Modified polyaryletherketone composite material with high dimensional stability and high conductivity and preparation method thereof
By functionalizing carbon nanomaterials and generating conductive nanomaterials in situ, combined with interface modifiers, the problems of high insulation and molding shrinkage of polyaryletherketone materials were solved, and a composite material with high conductivity and high dimensional stability was achieved.
Patent Information
- Application Number
- CN202511618020.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-06
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-11-06
AI Technical Summary
The high insulation and high molding shrinkage of polyaryletherketone materials limit their application in precision electronic devices, electrostatic protection and electromagnetic shielding. In addition, uneven dispersion of conductive fillers in traditional processes leads to interfacial stress concentration and dimensional distortion.
By functionalizing carbon nanomaterials, nano-conductive materials are generated in situ on their surface. Combined with interface modifiers, a composite conductive structure is formed, which reduces filler agglomeration and improves conductivity and dimensional stability.
While maintaining high conductivity, the interfacial shear strength is significantly improved, the thermal expansion coefficient and volume shrinkage rate of the composite are controlled, and the material achieves high dimensional stability.
Smart Images

Figure SMS_2 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite material processing technology, specifically to a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity, and its preparation method. Background Technology
[0002] With the rapid development of high-end industrial fields such as aerospace, precision instruments, biomedicine, and next-generation communication technologies, increasingly stringent requirements are being placed on the functionality of key structural materials. Ideal materials not only need to serve as load-bearing or encapsulating components, possessing excellent mechanical properties, thermal stability, and chemical stability, but are also expected to integrate electronic functions such as sensing, transmission, and electromagnetic shielding, achieving structural-functional integration. Against this backdrop, special engineering plastics, due to their unique performance advantages, are gradually expanding from traditional insulating structural components to functional and precision applications.
[0003] Polyaryletherketone (PAEK), as one of the top-tier materials in the specialty engineering plastics pyramid, possesses an unparalleled comprehensive performance due to the alternating aromatic rings, ether bonds, and ketone bonds in its molecular backbone. Its excellent high-temperature resistance (long-term operating temperature exceeding 250°C), superior mechanical strength, outstanding creep resistance, excellent chemical corrosion resistance, and inherent flame retardancy allow it to maintain stable performance even in harsh environments. Furthermore, PAEK exhibits good biocompatibility and has been widely used in orthopedic implants and surgical instruments. However, it is precisely its highly stable aromatic ring structure that limits its electrical insulation properties (volume resistivity typically higher than 10 Ω·cm). 16 The high viscosity (Ω·cm) and large molding shrinkage (1.5-3.0%) of PAEK significantly limit its direct application in precision electronic devices, electrostatic protection, electromagnetic shielding, and high-performance sensors. In existing technologies, adding conductive fillers can improve conductivity, but uneven filler dispersion easily leads to interfacial stress concentration, causing dimensional distortion. Furthermore, the high melt viscosity (>1000 Pa·s) of PAEK in traditional processes further exacerbates the problem of uneven filler distribution, resulting in poor continuity of the conductive network and insufficient dimensional stability. Summary of the Invention
[0004] To address the technical challenges of high insulation and high molding shrinkage in PAEK materials, this invention provides a modified polyaryletherketone composite material with high dimensional stability and high conductivity, along with its preparation method. This invention treats conductive carbon materials to form a composite conductive structure, and, combined with an interface modifier, reduces filler agglomeration while significantly improving the conductivity and dimensional stability of the composite material.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solution:
[0006] A modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity, comprising the following materials: modified carbon material with at least one dimension, interface modifier, and PAEK resin;
[0007] The modified carbon material has a structure in which a nano-conductive material is attached in situ to the surface of the carbon nanomaterial, and the nano-conductive material is a nano-conductive metal or a nano-conductive metal oxide.
[0008] Furthermore, the composite material comprises 100% by weight of the following materials: 5%-25% modified carbon material with at least one dimension, 1%-3% interface modifier, and the balance being PAEK resin.
