A method for preparing a surface-active coating

By preparing a two-layer surface-active coating on the surface of artificial joints, combining an inner TiO₂ nanotube array with an outer zinc/strontium co-doped mesoporous bioactive glass, the problems of loosening and insufficient antibacterial ability of artificial joint coatings are solved, achieving efficient osseointegration and long-lasting antibacterial effects.

CN121243487BActive Publication Date: 2026-11-20MAITU MEDICAL TECHNOLOGY (SHANDONG) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511778285.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-11-28
Publication Date
2026-11-20
Estimated Expiration
2045-11-28

AI Technical Summary

Technical Problem

Existing artificial joint coatings have limited functionality, poor osseointegration, and are prone to failure after prolonged use, leading to loosening. They also lack antibacterial properties and osteogenic synergy.

Method used

The surface-active coating employs a two-layer structure: an inner layer of magnesium-doped porous TiO₂ nanotube array and an outer layer of zinc/strontium co-doped mesoporous bioactive glass. It is grown in situ on the substrate using an electrochemical method to form a gradient structure, which synergistically releases magnesium, strontium, and zinc ions, mimicking the transition interface of natural bone tissue. It exhibits high bonding strength and strong antibacterial ability.

Benefits of technology

It significantly improves the stability and antibacterial ability of the coating, promotes osseointegration through the synergistic release of multiple ions, prolongs the functional life of the coating, reduces the risk of aseptic loosening, and achieves the unity and continuous high efficiency of antibacterial and osteogenic functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121243487B_ABST
    Figure CN121243487B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a surface active coating and application thereof, and belongs to the technical field of artificial joint coating. A magnesium-doped porous titanium dioxide nanotube array layer and a zinc-strontium co-doped mesoporous bioactive glass release layer are formed on the surface of a substrate. The coating not only surpasses other coatings in single performance such as coating bonding strength, osteogenic activity and antibacterial capacity, but also realizes the unity and continuous high efficiency of the performances through gradient and synergy system design. The application provides a new solution for solving two problems of artificial joint replacement, namely, aseptic loosening and antibacterial capacity, and has high clinical conversion value and market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of artificial joint coating technology, and in particular relates to a method for preparing a surface-active coating. Background Technology

[0002] Artificial joints are implantable prostheses made of biocompatible metallic materials and engineered to mimic the physiological joints of the human body. The aim is to remove lesions, eliminate pain, and restore joint mobility and function. Currently, total hip, knee, shoulder, and elbow replacement surgery has become one of the most successful surgical methods for treating end-stage joint diseases, significantly improving patients' quality of life. The long-term stability of interventional devices such as artificial joints, implants, bone screws, and spinal fusion devices depends on the formation of a strong and lasting osseointegration between the interventional device and the host bone. However, the surface of a simple metallic prosthesis is usually bioinert and difficult to form an effective biocompatible bond with bone tissue. Initially, prosthesis fixation mainly relied on the mechanical interlocking of bone cement. Although bone cement provides good immediate fixation, it carries the risk of long-term aging and fragmentation, and may cause complications such as allergic reactions. To achieve more ideal biocompatible fixation, surface modification technology has rapidly developed. By constructing specific coatings on the prosthesis surface, its surface properties can be significantly improved, thereby guiding bone tissue ingrowth and integration while maintaining the mechanical properties of the prosthesis matrix.

[0003] Despite significant advancements in coating technology, several shortcomings remain: 1. Traditional macroscopic coatings exhibit weak interfacial bonding, leading to easy peeling and detachment from the interface during long-term service; the degradation rate does not match the rate of new bone formation, resulting in premature loss of coating function; and they lack active antibacterial capabilities. 2. High doses of antibiotics or silver ions in single-functionalized coatings, while effectively antibacterial, may also be toxic to osteoblasts, inhibiting bone integration, resulting in a functional conflict between "antibacterial" and "osteogenic" processes; such coatings often face the challenges of initial burst release and subsequent failure, failing to achieve long-term, controllable release; simple physical mixing or single-layer structures struggle to coordinate the spatial distribution and release kinetics of multiple functional factors.

