A composite heat treatment method for improving the strength and toughness of high-strength structural steel

CN121183077BActive Publication Date: 2026-09-11CHONGQING UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202511326005.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-09-17
Publication Date
2026-09-11
Estimated Expiration
2045-09-17

AI Technical Summary

Technical Problem

[0005]本发明的目的在于提供一种提高高强度结构钢强度和韧性的复合热处理方法,解决现有船用高强度结构钢热处理方法对强度和低温韧性的改善不明显的问题

Benefits of technology

[0021] This invention first normalizes the steel to reduce grain size, then performs critical quenching in the two-phase region. By controlling the quenching temperature, a small amount of ferrite exists in the steel, which forms a two-phase structure with martensite. Martensite provides high hardness, while ferrite, as a toughening phase, improves toughness and reduces quenching internal stress. Subsequent cryogenic treatment transforms the retained austenite after critical quenching in the two-phase region into martensite, reducing the retained austenite content. Furthermore, cryogenic treatment causes martensite lattice shrinkage, precipitating ultrafine carbides that are uniformly distributed on the martensite matrix, eliminating internal defects and improving strength. In addition, cryogenic treatment partially fragments the martensite lath bundles, reducing lath size and improving both strength and low-temperature toughness. A composite process of low-temperature tempering and high-temperature tempering is employed. Low-temperature tempering eliminates the stress introduced by cryogenic treatment, while high-temperature tempering decomposes martensite into tempered sorbite, balancing strength and toughness and achieving a good match between the two. The composite heat treatment method of this invention achieves simultaneous improvement in the strength and low-temperature impact toughness of steel plates. The yield strength can reach 926.4 MPa, the tensile strength can reach 1135.8 MPa, the elongation at break is 17.2%, and the impact energy at -60℃ can reach 127.1 J. It can meet the performance requirements of high-strength structural steel for ships in special environments such as deep sea areas, and solves the problem of mismatch between strength and toughness of ship structural steel in traditional heat treatment methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005599731780000061
    Figure BDA0005599731780000061
Patent Text Reader

Abstract

The application belongs to the technical field of steel heat treatment, and discloses a composite heat treatment method for improving the strength and toughness of high-strength structural steel. The high-strength structural steel is subjected to annealing treatment, then is subjected to normalizing treatment by heating, and then is subjected to critical quenching in a two-phase region and is water-cooled to room temperature; then is subjected to cryogenic treatment, and then is subjected to first tempering treatment and is water-cooled to room temperature; and then is subjected to second tempering treatment and is air-cooled to room temperature. Through the composite heat treatment method, the strength and low-temperature impact toughness of the steel plate are simultaneously improved, the yield strength can reach 926.4 MPa, the tensile strength can reach 1135.8 MPa, the elongation at break is 17.2%, and the impact energy at-60 DEG C can reach 127.1 J, so that the performance requirements of the high-strength structural steel for special environment ships can be met, and the problem of mismatching between the strength and toughness of the structural steel for ships in the traditional heat treatment method is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of steel heat treatment technology, and in particular to a composite heat treatment method for improving the strength and toughness of high-strength structural steel. Background Technology

[0002] Marine high-strength structural steel, used to manufacture the main structure of ships such as hull side plates and bottom plates, needs to withstand wave impact and alternating loads. It also serves as a key load-bearing component and needs to resist local stress concentration. At the same time, with the continuous development of deep-sea exploration, higher requirements have been put forward for the performance of marine structural steel. Current research on marine high-strength structural steel mainly focuses on the following directions: (1) High-strength development: With the demand for larger and lighter ships, the development of ultra-high-strength steel of 1000MPa grade and above to improve the load-bearing capacity of ships and achieve lightweighting has become a research focus. (2) Low-temperature toughness improvement: With the development of ships used in low-temperature environments, steel that maintains good toughness at -40℃ or even lower temperatures has become a research hotspot.