[0009] The proportion of the nano-conductive material in the modified carbon material is in the range of 5%-60%, and preferably the proportion of the nano-conductive material in the modified carbon material is 15%-50%.
[0010] Furthermore, the carbon nanomaterial is one or more of carbon nanotubes, carbon nanorods, and carbon fibers with oxygen-containing groups (hydroxyl and / or carboxyl groups) on the surface;
[0011] The nano-conductive metal is one or more of nano-silver, nano-gold, and nano-copper generated in situ on the surface of the carbon nanomaterial.
[0012] The nano-conductive metal oxide is formed in situ on the surface of the carbon nanomaterial by one or more of nano-indium tin oxide, nano-tin antimony oxide, and nano-aluminum-doped zinc oxide.
[0013] Furthermore, the carbon nanomaterial is selected from one or more of the following: carbon nanotubes with a diameter less than 50 nm and an aspect ratio greater than 500, carbon nanorods with a diameter less than 50 nm and an aspect ratio greater than 500, and carbon fibers with a diameter less than 300 nm and a length of at least 1 μm; the average particle size of the nanoconductive material does not exceed 200 nm.
[0014] Furthermore, the modified carbon material is obtained by the following steps: forming functionalized carbon nanomaterials by giving the surface of the carbon nanomaterials oxygen-containing groups (hydroxyl and / or carboxyl groups); adsorbing metal ions using the oxygen-containing groups as anchoring sites; growing nano-conductive materials in situ on the surface of the functionalized carbon nanomaterials by one or more of chemical reduction, co-precipitation, hydrothermal, and solvothermal methods; and performing heat treatment or no heat treatment to obtain a modified carbon material with a structure in situ attached nano-conductive materials on the surface of carbon nanomaterials.
[0015] Furthermore, when the structure of the modified carbon material is that a nano-conductive metal is attached to the surface of a carbon nanomaterial in situ, the modified carbon material is obtained by the following steps: dispersing the functionalized carbon nanomaterial in one or more solutions of a water-soluble silver source, a water-soluble gold source, and a water-soluble copper source to form a reaction solution with a concentration of 5-10 g / L; heating to 60-100°C under a protective atmosphere; adding a reducing agent; stirring to carry out a reduction reaction for 0.5-4 h; and cooling, washing, and drying to obtain the modified carbon material with a structure of a nano-conductive metal attached to the surface of a carbon nanomaterial in situ.
[0016] The reducing agent is selected from sodium citrate and / or ascorbic acid; the water-soluble silver source is nitrate; the water-soluble gold source is chloroauric acid; and the water-soluble copper source is copper sulfate or copper acetate.
[0017] Furthermore, when the structure of the modified carbon material is that the carbon nanomaterial has nano-conductive metal oxides attached to its surface in situ, the modified carbon material is obtained by the following steps: dispersing the functionalized carbon nanomaterial in a water-soluble raw material solution to form a reaction solution with a concentration of 5-10 g / L, adding an alkaline precipitant dropwise under stirring until the final pH value is greater than 8, transferring it to a high-pressure reactor lined with polytetrafluoroethylene and carrying out a hydrothermal reaction at 120-200℃ for 6-24 h, cooling, washing, drying, and then calcining at 300-800℃ for 1-5 h to obtain the modified carbon material with the structure of carbon nanomaterial having nano-conductive metal oxides attached to its surface in situ;
[0018] The water-soluble raw material solution is one of the following: a mixed solution of tin tetrachloride (SnCl4) and antimony trichloride (SbCl3) prepared in an atomic ratio of Sn:Sb = 90:10-95:5; a mixed solution of indium trichloride (InCl3) and tin tetrachloride (SnCl4) prepared in an atomic ratio of In:Sn = 90:10; or a mixed solution of zinc acetate ((CH3COO)2Zn·2H2O) and aluminum nitrate (Al(NO3)3·9H2O) or aluminum isopropoxide (Al(O-iPr)3) prepared in an atomic ratio of Zn:Al = 95:5-98:2.
