each portion.
[0073] 5. The partially reacted solution is uniformly coated onto a glass plate using a casting method to form an h-BN / PI composite film for subsequent testing.
[0074] VI. A specific amount of the composite solution was applied to the polished aluminum alloy surface using a wire bar coater. The surface was then placed in an oven for gradient curing. The temperature progression was as follows: 80℃, 2 h; 120℃, 2 h; 150℃, 2 h; 180℃, 2 h; 210℃, 2 h; 240℃, 2 h; 280℃, 2 h.
[0075] Example 2: Preparation of h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0076] 1. Add 30 ml of N,N-dimethylacetamide as a solvent to a 100 ml three-necked flask equipped with a mechanical stirrer and nitrogen inlet / outlet, and purge with nitrogen. Add the diamine 2-(4-aminophenyl)-5-aminobenzoxazole to the three-necked flask and stir at room temperature until completely dissolved to obtain a diamine solution.
[0077] 2. Weigh the dried dianhydride monomer bisphenol A diether dianhydride and add it to the diamine solution in four portions. The molar ratio of the added dianhydride to the diamine is 1:1. The polymerization reaction is carried out under stirring for 12 hours to obtain a polyamic acid solution.
[0078] 3. Hexagonal boron nitride was subjected to ultrasonic-assisted liquid phase stripping in a solution of isopropanol and water at a volume ratio of 1:1 for 1 hour, filtered under reduced pressure, washed with deionized water, and vacuum dried at 60°C for 10 hours.
[0079] 4. The stripped hexagonal boron nitride was added to the PAA solution in four portions and stirred for 12 hours in still water. The mass fraction of hexagonal boron nitride was set to 1% for each portion.
[0080] 5. The partially reacted solution is uniformly coated onto a glass plate using a casting method to form an h-BN / PI composite film for subsequent testing. VI. A specific amount of the composite solution was applied to the polished aluminum alloy surface using a wire bar coater. The surface was then placed in an oven for gradient curing. The temperature progression was as follows: 80℃, 2 h; 120℃, 2 h; 150℃, 2 h; 180℃, 2 h; 210℃, 2 h; 240℃, 2 h; 280℃, 2 h.
[0081] Example 3: Preparation of h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0082] 1. Add 30 ml of N,N-dimethylacetamide as a solvent to a 100 ml three-necked flask equipped with a mechanical stirrer and nitrogen inlet / outlet, and purge with nitrogen. Add the diamine 2-(4-aminophenyl)-5-aminobenzoxazole to the three-necked flask and stir at room temperature until completely dissolved to obtain a diamine solution.
[0083] 2. Weigh the dried dianhydride monomer bisphenol A diether dianhydride and add it to the diamine solution in four portions. The molar ratio of the added dianhydride to the diamine is 1:1. The polymerization reaction is carried out under stirring for 12 hours to obtain a polyamic acid solution.
[0084] 3. Hexagonal boron nitride was subjected to ultrasonic-assisted liquid phase stripping in a solution of isopropanol and water at a volume ratio of 1:1 for 1 hour, filtered under reduced pressure, washed with deionized water, and vacuum dried at 60°C for 10 hours.
[0085] 4. The stripped hexagonal boron nitride was added to the PAA solution in four portions and stirred for 12 hours in still water. The mass fraction of hexagonal boron nitride was set to 2% for each portion.
[0086] 5. The partially reacted solution is uniformly coated onto a glass plate using a casting method to form an h-BN / PI composite film for subsequent testing. VI. A specific amount of the composite solution was applied to the polished aluminum alloy surface using a wire bar coater. The surface was then placed in an oven for gradient curing. The temperature progression was as follows: 80℃, 2 h; 120℃, 2 h; 150℃, 2 h; 180℃, 2 h; 210℃, 2 h; 240℃, 2 h; 280℃, 2 h.
[0087] The surface SEM microstructure of the h-BN / PI composite coating prepared in Example 3 is shown in Figure 3. Figure 2 As shown. The infrared spectrum of the h-BN / PI composite coating prepared in Example 3 is as follows. Figure 3 As shown. Figure 3 The characteristic absorption peaks are visible, indicating that the h-BN / PI composite film prepared in Example 3 has been completely imidized. The DSC spectrum of the h-BN / PI composite film prepared in Example 3 is shown below. Figure 4 As shown, the glass transition temperature of the h-BN / PI composite coating prepared in Example 3 is 251.6℃. The nanoindentation test curve of the h-BN / PI composite coating prepared in Example 3 is shown below. Figure 5 As shown, the test results indicate that the elastic modulus of the h-BN / PI composite coating prepared in Example 3 is 5.273 GPa, and the hardness of the composite coating is 0.286 GPa. Figure 6 The image shown is a corrosion diagram from a neutral salt spray test of the h-BN / PI composite coating prepared in this embodiment. Figure 6 Figure 1 shows a schematic diagram of the aluminum alloy surface after being coated with an h-BN / PI composite film. Figure 6 Figure 2 shows a schematic diagram of the metal surface of the h-BN / PI composite film after a 20-day neutral salt spray test. Figure 6 Figure 3 shows a schematic diagram of the metal surface of the h-BN / PI composite film after a 40-day neutral salt spray test. Figure 6 As can be seen from the results, after 20 and 40 days of neutral salt spray testing, no corrosion was observed in the metal of the h-BN / PI composite coating prepared in Example 3, and the appearance of the coating did not change significantly, indicating that the composite coating has good corrosion resistance.
