Preparation method and application of solvent-free salt mist resistant 10000-cps elastic glue
By optimizing the anti-corrosion powder and prepolymer through solvent-free formulation and modification, a dense and stable anti-corrosion protective layer is formed, which solves the problems of solvent pollution, insufficient adhesion and poor salt spray resistance of existing anti-corrosion elastic adhesives, and realizes the multi-field application of high-performance and environmentally friendly anti-corrosion materials.
Patent Information
- Application Number
- CN202511508310.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2045-10-22
AI Technical Summary
Existing anti-corrosion elastic adhesive products suffer from problems such as solvent evaporation pollution, insufficient adhesion, poor salt spray resistance, insufficient elasticity, inconvenient construction, and poor water resistance, failing to meet the demand for high-performance and environmentally friendly anti-corrosion materials.
Using a solvent-free formulation, through specific modification treatment and compounding with coupling agents, the components of anti-corrosion powder and prepolymer are optimized. Combined with corrosion inhibitors, a dense and stable anti-corrosion protective layer is formed, which is suitable for a variety of substrates, reduces construction viscosity, and enhances the density and anti-swelling ability of the film.
It achieves breakthroughs in multiple dimensions of performance, including environmental friendliness, adhesion, salt spray resistance, elasticity, storage stability, and workability. It is adaptable to various substrates, extends the protection period, reduces energy consumption, and improves ease of operation and anti-corrosion effect.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion elastic adhesive technology, specifically to a method for preparing and applying a solvent-free, salt spray resistant, universally adhesive anti-corrosion elastic adhesive. Background Technology
[0002] In fields such as industrial equipment corrosion protection, marine engineering protection, and waterproofing and corrosion protection of building concrete, anti-corrosion elastic adhesives are key materials for ensuring the long-term stable use of substrates. They must simultaneously meet multiple requirements, including environmental friendliness, high adhesion, salt spray resistance, excellent elasticity, stable storage, and convenient application. However, existing anti-corrosion elastic adhesive products still have several technical drawbacks: some products are solvent-based systems, which can generate volatile organic compounds during application and use due to solvent evaporation, causing environmental pollution and potentially posing a threat to the health of operators; regarding adhesion, existing products are difficult to adapt to multiple substrates such as metals, concrete, and fiberglass, especially showing weak adhesion to non-metallic substrates, easily leading to delamination and affecting the anti-corrosion effect; insufficient salt spray resistance means that in marine or high-salt-spray industrial environments, the adhesive film is easily corroded by salt spray, leading to substrate corrosion and shortening the protection period. The existing anti-corrosion elastic adhesives suffer from several drawbacks. Their elastic properties are ill-suited for wide-temperature applications, easily becoming brittle at low temperatures and softening at high temperatures, failing to cope with stresses caused by thermal expansion and contraction or vibration of the substrate. Furthermore, the poor dispersibility of the anti-corrosion powder in some products leads to sedimentation during storage, resulting in uneven product performance and affecting application effectiveness. High application viscosity makes coating inconvenient, requiring additional high-temperature viscosity reduction treatment, increasing energy consumption and potentially damaging the substrate. Poor long-term water resistance means the adhesive film easily absorbs water and swells in humid or underwater environments, increasing weight loss and reducing anti-corrosion lifespan. These issues severely limit the application range and effectiveness of existing anti-corrosion elastic adhesives, failing to meet the current demand for high-performance, environmentally friendly anti-corrosion materials across various fields. Summary of the Invention
[0003] The purpose of this invention is to address the shortcomings of existing technologies by proposing a method for preparing and applying a solvent-free, salt spray-resistant, universally adhesive, and corrosion-resistant elastic adhesive.
[0004] To achieve the above objectives, the present invention provides the following technical solutions. A solvent-free, salt spray resistant, highly adhesive, corrosion-resistant elastic adhesive is composed of the following components: HTPB, MDI, corrosion-resistant powder, carbon black, plasticizer, coupling agent KH550, and catalyst DBTDL; the corrosion-resistant powder is ordinary zinc powder or nano zinc-aluminum alloy powder, and the plasticizer is DOP.
[0005] A method for preparing a solvent-free, salt spray-resistant, highly adhesive, and corrosion-resistant elastic adhesive includes the following steps: (1) Add HTPB, anti-corrosion powder, carbon black and plasticizer DOP to the high-speed disperser, disperse at the preset speed for the preset time, and then heat to the preset temperature and keep warm to remove air bubbles. (2) Cool down to the preset temperature, add coupling agent KH550 and catalyst DBTDL, and stir evenly; (3) Slowly add MDI, control the dripping speed, and stir at a preset speed for a preset time after the dripping is completed to obtain a solvent-free salt spray resistant, universally adhesive, corrosion-resistant elastic adhesive; the corrosion-resistant powder is ordinary zinc powder or nano zinc-aluminum alloy powder.
[0006] Preferably, the HTPB is KH550 modified HTPB; the preparation method of the KH550 modified HTPB is as follows: take HTPB, KH550 and DBTDL, react them at a preset temperature for a preset time, detect the Si-OC characteristic peak by infrared detection, and then cool them to a preset temperature for later use.
[0007] Preferably, the anti-corrosion powder is nano-zinc-aluminum alloy powder, and also includes corrosion inhibitor BTA; after the nano-zinc-aluminum alloy powder and BTA are mixed and ground for a preset time, it is then mixed with HTPB, carbon black and plasticizer DOP.