[0019] The alkaline precipitant is a 0.5-2 mol / L sodium hydroxide solution or an ammonia solution; when in-situ generation of nano-indium tin oxide is required, the endpoint pH is 8.5-9.5; when in-situ generation of nano-tin antimony oxide is required, the endpoint pH is 8.0-9.0; when in-situ generation of nano-aluminum-doped zinc oxide is required, the endpoint pH is 8.0-9.0.
[0020] Furthermore, a method for functionalizing carbon nanomaterials by giving the surface of the carbon nanomaterials oxygen-containing groups is as follows: the carbon nanomaterials are ultrasonically treated at 140-150°C for 1-2 hours with a mixed acid of nitric acid and sulfuric acid in a volume ratio of 1:2-4, washed with water until neutral, and then dried to obtain functionalized carbon nanomaterials.
[0021] The PAEK resin is selected from one or more of polyetheretherketone (PEEK), polyetherketone (PEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), and polyetherketoneetherketoneketone (PEKEKK).
[0022] The interface modifier is a sulfonated bisphenol AF type polyether ether ketone. Bisphenol AF type polyether ether ketone powder with an average particle size of less than 1 mm is mixed with 95wt%-98wt% concentrated sulfuric acid at a ratio of 1 g: 5-20 mL. The mixture is stirred and reacted at 40-60℃ for 0.5-4 h. The product is precipitated with cold water, washed, and dried to obtain the sulfonated bisphenol AF type polyether ether ketone. The degree of sulfonation is controlled to be approximately 30%-50%.
[0023] The M of the bisphenol AF type polyether ether ketone n =1-3×10 5 g / mol, M w =5-8×10 5 g / mol, PDI = 1-3.5.
[0024] For example, the chemical structure of bisphenol AF type polyether ether ketone can be:
[0025] ;
[0026] The conventional method for preparing polyether ether ketone involves, under a protective atmosphere, bisphenol AF and 4,4'-difluorobenzophenone in an equimolar ratio in the presence of anhydrous sodium carbonate and / or anhydrous potassium carbonate (100%-120% of the molar amount of bisphenol AF) in a sulfolane solvent and a dehydrating agent. The mixture is first heated to 130-150°C and refluxed until the theoretical water yield is reached. The dehydrating agent is then evaporated, and the temperature is raised to 190-220°C for polymerization for 3-8 hours. After the reaction is complete, the product is precipitated using a poor solvent (such as water), washed, and dried to obtain bisphenol AF-type polyether ether ketone.
[0027] The second aspect of the present invention provides a method for preparing a modified polyaryletherketone composite material with high dimensional stability and high conductivity, comprising the following steps: mixing a modified carbon material having at least one dimension, an interface modifier, and PAEK resin according to a formula, followed by melt blending to obtain granules, and then crystallizing them.
[0028] The modified carbon material is composed of a carbon nanomaterial with an in-situ attached nano-conductive material on its surface, wherein the nano-conductive material is a nano-conductive metal or a nano-conductive metal oxide.
[0029] The melt blending is achieved using a twin-screw extruder with the following parameters: melt blending temperature 350-400℃, vacuum devouring pressure less than 10kPa;
[0030] The crystallization process involves placing the obtained granules in a molding die and pressing them under pressure of at least 8 MPa and heating them at 380-400°C for 10-40 minutes, followed by cooling at a rate of less than 3°C / min to induce crystallization.