[0004] To address the bonding strength issue, patent CN112545711A discloses a femoral stem prosthesis and its preparation method, in which the bioactive coating includes a porous titanium coating and a hydroxyapatite coating. Although the bonding strength has been improved, the double-layer coating attempts to balance the strong bonding of the titanium coating with the bioactivity of HA. However, the problem of distal fibrous tissue growth still exists, which may lead to postoperative discomfort. Furthermore, the synergistic and unified function of antibacterial and osteogenic properties has not yet been achieved. Summary of the Invention

[0005] The purpose of this application is to provide a method for preparing a surface-active coating to solve the technical problems of existing artificial joint coatings having limited functionality, poor osseointegration, and easy failure after long-term use, leading to loosening.

[0006] To achieve the above objectives, the technical solution adopted in this application is: to provide a method for preparing a surface-active coating, specifically including the following steps: (i) Substrate pretreatment: The titanium alloy is ultrasonically cleaned and dried to obtain a pretreated substrate; (II) Inner Layer Preparation: S1. First anodizing: The pretreated substrate is placed in an electrolyte for oxidation reaction, forming a TiO2 nanotube array on the surface of the pretreated substrate to obtain the first substrate; S2, Nanotube Array Exfoliation: The first substrate is ultrasonically exfoliated to peel the TiO2 nanotube array layer from the first substrate, forming sites on the surface to obtain the second substrate; S3, Second Anodizing: The second substrate is placed in a magnesium-containing electrolyte for oxidation reaction. After the reaction is completed, crystallization treatment is performed, and magnesium is doped at the sites to form an inner layer, thus obtaining the third substrate; (III) Preparation of the outer layer: S1. Preparation of precursor solution: Hexadecyltrimethylammonium bromide, zinc nitrate, strontium nitrate and auxiliary components are mixed and stirred to prepare precursor solution; S2. Coating and self-assembly: The third substrate is immersed in the precursor solution, pulled out, aged, and heated; then cooled to room temperature, immersed in an aqueous solution containing BMP-2 mimic peptide and polyacrylic acid, and dried to obtain a surface-active coating.

[0007] In one embodiment, Step (1) The specific steps of ultrasonic cleaning are as follows: ultrasonically clean for 15 min each in acetone, anhydrous ethanol, 10 vol% dilute hydrochloric acid and deionized water.

[0008] In one embodiment, In step (ii) S1, the electrolyte is an ethylene glycol electrolyte containing 0.5 wt% NH4F and 2 vol% deionized water; the voltage for the oxidation reaction is 60 V.

[0009] In one embodiment, In step (ii) S2, the specific steps of ultrasound are as follows: immerse in 15% H2O2 solution and sonicate at 150 W for 10 min.

[0010] In one embodiment, In step (ii) S3, the electrolyte is an ethylene glycol electrolyte containing 0.5 wt% NH4F and 0.1 M magnesium acetate; the voltage for the oxidation reaction is 30-80 V.

[0011] In one embodiment, In step (ii) S3, the specific steps of the crystallization treatment are as follows: After the reaction is completed, the dried sample is placed in a muffle furnace and heated to 450 °C in air at a heating rate of 5 °C / min, held for 2 h, and then cooled with the furnace.

[0012] In one embodiment, In step (iii) S1, the precursor solution is prepared by dissolving hexadecyltrimethylammonium bromide in a mixed solution of deionized water and anhydrous ethanol, and then sequentially adding tetraethyl orthosilicate, calcium nitrate tetrahydrate, zinc nitrate, strontium nitrate and triethyl phosphate, stirring and mixing to obtain the precursor solution. The mass ratio of zinc nitrate to strontium nitrate is 1:1.0-2.0, and the pH of the precursor solution is 2.8-3.2.