[0088] Example 4: Preparation of h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0089] 1. Add 30 ml of N,N-dimethylacetamide as a solvent to a 100 ml three-necked flask equipped with a mechanical stirrer and nitrogen inlet / outlet, and purge with nitrogen. Add the diamine 2-(4-aminophenyl)-5-aminobenzoxazole to the three-necked flask and stir at room temperature until completely dissolved to obtain a diamine solution.
[0090] 2. Weigh the dried dianhydride monomer bisphenol A diether dianhydride and add it to the diamine solution in four portions. The molar ratio of the added dianhydride to the diamine is 1:1. The polymerization reaction is carried out under stirring for 12 hours to obtain a polyamic acid solution.
[0091] 3. Hexagonal boron nitride was subjected to ultrasonic-assisted liquid phase stripping in a solution of isopropanol and water at a volume ratio of 1:1 for 1 hour, filtered under reduced pressure, washed with deionized water, and vacuum dried at 60°C for 10 hours.
[0092] 4. The stripped hexagonal boron nitride was added to the PAA solution in four portions and stirred for 12 hours in still water. The mass fraction of hexagonal boron nitride was set to 3%.
[0093] 5. The partially reacted solution is uniformly coated onto a glass plate using a casting method to form an h-BN / PI composite film for subsequent testing. VI. A specific amount of the composite solution was applied to the polished aluminum alloy surface using a wire bar coater. The surface was then placed in an oven for gradient curing. The temperature progression was as follows: 80℃, 2 h; 120℃, 2 h; 150℃, 2 h; 180℃, 2 h; 210℃, 2 h; 240℃, 2 h; 280℃, 2 h.
[0094] Example 5: Preparation of h-BN / PI high-temperature resistant and corrosion-resistant coating.
[0095] 1. Add 30 ml of N,N-dimethylacetamide as a solvent to a 100 ml three-necked flask equipped with a mechanical stirrer and nitrogen inlet / outlet, and purge with nitrogen. Add the diamine 2-(4-aminophenyl)-5-aminobenzoxazole to the three-necked flask and stir at room temperature until completely dissolved to obtain a diamine solution.
[0096] 2. Weigh the dried dianhydride monomer bisphenol A diether dianhydride and add it to the diamine solution in four portions. The molar ratio of the added dianhydride to the diamine is 1:1. The polymerization reaction is carried out under stirring for 12 hours to obtain a polyamic acid solution.
[0097] 3. Hexagonal boron nitride was subjected to ultrasonic-assisted liquid phase stripping in a solution of isopropanol and water at a volume ratio of 1:1 for 1 hour, filtered under reduced pressure, washed with deionized water, and vacuum dried at 60°C for 10 hours.
[0098] 4. The stripped hexagonal boron nitride was added to the PAA solution in four portions and stirred for 12 hours in still water. The mass fraction of the hexagonal boron nitride was set to 5%.
[0099] 5. The partially reacted solution is uniformly coated onto a glass plate using a casting method to prepare a PI / h-BN composite film for subsequent testing. VI. A specific amount of the composite solution was applied to the polished aluminum alloy surface using a wire bar coater. The surface was then placed in an oven for gradient curing. The temperature progression was as follows: 80℃, 2 h; 120℃, 2 h; 150℃, 2 h; 180℃, 2 h; 210℃, 2 h; 240℃, 2 h; 280℃, 2 h.
[0100] Comparative Example 1: Preparation of pure PI coating.
[0101] 1. Add 30 ml of N,N-dimethylacetamide as a solvent to a 100 ml three-necked flask equipped with a mechanical stirrer and nitrogen inlet / outlet, and purge with nitrogen. Add the diamine 2-(4-aminophenyl)-5-aminobenzoxazole to the three-necked flask and stir at room temperature until completely dissolved to obtain a diamine solution.
[0102] 2. Weigh the dried dianhydride monomer bisphenol A diether dianhydride and add it to the diamine solution in four portions. The molar ratio of the added dianhydride to the diamine is 1:1. The polymerization reaction is carried out under stirring for 12 hours to obtain a polyamic acid solution.
[0103] 3. The partially reacted solution is uniformly coated onto a glass plate using a casting method to form a PI film for subsequent testing. 4. A specific amount of solution was applied to the polished aluminum alloy surface using a wire bar coater. The surface was then placed in an oven for gradient curing. The temperature program was as follows: 80℃, 2 h; 120℃, 2 h; 150℃, 2 h; 180℃, 2 h; 210℃, 2 h; 240℃, 2 h; 280℃, 2 h.