[0031] Beneficial technical effects: This invention functionalizes nano-carbon materials with oxygen-containing groups, and then generates nano-conductive materials in situ on their surface to form a composite synergy, creating a "skeleton-bridging" composite conductive structure. This reduces stress concentration caused by filler agglomeration while reducing the amount of filler added. Combined with sulfonated polyether ether ketone as an interface modifier, the sulfonic acid groups form strong hydrogen bonds with the carboxyl groups on the filler surface, while the fluoride molecular chains can better integrate with the matrix resin. This allows the composite material to maintain high conductivity while significantly improving interfacial shear strength, and controlling the thermal expansion coefficient and volume shrinkage rate of the composite material at a low level. Detailed Implementation
[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0033] Unless otherwise specifically stated, the numerical values set forth in these embodiments do not limit the scope of the invention. Techniques and methods known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques and methods should be considered part of the specification. In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that values expressed, for example, as "within the range of ab" or "between the range of ab," do not include the endpoint values a and b; values expressed as "for ab," "is ab," or "ab" include the endpoint values a and b.
[0034] Experimental methods not specified in the following examples are generally performed according to national standards; if there is no corresponding national standard, they are performed according to general standard requirements or general methods.
[0035] Preparation Example 1
[0036] The preparation method of bisphenol AF type polyether ether ketone includes the following steps:
[0037] 0.5 mol of bisphenol AF, 0.5 mol of 4,4'-difluorobenzophenone, 0.55 mol of anhydrous sodium carbonate (200 mesh), 300 mL of sulfolane solvent, and 60 mL of xylene as a dehydrating agent were added to the reaction vessel. Under a nitrogen-denitrile atmosphere, the mixture was first heated to 150 °C for reflux to remove water until the theoretical water output was reached. The reaction was continued at this temperature for 30 min. The xylene was then evaporated by heating, and the temperature was raised to 220 °C for polymerization for 5.5 h. After the reaction was complete, the product was precipitated with water, washed, and dried to obtain bisphenol AF-type polyether ether ketone. GPC molecular weight analysis showed that the product M... n =2.7×10 5 g / mol, M w =7.9×10 5 g / mol, PDI=2.92.
[0038] Preparation Example 2
[0039] The bisphenol AF type polyether ether ketone obtained in Preparation Example 1 was pulverized to an average particle size of less than 500 micrometers. It was then added to 98wt% concentrated sulfuric acid at a ratio of 1g:10mL. After stirring and dissolving at 50°C, the reaction was continued for 3 hours. The product was precipitated by cold water, washed, and dried to obtain the sulfonated bisphenol AF type polyether ether ketone, which was designated as SF-PEEK-1.
[0040] Preparation Example 3
[0041] The bisphenol AF type polyether ether ketone obtained in Preparation Example 1 was pulverized to an average particle size of less than 500 micrometers. It was then added to 98wt% concentrated sulfuric acid at a ratio of 1g:10mL. After stirring and dissolving at 40°C, the reaction was continued for 4 hours. The product was precipitated by cold water, washed, and dried to obtain the sulfonated bisphenol AF type polyether ether ketone, which was designated as SF-PEEK-2.
[0042] Preparation Example 4
[0043] The bisphenol AF type polyether ether ketone obtained in Preparation Example 1 was pulverized to an average particle size of less than 500 micrometers. It was then added to 98wt% concentrated sulfuric acid at a ratio of 1g:15mL. After stirring and dissolving at 60°C, the reaction was continued for 2 hours. The product was precipitated by cold water, washed, and dried to obtain the sulfonated bisphenol AF type polyether ether ketone, which was designated as SF-PEEK-3.
[0044] Preparation Example 5
[0045] The modified carbon material in this case consists of multi-walled carbon nanotubes with in-situ attached silver nanoparticles. The preparation process is as follows:
[0046] Multi-walled carbon nanotubes (inner diameter 10-40 nm, aspect ratio greater than 500) were dispersed in a mixed acid of nitric acid and sulfuric acid with a volume ratio of 1:3. The amount of multi-walled carbon nanotubes and mixed acid was 1 g / 10 mL. The mixture was ultrasonically treated at 150 °C for 1 h, washed with water until neutral, and then dried to obtain multi-walled carbon nanotubes with oxygen-containing groups (hydroxyl and / or carboxyl groups).