[0003] Currently, to adapt to the high-strength development and low-temperature toughness improvement of marine structural steel, traditional methods often employ optimization of the steel's chemical composition and factory heat treatment (quenching + tempering). However, for high-strength and high-toughness marine structural steel with a certain thickness, composition optimization and factory heat treatment alone are insufficient to simultaneously improve strength and toughness. Therefore, composite heat treatment of steel can further enhance strength and toughness to a certain extent. For example, patent CN111500926A discloses a marine steel material and its manufacturing method. By controlling the Cr content in the marine steel material to 0.15–0.24 wt%, the mechanical properties of the steel material can be improved. After forging, annealing, normalizing, and tempering processes are employed. Annealing and normalizing can achieve uniform chemical composition and microstructure, refine grains, adjust hardness, eliminate internal stress, and reduce work hardening. Normalizing, in particular, can eliminate overheating defects such as coarse grains and banded structures, achieving grain refinement, uniform microstructure, and providing good microstructure preparation for subsequent hot working. Tempering can improve the toughness and plasticity of the steel. However, the yield strength of the marine steel obtained by this method is only 450 MPa at most, and the impact energy is only about 20 J. It is tempered immediately after normalizing and has not undergone quenching treatment. The tempering has a limited effect on improving strength and toughness and cannot meet the requirements of higher impact toughness in high-latitude sea areas below -20℃.

[0004] Therefore, in response to the application requirements of high-strength structural steel for ships under harsh service conditions for ultra-high strength and high and low temperature toughness, how to provide an advanced composite heat treatment method to improve the strength and low temperature toughness of high-strength structural steel is an urgent problem to be solved. Summary of the Invention

[0005] The purpose of this invention is to provide a composite heat treatment method to improve the strength and toughness of high-strength structural steel, thereby solving the problem that existing heat treatment methods for marine high-strength structural steel do not significantly improve strength and low-temperature toughness.

[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0007] This invention provides a composite heat treatment method for improving the strength and toughness of steel, comprising the following steps:

[0008] High-strength structural steel is annealed and then oil-cooled to room temperature to obtain pretreated steel.

[0009] The pretreated steel is heated to normalize, then subjected to critical quenching in the two-phase region, and then water-cooled to room temperature to obtain quenched steel.

[0010] Quenched steel is subjected to cryogenic treatment and then warmed back to room temperature to obtain cryogenic steel.

[0011] The cryogenic steel undergoes a first tempering treatment, followed by water cooling to room temperature; then a second tempering treatment is performed, followed by air cooling to room temperature, thus completing the composite heat treatment for improving the strength and toughness of high-strength structural steel.

[0012] The high-strength structural steel mentioned above is marine high-strength structural steel.

[0013] Preferably, the annealing temperature is 600–700°C, and the annealing time is 0.5–2 hours.

[0014] Preferably, the normalizing temperature is 900–920°C, and the normalizing time is 0.5–1 hour.

[0015] Preferably, the critical quenching temperature of the two-phase region is 750–850°C, and the critical quenching time of the two-phase region is 0.5–1 h.

[0016] Preferably, the rate of water cooling to room temperature after critical quenching in the two-phase region is 50–150 °C / s.

[0017] Preferably, the cryogenic treatment method is liquid nitrogen cooling; the cryogenic treatment temperature is -196°C; and the cryogenic treatment time is 1 to 4 hours.

[0018] Preferably, the temperature of the first tempering treatment is 300–350°C, and the time of the first tempering treatment is 0.5–2 hours.

[0019] Preferably, the temperature of the second tempering treatment is 550–580°C, and the time of the second tempering treatment is 0.5–2 hours.

[0020] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects:

[0021] This invention first normalizes the steel to reduce grain size, then performs critical quenching in the two-phase region. By controlling the quenching temperature, a small amount of ferrite exists in the steel, which forms a two-phase structure with martensite. Martensite provides high hardness, while ferrite, as a toughening phase, improves toughness and reduces quenching internal stress. Subsequent cryogenic treatment transforms the retained austenite after critical quenching in the two-phase region into martensite, reducing the retained austenite content. Furthermore, cryogenic treatment causes martensite lattice shrinkage, precipitating ultrafine carbides that are uniformly distributed on the martensite matrix, eliminating internal defects and improving strength. In addition, cryogenic treatment partially fragments the martensite lath bundles, reducing lath size and improving both strength and low-temperature toughness. A composite process of low-temperature tempering and high-temperature tempering is employed. Low-temperature tempering eliminates the stress introduced by cryogenic treatment, while high-temperature tempering decomposes martensite into tempered sorbite, balancing strength and toughness and achieving a good match between the two. The composite heat treatment method of this invention achieves simultaneous improvement in the strength and low-temperature impact toughness of steel plates. The yield strength can reach 926.4 MPa, the tensile strength can reach 1135.8 MPa, the elongation at break is 17.2%, and the impact energy at -60℃ can reach 127.1 J. It can meet the performance requirements of high-strength structural steel for ships in special environments such as deep sea areas, and solves the problem of mismatch between strength and toughness of ship structural steel in traditional heat treatment methods. Detailed Implementation

[0022] This invention provides a composite heat treatment method for improving the strength and toughness of high-strength structural steel, comprising the following steps:

[0023] High-strength structural steel is annealed and then oil-cooled to room temperature to obtain pretreated steel.