[0104] Figure 7 The DSC spectrum of the polyimide prepared in Comparative Example 1 is shown, indicating that the glass transition temperature of the PI film prepared in Comparative Example 1 is 250.0℃, which is 1.6℃ lower than that of the h-BN / PI composite film prepared in Example 3. Figure 8 The figure shown is a nanoindentation test curve of the PI coating prepared in Comparative Example 1. Figure 8 As can be seen from the data, the elastic modulus of the PI coating prepared in the comparative example is 5.232 GPa, and the hardness of the composite coating is 0.284 GPa, both of which are lower than those in Example 3. Figure 9 The image shown is a corrosion diagram of the PI coating prepared in Comparative Example 1 under a neutral salt spray test. Figure 9 Figure 1 shows a schematic diagram of the aluminum alloy surface after a PI film has been applied. Figure 9 Figure 2 shows a schematic diagram of the metal surface after a 20-day neutral salt spray test of the PI coating. Figure 9 As can be seen from Figure 2, the PI coating underwent significant corrosion after 20 days of neutral salt spray testing, while the h-BN / PI composite coating in Example 3 showed no significant changes after 40 days of neutral salt spray testing.
[0105] It can be seen that the h-BN / PI high-temperature resistant and anti-corrosion coating obtained by the present invention has better high-temperature resistance, better kinetic properties and excellent corrosion resistance.
[0106] While the present invention has been disclosed above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and all such changes and modifications will fall within the scope of protection of the present invention.
Claims
1. A method for preparing an h-BN / PI high-temperature resistant and corrosion-resistant coating, characterized in that, Includes the following steps: Under an inert atmosphere, an aromatic diamine containing a five-membered ring of heterogeneous elements and an aromatic dianhydride containing an ether bond are polymerized in a polar aprotic solvent to obtain a polyamic acid solution. Micron-sized hexagonal boron nitride was subjected to ultrasonic-assisted liquid-phase exfoliation to obtain a single layer of hexagonal boron nitride. The single-layer hexagonal boron nitride was added to the polyamic acid solution in multiple portions and stirred until homogeneous to obtain a hexagonal boron nitride / polyimide composite solution. The hexagonal boron nitride / polyimide composite liquid is applied to the surface to be coated and cured by gradient temperature increase to obtain h-BN / PI high temperature resistant and anti-corrosion coating.
2. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The aromatic diamine is 2-(4-aminophenyl)-5-aminobenzoxazole, and the aromatic dianhydride is bisphenol A type diether dianhydride.
3. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The molar ratio of the aromatic diamine to the aromatic dianhydride is 1:2 to 2:
1.
4. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The polar aprotic solvent includes one of N-methyl-2-pyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
5. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, In the hexagonal boron nitride / polyimide composite solution, the mass fraction of the monolayer hexagonal boron nitride is from 0.5 wt% to 7 wt%.
6. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The solid content of the polyamic acid solution is 23%.
7. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, During the polymerization reaction, the reaction temperature is 20 to 25°C and the reaction time is 24 to 28 hours.
8. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The gradient temperature curing process includes: holding at 70-90℃ for 1 to 2 hours, raising the temperature to 110-130℃ and holding for 1 to 2 hours, raising the temperature to 140-160℃ and holding for 1 to 2 hours, raising the temperature to 170-190℃ and holding for 1 to 2 hours, raising the temperature to 200-220℃ and holding for 1 to 2 hours, raising the temperature to 230-250℃ and holding for 1 to 2 hours, and raising the temperature to 270-290℃ and holding for 1 to 2 hours.
9. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The process of ultrasonic-assisted liquid-phase exfoliation of micron-sized hexagonal boron nitride includes: ultrasonically assisted liquid-phase exfoliation of the micron-sized hexagonal boron nitride in a solution of isopropanol and water in a volume ratio of 1:1 for more than 1 hour, followed by vacuum filtration to obtain the monolayer hexagonal boron nitride, washing the monolayer hexagonal boron nitride with deionized water, and vacuum drying at 50 to 70°C for 9 to 11 hours.
10. The method for preparing the h-BN / PI high-temperature resistant and corrosion-resistant coating according to claim 1, characterized in that, The monolayer hexagonal boron nitride is added to the polyamic acid solution in multiple portions and stirred until homogeneous, including: adding the monolayer hexagonal boron nitride to the polyamic acid solution in four to six portions and mechanically stirring for more than 12 hours.
Citation Information
Cited By
Self-repairing hydrogen barrier composite coating for hydrogen storage or transportation device as well as preparation method and application of self-repairing hydrogen barrier composite coating
CN121293874A
High-temperature-resistant and corrosion-resistant coating for aluminum alloy heat exchange tube and preparation method thereof
CN121343472A
High temperature corrosion resistant coating for aluminum alloy heat exchange tubes and method of making
CN121343472B
Shell, preparation method of shell and battery
CN121709779A