[0047] The obtained functionalized multi-walled carbon nanotubes were added to an aqueous solution of silver nitrate, with a concentration of 5 g / L. The amount of silver nitrate used was calculated based on the Ag loading being 20% of the mass of the functionalized multi-walled carbon nanotubes. After ultrasonic treatment in an ultrasonic cleaner for 30 min, the mixture was stirred at room temperature for 1 h to allow silver ions to be fully adsorbed onto the surface of the carbon nanotubes. Under a nitrogen protective atmosphere, the mixture was heated to 80 °C, and ascorbic acid solution (molar ratio of ascorbic acid to silver ions was 1.5:1) was added dropwise. The mixture was stirred for another 2 h to carry out the reduction reaction. After the reaction was completed, the mixture was naturally cooled to room temperature and washed multiple times with deionized water and ethanol by centrifugation. Finally, the mixture was dried in a vacuum drying oven at 60 °C for 12 h to obtain a modified carbon material with in-situ silver nanoparticles attached to the surface of carbon nanotubes.
[0048] Preparation Example 6
[0049] The modified carbon material in this case has a structure of in-situ attached copper nanotubes on the surface of multi-walled carbon nanotubes. The preparation process is as follows:
[0050] Multi-walled carbon nanotubes (inner diameter 10-40 nm, aspect ratio greater than 500) were dispersed in a mixed acid of nitric acid and sulfuric acid with a volume ratio of 1:3. The amount of multi-walled carbon nanotubes and mixed acid was 1 g / 8 mL. The mixture was ultrasonically treated at 145 °C for 1.5 h, washed with water until neutral, and then dried to obtain multi-walled carbon nanotubes with oxygen-containing groups (hydroxyl and / or carboxyl groups).
[0051] Under nitrogen protection, the obtained functionalized multi-walled carbon nanotubes were added to an aqueous solution of copper acetate. The concentration of the functionalized multi-walled carbon nanotubes in the aqueous solution of copper acetate was 8 g / L. The amount of copper acetate used was calculated based on the loading of Cu being 35% of the mass of the functionalized multi-walled carbon nanotubes. PVP30 was then added as a stabilizer (concentration of 1 wt% in the system). After ultrasonic treatment in an ultrasonic cleaner for 30 min, the mixture was stirred at room temperature for 1 h to allow copper ions to be fully adsorbed onto the surface of the carbon nanotubes. The mixture was then heated to 80 °C, and ascorbic acid solution (molar ratio of ascorbic acid to silver ions was 2:1, and the addition was completed over 15-20 minutes) was added dropwise. The mixture was stirred for 3 h to carry out the reduction reaction. After the reaction was completed, the mixture was naturally cooled to room temperature. It was then centrifuged and washed multiple times with deionized water and ethanol, freeze-dried, and then vacuum-dried at 60 °C to obtain a modified carbon material with in-situ attached nano-copper on the surface of carbon nanotubes.
[0052] Preparation Example 7
[0053] The modified carbon material in this case consists of multi-walled carbon nanotubes with in-situ attached aluminum-doped zinc oxide nanoparticles. The preparation process is as follows:
[0054] Multi-walled carbon nanotubes (inner diameter 10-40 nm, aspect ratio greater than 500) were dispersed in a mixed acid of nitric acid and sulfuric acid with a volume ratio of 1:3. The amount of multi-walled carbon nanotubes and mixed acid was 1 g / 5 mL. The mixture was ultrasonically treated at 140 °C for 2 h, washed with water until neutral, and then dried to obtain multi-walled carbon nanotubes with oxygen-containing groups (hydroxyl and / or carboxyl groups).