[0024] The pretreated steel is heated to normalize, then subjected to critical quenching in the two-phase region, and then water-cooled to room temperature to obtain quenched steel.

[0025] Quenched steel is subjected to cryogenic treatment and then warmed back to room temperature to obtain cryogenic steel.

[0026] The cryogenic steel undergoes a first tempering treatment, followed by water cooling to room temperature; then a second tempering treatment is performed, followed by air cooling to room temperature, thus completing the composite heat treatment for improving the strength and toughness of high-strength structural steel.

[0027] In this invention, the high-strength structural steel is preferably marine high-strength structural steel. In this embodiment of the invention, the marine high-strength structural steel is preferably HG785D structural steel.

[0028] In this invention, the annealing temperature is preferably 600-700℃, more preferably 620-680℃, and even more preferably 650℃; the annealing time is preferably 0.5-2h, more preferably 0.5-1.5h, and even more preferably 1h; the heating rate of the annealing is preferably 5-10℃ / min, more preferably 8-10℃ / min, and even more preferably 10℃ / min.

[0029] In this invention, the rate of oil cooling to room temperature after annealing is preferably 10-20°C / s, more preferably 10-15°C / s, and even more preferably 10°C / s.

[0030] In this invention, the normalizing temperature is preferably 900-920°C, more preferably 905-915°C, and even more preferably 910°C; the normalizing time is preferably 0.5-1h, more preferably 0.5h; and the normalizing heating rate is preferably 1-10°C / min, more preferably 3-7°C / min, and even more preferably 5°C / min.

[0031] In this invention, the critical quenching temperature of the two-phase region is preferably 750-850℃, more preferably 780-820℃, and even more preferably 800℃; the critical quenching time of the two-phase region is preferably 0.5-1h, and even more preferably 1h.

[0032] In this invention, the rate of water cooling to room temperature after critical quenching in the two-phase region is preferably 50-150℃ / s, more preferably 50-100℃ / s, and even more preferably 50℃ / s.

[0033] In this invention, the cryogenic treatment method is preferably liquid nitrogen cooling; the cryogenic treatment temperature is preferably -196°C; and the cryogenic treatment time is preferably 1 to 4 hours, more preferably 2 to 4 hours, and even more preferably 3 hours.

[0034] In this invention, the temperature of the first tempering treatment is preferably 300-350°C, more preferably 310-330°C, and even more preferably 320°C; the time of the first tempering treatment is preferably 0.5-2h, more preferably 1-2h, and even more preferably 1.5h; the heating rate of the first tempering treatment is preferably 1-5°C / min, more preferably 2-5°C / min, and even more preferably 5°C / min.

[0035] In this invention, the rate of water cooling to room temperature after the first tempering treatment is preferably 20-50°C / s, more preferably 25-40°C / s, and even more preferably 30°C / s.

[0036] In this invention, the temperature of the second tempering treatment is preferably 550-580°C, more preferably 560-580°C, and even more preferably 580°C; the time of the second tempering treatment is preferably 0.5-2h, more preferably 0.5-1.5h, and even more preferably 1h; the heating rate of the second tempering treatment is preferably 5-10°C / min, more preferably 7-10°C / min, and even more preferably 10°C / min.

[0037] In this invention, the room temperature is preferably 25°C.

[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0039] Example 1

[0040] This embodiment provides a composite heat treatment method for improving the strength and toughness of high-strength structural steel, including the following steps:

[0041] (1) Heat the steel (HG785D structural steel, 10mm thickness) to 650℃ at a rate of 10℃ / min for annealing for 1h, and then cool it to room temperature in oil at a rate of 10℃ / s to obtain the pretreated steel.

[0042] (2) The pretreated steel is heated to 910℃ at a rate of 5℃ / min for normalizing treatment for 0.5h, then air-cooled to room temperature, and then heated to 800℃ at a rate of 5℃ / min for critical quenching in the two-phase region, held for 1h, and then water-cooled to room temperature at a rate of 50℃ / s to obtain quenched steel.