[0013] In one embodiment, In step (iii) S2, the specific heating steps are as follows: place the aged sample into a tube furnace, heat it to 200 °C at a rate of 1 °C / min under nitrogen protection, and hold it at that temperature for 2 h.

[0014] In one embodiment, In step (iii) S2, the mass ratio of BMP-2 mimic peptide to polyacrylic acid is 1:2.

[0015] This application also provides an application of a surface-active coating, wherein any of the surface-active coatings described in the above embodiments is applied to artificial joints, artificial implants, bone screws, or spinal fusion devices.

[0016] This application provides a method for preparing a surface-active coating, which has the following advantages compared with the prior art: 1. In the two-layer structure, magnesium ions in the inner layer focus on strong bonding with the matrix and long-term osteogenic effect; the outer layer acts as a buffer and regulatory center, synergistically releasing osteogenic ions strontium and mild antibacterial ions zinc; the gradient structure simulates the transition interface of natural bone tissue in terms of physical properties and chemical composition, avoiding performance mutations, and is more conducive to host cell recognition, adhesion and tissue ingrowth. It is a biological fixation that significantly improves stability and solves the problem of mutual inhibition between antibacterial and osteogenic functions. 2. Under normal physiological pH conditions, the outer layer's nanovalve (polyacrylic acid) is in a contracted state, releasing strontium ions and BMP-2 mimic peptides at a slow, constant rate, continuously nourishing bone tissue and promoting bone integration. Under infected conditions, when bacterial growth leads to acidification of the local microenvironment, the polyacrylic acid segments expand, opening mesoporous channels and accelerating the release of zinc ions, providing precise antibacterial action on the infected area and extending the coating's functional lifespan. The synergistic effect of multiple ions changes the strategy of relying on a single ion or drug, constructing a Mg-Zn-Sr ion synergistic network. Magnesium ions promote early osteoblast adhesion and proliferation, strontium ions strongly stimulate bone formation and inhibit osteoclast activity, and zinc ions provide broad-spectrum, long-lasting, and low-cytotoxic antibacterial capabilities, while also aiding in osteogenic processes. The release of these three ions matches different stages of the bone healing process, resulting in osteogenic efficiency far exceeding that of single-ion coatings. The outer layer's pH-responsive antibacterial action ensures that even if a small number of bacteria invade, they are confined by the nanotube structure and cannot penetrate deeply. 3. The inner TiO2 nanotube array of this application is grown in situ on the substrate by electrochemical method, forming a strong chemical bond and mechanical interlock with the substrate. Its bonding strength is better than that of traditional spray coatings, reducing the risk of aseptic loosening caused by coating peeling and providing mechanical protection for the service life of the coating. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a partial SEM image of a TiO2 nanotube array. Figure 2 This is a BMP-2 mimic peptide release curve; Figure 3 This is a graph showing the number of bacterial colonies on a plate, as shown in Comparative Example 1. Figure 4 This is a graph showing the number of bacterial colonies on a plate in Example 1. Detailed Implementation

[0019] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, this application will be further described in detail. It should be understood that the specific embodiments described herein are only for explaining this application and are not intended to limit this application.