[0055] The obtained functionalized multi-walled carbon nanotubes were added to a mixed aqueous solution of zinc acetate and aluminum nitrate. The concentration of the functionalized multi-walled carbon nanotubes in the silver nitrate aqueous solution was 5 g / L. The amount of AZO was calculated based on the AZO loading being 25% of the mass of the functionalized multi-walled carbon nanotubes. Then, based on the AZO amount, the amounts of zinc acetate and aluminum nitrate were prepared according to the Zn:Al atomic ratio of 97:3. After ultrasonic treatment in an ultrasonic cleaner for 30 min, continuous stirring for 1 h, and then heating to 60℃ and holding at that temperature, 1 mol / L aluminum nitrate was added dropwise. Ammonia water was used for co-precipitation. The pH value of the solution was monitored in real time with a pH meter and the pH value was precisely controlled between 8.5 and 9.0. After reaching the target pH, the solution was stirred at 60°C for 2 hours to age the precipitate. After separating the precipitate, it was washed three times with deionized water and anhydrous ethanol alternately to thoroughly remove impurities such as ammonium ions and nitrate ions. The precipitate was dried in an oven at 80°C for 12 hours to obtain the precursor powder. Then, under nitrogen protection, the temperature was increased to 500°C at 3°C / min and calcined for 2 hours. After cooling along the path, the modified carbon material with the structure of in-situ attached nano-AZO on the surface of carbon nanotubes was obtained.
[0056] Example 1
[0057] This case study describes a method for preparing a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity, including the following steps:
[0058] In Preparation Example 5, 12 wt% of a modified carbon material with in-situ attached silver nanoparticles on the surface of carbon nanotubes, 2 wt% of an interface modifier SF-PEEK-1, and the balance up to 100 wt% of PEEK resin were mixed evenly. The mixture was then melt-blended and extruded using a twin-screw extruder at 360-390°C and a vacuum devouring pressure of less than 10 kPa to obtain granules. The granules were then placed in a molding die and molded under a pressure of 10 MPa and a heating temperature of 380°C for 30 min. After that, the mixture was cooled at a rate of less than 3°C / min to induce crystallization, resulting in a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity.
[0059] Example 2
[0060] This case study describes a method for preparing a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity, including the following steps:
[0061] In Preparation Example 6, 18 wt% of a modified carbon material with in-situ attached copper nanotubes, 2 wt% of an interface modifier SF-PEEK-2, and the balance up to 100 wt% of PEEK resin were mixed evenly. The mixture was then melt-blended and extruded using a twin-screw extruder at 360-390°C and a vacuum devouring pressure of less than 10 kPa to obtain granules. The granules were then placed in a molding die and molded at 15 MPa and 380°C for 30 min. Afterward, the mixture was cooled at a rate of less than 3°C / min to induce crystallization, resulting in a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity.
[0062] Example 3
[0063] This case study describes a method for preparing a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity, including the following steps:
[0064] In Preparation Example 7, 25 wt% of a modified carbon material with in-situ attached nano-AZO on the surface of carbon nanotubes, 3 wt% of an interface modifier SF-PEEK-3, and the balance up to 100 wt% of PEEK resin were mixed evenly. The mixture was then melt-blended and extruded using a twin-screw extruder at 360-390°C and a vacuum devouring pressure of less than 10 kPa to obtain granules. The granules were then placed in a molding die and molded at 12 MPa and 380°C for 40 min. After that, the mixture was cooled at a rate of less than 3°C / min to induce crystallization, resulting in a modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity.
[0065] Comparative Example 1
[0066] The preparation process in this case is the same as in Example 1, except that the modified carbon material is replaced with 10wt% of multi-walled carbon nanotubes (inner diameter 10-40nm, aspect ratio greater than 500) and 2wt% of silver nanoparticles (20-50nm).
[0067] Comparative Example 2
[0068] The preparation process in this case is the same as in Example 1, except that the modified carbon material is replaced with 12wt% of multi-walled carbon nanotubes (inner diameter 10-40nm, aspect ratio greater than 500).
[0069] Comparative Example 3
[0070] The preparation process in this case is the same as in Example 1, except that the modified carbon material is replaced with 12wt% of nano-silver particles (20-50nm).