[0043] (3) Quenched steel is subjected to cryogenic treatment at -196℃ for 3 hours using liquid nitrogen as the cooling medium, and then naturally cooled to room temperature to obtain cryogenic steel.

[0044] (4) The cryogenic steel is heated to 320°C at a rate of 5°C / min for the first tempering treatment, held for 1.5h, and then water-cooled to room temperature at a rate of 30°C / s; then heated to 580°C at a rate of 10°C / min for the second tempering treatment, held for 1h, and then air-cooled to room temperature with the furnace.

[0045] Example 2

[0046] This embodiment provides a composite heat treatment method to improve the strength and toughness of high-strength structural steel. See Embodiment 1 for details. The difference is that the quenching temperature in step (2) is 770℃ and the quenching holding time is 0.5h, while the cryogenic treatment time in step (3) is 1h.

[0047] Example 3

[0048] This embodiment provides a composite heat treatment method to improve the strength and toughness of high-strength structural steel. For details, please refer to Embodiment 1. The difference is that in step (4), the first tempering treatment temperature is 300℃ and the holding time is 0.5h, and the second tempering treatment temperature is 570℃ and the holding time is 2h.

[0049] Comparative Example 1

[0050] This comparative example provides a composite heat treatment method, specifically as described in Example 1, except that the quenching temperature in step (2) is 950℃.

[0051] Comparative Example 2

[0052] This comparative example provides a composite heat treatment method, specifically as described in Example 1, except that the deep cryogenic treatment in step (3) is not performed.

[0053] Comparative Example 3

[0054] This comparative example provides a composite heat treatment method, specifically as described in Example 1, except that the first tempering treatment in step (4) is not performed.

[0055] The high-strength structural steels of Examples 1-3 and Comparative Examples 1-3 that underwent composite heat treatment were subjected to mechanical property tests and impact toughness tests. The results are shown in Table 1.

[0056] Table 1 Results of mechanical property tests and impact toughness tests

[0057]

[0058] As shown in Table 1, the heat treatment method of the present invention effectively improves the strength and low-temperature impact toughness of high-strength structural steel, while the performance of steel plates cannot be significantly improved without cryogenic treatment or first tempering treatment.

[0059] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A composite heat treatment method for improving the strength and toughness of high-strength structural steel, characterized in that, Includes the following steps: High-strength structural steel is annealed and then oil-cooled to room temperature to obtain pretreated steel. The pretreated steel is heated to normalize, then subjected to critical quenching in the two-phase region, and then water-cooled to room temperature to obtain quenched steel. The normalizing temperature is 900~920℃ and the normalizing time is 0.5~1h. The critical quenching temperature in the two-phase region is 750~850℃ and the critical quenching time in the two-phase region is 0.5~1h. Quenched steel is subjected to cryogenic treatment and then warmed back to room temperature to obtain cryogenic steel. The cryogenic steel undergoes a first tempering treatment, followed by water cooling to room temperature; then a second tempering treatment is performed, followed by air cooling to room temperature, thus completing the composite heat treatment for improving the strength and toughness of high-strength structural steel. The temperature of the first tempering treatment is 300~350℃, and the duration of the first tempering treatment is 0.5~2 hours. The temperature of the second tempering treatment is 550~580℃, and the duration of the second tempering treatment is 0.5~2 hours. The high-strength structural steel mentioned above is marine high-strength structural steel.

2. The composite heat treatment method for improving the strength and toughness of high-strength structural steel according to claim 1, characterized in that, The annealing temperature is 600~700℃; the annealing time is 0.5~2h.

3. The composite heat treatment method for improving the strength and toughness of high-strength structural steel according to claim 1, characterized in that, The rate at which the two-phase region is water-cooled to room temperature after critical quenching is 50~150℃ / s.

4. The composite heat treatment method for improving the strength and toughness of high-strength structural steel according to claim 3, characterized in that, The cryogenic treatment method is liquid nitrogen cooling; the cryogenic treatment temperature is -196℃; and the cryogenic treatment time is 1~4 hours.

Citation Information

Patent Citations

  • Heat treatment process of AISI410 steel for compressor

    CN117107019A

  • Heat treatment method of structural steel for ship body and structural steel for ship body

    CN118147410A

  • Ultra-pure large-thickness 800MPa-grade high-toughness corrosion-resistant forged steel and production method thereof

    CN118773516A