[0020] Example 1 (I) Substrate Pretreatment: Medical-grade Ti-6Al-4VELI titanium alloy was selected as the substrate material and cut into 10mm×10mm×1mm test pieces. The substrate was then ultrasonically cleaned for 15 minutes each in acetone, anhydrous ethanol, 10 vol% dilute hydrochloric acid, and deionized water to remove surface oil and natural oxide film. It was then dried with nitrogen to obtain the pretreated substrate. The surface roughness of the pretreated substrate was Ra = 0.36 μm, and the contact angle was <30°. ° ; (II) Inner layer preparation: (Magnesium-doped porous titanium dioxide nanotube array) S1. First anodizing: Using the pretreated substrate as the anode and the platinum electrode as the cathode, magnetic stirring was turned on, and the oxidation reaction was carried out at room temperature in an ethylene glycol electrolyte containing 0.5 wt% NH4F and 2 vol% deionized water at a DC voltage of 60 V for 2 h. After the reaction was completed, the substrate was rinsed with deionized water and dried to form a TiO2 nanotube array on the surface of the pretreated substrate, thus obtaining the first substrate. S2. Exfoliation of the nanotube array: The first substrate is immersed in a 15% H2O2 solution and sonicated at 150 W for 10 min to peel off the formed nanotube array layer from the first substrate, leaving regular and orderly pits on the surface as sites for the second oxidation; after peeling, the substrate is ultrasonically cleaned 3 times (3 min each time) with deionized water to remove residual H2O2 and obtain the second substrate. S3. Second Anodizing: Using the second substrate as the anode, the oxidation reaction was carried out at room temperature in an ethylene glycol electrolyte containing 0.5 wt% NH4F and 0.1 M magnesium acetate at 50 V DC for 1 h. After the reaction, the sample was thoroughly rinsed with deionized water and vacuum dried at 80 °C for 2 h. Crystallization Treatment: The dried sample was placed in a muffle furnace and heated to 450 °C in air at a heating rate of 5 °C / min, held at that temperature for 2 h, and then cooled with the furnace. This process transformed the amorphous TiO2 into anatase crystal (XRD detection showed that the purity of the anatase phase was >90%), and completed the doping of magnesium element, forming an inner layer to obtain the third substrate. (III) Outer layer preparation: (zinc / strontium co-doped mesoporous bioactive glass release layer) S1. Preparation of precursor solution: Dissolve 2.0 g of cetyltrimethylammonium bromide (CTAB) as a template agent in a mixed solution of 100 mL of deionized water and 20 mL of anhydrous ethanol. Then add 10 mL of tetraethyl orthosilicate (TEOS), 0.4 g of calcium nitrate tetrahydrate, 0.12 g of zinc nitrate, 0.18 g of strontium nitrate and 0.2 g of triethyl phosphate (TEP) in sequence. Stir vigorously for 4 h to ensure thorough mixing and hydrolysis. Control the pH of the solution at 2.8-3.2 with 0.1 M hydrochloric acid to obtain the precursor solution. S2. Coating and Self-Assembly: The third substrate was immersed in the precursor solution and pulled out at a uniform speed of 1 cm / min to ensure uniform adhesion of the solution to the inner and outer walls of the nanotube. The sample was then aged at 50 °C for 24 h. The aged sample was placed in a tube furnace and heated to 200 °C at a rate of 1 °C / min under nitrogen protection and held for 2 h to remove CTAB and fix the mesoporous structure. The sample was then cooled to room temperature and immersed in an aqueous solution containing 50 mg of BMP-2 mimic peptide (sequence: KIPKASSVPTELSAISTLYL, obtained by solid-phase synthesis) and 100 mg of polyacrylic acid (nanovalve). The sample was then vacuum-impregnated at 40 °C for 2 h to allow the mimic peptide and polyacrylic acid to enter the mesoporous channels (the mesoporous pore size was measured by BET, with an average pore size of 8 ± 0.7 nm). Finally, the sample was vacuum-dried at 80 °C for 2 h to obtain a surface-active coating with a two-layer structure.

[0021] Example 2 The difference between this embodiment and embodiment 1 is that in step (ii) S3, the DC voltage for the oxidation reaction is 30 V, while the rest of the operation is the same, and a surface-active coating is obtained.

[0022] Example 3 The difference between this embodiment and embodiment 1 is that in step (ii) S3, the DC voltage for the oxidation reaction is 80 V, while the rest of the operation is the same, and a surface-active coating is obtained.

[0023] Example 4 The difference between this embodiment and Example 1 is that the mass ratio of zinc nitrate to strontium nitrate is 1:1.0, while the rest of the operations are the same, and a surface-active coating is obtained.