[0071] Comparative Example 4
[0072] The preparation process in this case is the same as in Example 1, except that the interface modifier is sulfonated polyether ether ketone (sulfonation degree 45%).
[0073] Comparative Example 5
[0074] The preparation process in this case is the same as in Example 1, except that the interface modifier is the fluorinated polyether ether ketone used in Preparation Example 1.
[0075] Test case
[0076] The performance of the composite materials in the above cases was tested, and the results are shown in Table 1.
[0077] Table 1 Properties of Composite Materials
[0078]
[0079] As shown in Table 1, this invention functionalizes multi-walled carbon nanotubes with oxygen-containing groups, and then generates a composite synergistic conductive structure of nano-conductive materials in situ on their surface. Combined with sulfonated polyether ether ketone as an interface modifier, the sulfonic acid groups form strong hydrogen bonds with the carboxyl groups on the filler surface, while the fluoride molecular chains can better integrate with the matrix resin. This reduces filler agglomeration in the composite material and enables high conductivity with a low filler addition amount, while significantly improving the interfacial shear strength and controlling the thermal expansion coefficient and volume shrinkage rate of the composite material at a low level.
[0080] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A modified polyaryletherketone composite material with high dimensional stability and high electrical conductivity, characterized in that, The material comprises the following 100% by weight percentages: 5%-25% modified carbon material, 1%-3% interface modifier, and the balance being PAEK resin; The modified carbon material has a structure in which a nano-conductive material is attached in situ to the surface of a carbon nanomaterial. The nano-conductive material is a nano-conductive metal or a nano-conductive metal oxide. The proportion of the nano-conductive material in the modified carbon material is 15%-50%. The carbon nanomaterial is a carbon nanotube with oxygen-containing groups on its surface, the carbon nanotube has a diameter of less than 50 nm and an aspect ratio of greater than 500; the average particle size of the nano-conductive material does not exceed 200 nm. The nano-conductive metal is one or more of nano-silver, nano-gold, and nano-copper generated in situ on the surface of the carbon nanomaterial. The nano-conductive metal oxide is formed in situ on the surface of the carbon nanomaterial by one or more of nano-indium tin oxide, nano-tin antimony oxide, and nano-aluminum-doped zinc oxide. A method for forming carbon nanotubes with oxygen-containing groups on the surface: The carbon nanotubes are ultrasonically treated at 140-150℃ for 1-2 hours with a mixed acid of nitric acid and sulfuric acid in a volume ratio of 1:2-4, washed with water until neutral, and then dried. The interface modifier is a sulfonated bisphenol AF type polyether ether ketone. Bisphenol AF type polyether ether ketone powder with an average particle size of less than 1 mm is added to 95 wt%-98 wt% concentrated sulfuric acid at a ratio of 1 g: 5-20 mL. The mixture is stirred and reacted at 40-60℃ for 0.5-4 h. The product is precipitated with cold water, washed, and dried to obtain the sulfonated bisphenol AF type polyether ether ketone. The Mn of the bisphenol AF type polyether ether ketone is 1-3×10. 5 g / mol, Mw = 5-8 × 10 5 g / mol, PDI = 1-3.5; the chemical structure of the bisphenol AF type polyether ether ketone is: 。 2. The modified polyaryletherketone composite material with high dimensional stability and high conductivity according to claim 1, characterized in that, The modified carbon material is obtained by the following steps: forming functionalized carbon nanomaterials by giving the surface of the carbon nanomaterials oxygen-containing groups; adsorbing metal ions using the oxygen-containing groups as anchoring sites; growing nano-conductive materials in situ on the surface of the functionalized carbon nanomaterials by one or more of the following methods: chemical reduction, co-precipitation, hydrothermal, and solvothermal; and performing heat treatment or no heat treatment to obtain a modified carbon material with the structure of nano-conductive materials attached to the surface of carbon nanomaterials in situ.