[0024] Example 5 The difference between this embodiment and Example 1 is that the mass ratio of zinc nitrate to strontium nitrate is 1:2.0, while the rest of the operations are the same, and a surface-active coating is obtained.

[0025] Comparative Example 1 Medical-grade Ti-6Al-4VELI titanium alloy plasma-sprayed hydroxyapatite coating.

[0026] Comparative Example 2 Samples were prepared with only the inner layer and not the outer layer.

[0027] Experimental Example 1 TiO2 nanotube array diameter SEM measurement: The coating morphology of the third substrate prepared in Example 1 was characterized by scanning electron microscopy, such as... Figure 1 As shown, a highly ordered array of nanotubes with clear openings was formed on the sample surface; the average inner diameter of randomly selected nanotubes was 85±8 nm.

[0028] TiO2 nanotube array tube length measurement: The "spin coating + pull-up combination" process was adopted. The sample was first fixed on the rotating stage, the rotation speed was 500 rpm, the precursor solution (1 mL / cm²) was added and the rotation was 10 s, and then the tube was pulled up at a speed of 1 cm / min. The average tube length was measured to be 1.8 ± 0.1 μm.

[0029] Experiment Example 2 BMP-2 simulated peptide release: The final product prepared in Example 1 was placed in PBS buffer and incubated in a constant-temperature shaker at 37 °C to simulate the internal environment of the human body; a certain amount of release medium was collected on days 1, 3, 7, 14, 21, and 28, and an equal amount of fresh buffer was added at the same temperature to maintain a constant total volume; the peptide concentration was quantitatively analyzed by HPLC, and the release curve was plotted as shown in the figure. Figure 2 As shown, the release rate of the BMP-2-mimicking peptide coating was 73±2.06% on day 12, and then entered a sustained slow release phase, with a cumulative release rate of 86±1.43% over 28 days, which meets the sustained release requirements for bone repair.

[0030] Experimental Example 3 The bond strength pull-out test was performed according to ASTM C633 standard, and the results are as follows: Comparative Example 1: 35 MPa; Comparative Example 2: 60 MPa; Example 1: 55 MPa. Fracture occurred in the adhesive or outer layer. The entire coating system was firmly bonded to the substrate, meeting the requirements for implants.

[0031] Experiment Example 4 In vitro wear tests were conducted using ASTM F732 standard to simulate joint friction conditions. The coated substrate prepared in Example 1 was mounted on a pin-disc friction and wear tester as a fixed disk, with medical-grade zirconia ceramic balls as the mating element. The test was conducted at 37 °C in 25% fetal bovine serum lubricant, with a vertical load of 20 N, a sliding frequency of 1 Hz, and a total sliding distance of 1000 m. After the test, the wear trajectory on the disk surface was measured using a white light interferometer, and the volumetric wear of the coating was calculated. The results showed that the specific wear rate of the coating of this invention was 1 × 10⁻⁶. -6 mm³ / (N It has excellent wear resistance.

[0032] Experimental Example 5 To evaluate the bactericidal ability of the coating of the present invention against surface-adhered bacteria, Staphylococcus aureus (S. aureus, ATCC 25923) was cultured on the coatings of Example 1 and Comparative Example 1, respectively, and incubated on a shaker at 37 °C for 24 h for in vitro antibacterial performance evaluation. Comparative Example 1 served as the negative control group, and Example 1 served as the experimental group. After 24 h, the bacteria co-cultured in the negative control group and the experimental group were diluted to 10⁵ CFU / mL, spread on LB agar plates, and observed after incubation at 37 °C for 24 h. The results are as follows. Figure 3-4 As shown, the number of Staphylococcus aureus on the plate clearly shows a significant difference between the two. The coating prepared in Comparative Example 1 has a large number of live bacteria on its surface, while the coating prepared in Example 1 can effectively kill the bacteria adhering to its surface and has excellent contact antibacterial ability.