3. The modified polyaryletherketone composite material with high dimensional stability and high conductivity according to claim 2, characterized in that, When the structure of the modified carbon material is that the conductive metal nanoparticles are attached to the surface of the carbon nanomaterials in situ, the modified carbon material is obtained by the following steps: dispersing the functionalized carbon nanomaterials in one or more solutions of water-soluble silver source, water-soluble gold source, and water-soluble copper source to form a reaction solution with a concentration of 5-10 g / L; heating to 60-100°C under a protective atmosphere; adding a reducing agent; stirring to carry out a reduction reaction for 0.5-4 h; cooling, washing, and drying to obtain the modified carbon material with the structure of conductive metal nanoparticles attached to the surface of the carbon nanomaterials in situ. The reducing agent is selected from sodium citrate and / or ascorbic acid; the water-soluble silver source is nitrate; the water-soluble gold source is chloroauric acid; and the water-soluble copper source is copper sulfate or copper acetate.
4. The modified polyaryletherketone composite material with high dimensional stability and high conductivity according to claim 2, characterized in that, When the structure of the modified carbon material is that the nano-conductive metal oxide is attached to the surface of the carbon nanomaterial in situ, the modified carbon material is obtained by the following steps: dispersing the functionalized carbon nanomaterial in a water-soluble raw material solution to form a reaction solution with a concentration of 5-10 g / L, adding an alkaline precipitant dropwise under stirring until the final pH value is greater than 8, transferring it to a high-pressure reactor lined with polytetrafluoroethylene and carrying out a hydrothermal reaction at 120-200℃ for 6-24 h, cooling, washing, drying, and then calcining at 300-800℃ for 1-5 h to obtain the modified carbon material with the structure of nano-conductive metal oxide attached to the surface of the carbon nanomaterial in situ; The water-soluble raw material solution is one of the following: a mixed solution of tin tetrachloride and antimony trichloride prepared in an atomic ratio of Sn:Sb=90:10-95:5; a mixed solution of indium trichloride and tin tetrachloride prepared in an atomic ratio of In:Sn=90:10; or a mixed solution of zinc acetate and aluminum nitrate or aluminum isopropoxide prepared in an atomic ratio of Zn:Al=95:5-98:
2. The alkaline precipitant is a 0.5-2 mol / L sodium hydroxide solution or an ammonia solution; when in-situ generation of nano-indium tin oxide is required, the endpoint pH is 8.5-9.5; when in-situ generation of nano-tin antimony oxide is required, the endpoint pH is 8.0-9.0; when in-situ generation of nano-aluminum-doped zinc oxide is required, the endpoint pH is 8.0-9.
0.
5. The modified polyaryletherketone composite material with high dimensional stability and high conductivity according to claim 1, characterized in that, The PAEK resin is selected from one or more of polyetheretherketone, polyetherketone, polyetherketoneketone, polyetheretherketoneketone, and polyetherketoneetherketoneketone.
6. A method for preparing a modified polyaryletherketone composite material with high dimensional stability and high conductivity, applicable to the preparation of the composite material according to any one of claims 1-5, comprising the following steps: mixing a modified carbon material having at least one dimension, an interface modifier, and PAEK resin according to a formula, followed by melt blending to obtain granules, and then crystallizing them. The modified carbon material is composed of a carbon nanomaterial with an in-situ attached nano-conductive material on its surface, wherein the nano-conductive material is a nano-conductive metal or a nano-conductive metal oxide. The melt blending is achieved using a twin-screw extruder with the following parameters: melt blending temperature 350-400℃, vacuum devouring pressure less than 10kPa; The crystallization molding process involves placing the obtained granules in a molding die and molding them under pressure of at least 8 MPa and a heating temperature of 380-400°C for 10-40 minutes, followed by cooling at a rate of less than 3°C / min.
Citation Information
Patent Citations
Long fiber reinforced polyether-ether-ketone master batch, preparation method thereof and polyaryletherketone composite material