[0033] This application provides a method for preparing a surface-active coating. The surface-active coating prepared in this application not only surpasses the existing technology in terms of individual properties such as coating bonding strength, osteogenic activity and antibacterial ability, but more importantly, it achieves the unification and continuous high efficiency of these properties through its gradient and synergistic system design. It provides a new solution to solve the two major problems of artificial joint replacement: aseptic loosening and antibacterial ability, and has extremely high clinical translational value and market prospects.

[0034] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0035] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method for preparing a surface-active coating, characterized in that, Specifically, the following steps are included: (i) Substrate pretreatment: The titanium alloy is ultrasonically cleaned and dried to obtain a pretreated substrate; (II) Inner Layer Preparation: S1. First anodizing: The pretreated substrate is placed in an electrolyte for an oxidation reaction, and a TiO2 nanotube array is formed on the surface of the pretreated substrate to obtain the first substrate; S2, Nanotube array peeling: The first substrate is ultrasonically peeled off the TiO2 nanotube array layer from the first substrate, forming sites on the surface to obtain the second substrate; S3. Second anodizing: The second substrate is placed in a magnesium-containing electrolyte for oxidation reaction. After the reaction is completed, crystallization treatment is performed, and magnesium is doped at the site to form an inner layer, thus obtaining the third substrate. (III) Preparation of the outer layer: S1. Preparation of the precursor solution: Hexadecyltrimethylammonium bromide is dissolved in a mixed solution of deionized water and anhydrous ethanol. Tetraethyl orthosilicate, calcium nitrate tetrahydrate, zinc nitrate, strontium nitrate, and triethyl phosphate are added sequentially and stirred to obtain the precursor solution. The mass ratio of zinc nitrate to strontium nitrate is 1:1.0-2.0, and the pH of the precursor solution is 2.8-3.

2. S2. Coating and self-assembly: The third substrate is immersed in the precursor solution, pulled out, aged, and heated; cooled to room temperature, immersed in an aqueous solution containing BMP-2 mimic peptide and polyacrylic acid, and dried to obtain a surface-active coating. In step (ii) S1, the electrolyte is an ethylene glycol electrolyte containing 0.5 wt% NH4F and 2 vol% deionized water; the voltage of the oxidation reaction is 60 V; In step (ii) S3, the electrolyte is an ethylene glycol electrolyte containing 0.5 wt% NH4F and 0.1 M magnesium acetate; the voltage for the oxidation reaction is 30-80 V; In step (iii) S2, the mass ratio of the BMP-2 mimic peptide to polyacrylic acid is 1:

2.

2. The method for preparing a surface-active coating according to claim 1, characterized in that, The specific steps of ultrasonic cleaning in step (1) are as follows: ultrasonic cleaning for 15 minutes each in acetone, anhydrous ethanol, 10 vol% dilute hydrochloric acid and deionized water.

3. The method for preparing a surface-active coating according to claim 1, characterized in that, In step (ii) S2, the specific steps of the ultrasound are as follows: immerse in a 15% H2O2 solution and sonicate at 150 W for 10 min.

4. The method for preparing a surface-active coating according to claim 1, characterized in that, In step (ii) S3, the specific steps of the crystallization treatment are as follows: after the reaction is completed, the dried sample is placed in a muffle furnace and heated to 450 °C in air at a heating rate of 5 °C / min, held for 2 h, and then cooled with the furnace.

5. The method for preparing a surface-active coating according to claim 1, characterized in that, In step (iii) S2, the specific heating steps are as follows: the aged sample is placed in a tube furnace and heated to 200 °C at a rate of 1 °C / min under nitrogen protection, and held at that temperature for 2 h.

Citation Information

Patent Citations

  • Femoral stem prosthesis and preparation method thereof

    CN112545711A

  • TiO2 nanometer pore array material preparation method and uses thereof