[0008] Preferably, it also includes polyether polyol; in step (3), the MDI is an MDI-polyether prepolymer, and the preparation method of the MDI-polyether prepolymer is: take MDI and polyether polyol, react them at a preset temperature for a preset time, and control the NCO content.
[0009] Preferably, it also includes cashew phenol modified epoxy resin and coupling agent KH560; before step (1), KH550 modified HTPB and cashew phenol modified epoxy resin are stirred at a preset temperature for a preset time to form an interpenetrating network matrix, and then the KH550 and KH560 compound system is added. After heat preservation for a preset time, the mixing in step (1) is carried out.
[0010] Preferably, the polyether polyol is a compound of PTMG and PCL; the MDI-polyether prepolymer is an MDI-PTMG-PCL prepolymer, which is prepared by taking MDI, PTMG, and PCL, reacting them at a preset temperature for a preset time, and controlling the NCO content.
[0011] Preferably, the nano zinc-aluminum alloy powder is MPEG modified nano zinc-aluminum alloy powder; the preparation method of the MPEG modified nano zinc-aluminum alloy powder is as follows: take nano zinc-aluminum alloy powder and MPEG, and process them in a high-speed disperser at a preset speed for a preset time; it also includes dispersant BYK-052, which is added to the high-speed disperser together with HTPB, modified nano zinc-aluminum alloy powder, carbon black and plasticizer DOP in step (1).
[0012] Preferably, the solvent-free, salt spray-resistant, universally adhesive, and corrosion-resistant elastic adhesive is coated onto the surface of a substrate and cured to form an adhesive film; the substrate is a Q235 steel sheet, a C30 concrete block, or a fiberglass substrate.
[0013] Preferably, the substrate is pretreated before coating: Q235 steel sheets are sandblasted to remove rust and then wiped with ethanol; C30 concrete test blocks are sandblasted to expose the aggregate and then wiped with ethanol; fiberglass substrates are sanded to roughness and then wiped with ethanol; the curing conditions are room temperature curing for a preset time, and the resulting film thickness is a preset thickness.
[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention adopts a solvent-free formulation design, which avoids the volatilization of volatile organic compounds in solvent-based products. It not only meets the requirements of current environmental protection regulations, but also reduces environmental pollution and potential threats to the health of operators. It can be widely used in scenarios with high environmental protection requirements.
[0015] 2. By introducing a specific modification treatment and coupling agent compound system, this invention not only significantly enhances the adhesion to metal substrates, but also effectively improves the bonding force to non-metallic substrates such as concrete and fiberglass, achieving compatibility with multiple substrates, avoiding delamination during use, ensuring long-term anti-corrosion effect, and expanding the application scenarios of the product.
[0016] 3. This invention constructs a dense and stable anti-corrosion protective layer through the optimized selection of anti-corrosion powder and the synergistic effect of corrosion inhibitors. This layer can effectively hinder salt spray erosion, significantly extend the protection period in marine or high-salt-spray industrial environments, and improve the service life of the substrate.
[0017] 4. Through the compound design of prepolymer components, this invention achieves a wide temperature range elastic balance that is not easily brittle at low temperatures and not easily softened at high temperatures. It can effectively cope with the thermal expansion and contraction or vibration stress of the substrate caused by temperature changes, avoid film cracking, and ensure protective stability.
[0018] 5. This invention solves the problem of easy agglomeration and sedimentation of anti-corrosion powder through the synergistic effect of powder modification and dispersant, reduces the generation of bottom sediment during storage, ensures uniform product performance, extends the product storage period, and reduces usage costs.
[0019] 6. This invention significantly reduces the application viscosity of the product through component optimization, eliminating the need for additional high-temperature viscosity reduction treatment. This not only reduces application energy consumption but also avoids potential damage to the substrate caused by high temperatures. It is compatible with conventional application methods such as brushing and roller coating, improving ease of operation and application efficiency.
[0020] 7. This invention enhances the density and anti-swelling ability of the film through the synergistic effect of multiple components, reduces the erosion of the film by water in humid or underwater environments, reduces the weight loss rate after long-term water immersion, and ensures long-term anti-corrosion effect in humid or underwater scenarios.
[0021] In summary, the product of this invention has achieved breakthroughs in multiple dimensions in terms of environmental protection, adhesion, salt spray resistance, elasticity, storage stability, workability, and water resistance. The various properties are synergistically balanced, which can meet the high-performance requirements of many fields such as industrial equipment corrosion protection, marine engineering protection, and waterproofing and corrosion protection of building concrete. It has significant technological advancement and practical application value. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Example 1: Component dosage (parts by weight): HTPB90, MDI9, ordinary zinc powder 25, ordinary carbon black 12, DOP6, KH5502, DBTDL0.4; ordinary zinc powder particle size 5μm, ordinary carbon black unmodified; Preparation steps: Add HTPB, ordinary zinc powder, ordinary carbon black and DOP to a high-speed disperser, disperse at 3000 r / min for 30 min, heat to 60℃ and keep warm for 10 min to remove air bubbles; Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; Slowly add MDI at a rate of 5 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film.
[0024] Example 2: Component dosage (parts by weight): HTPB100, MDI10, ordinary zinc powder 30, ordinary carbon black 15, DOP8, KH5503, DBTDL0.5; ordinary zinc powder particle size 5μm, ordinary carbon black unmodified; Preparation steps: Same as the preparation steps in Example 1 above, only the amount of ingredients is adjusted according to Example 2.
[0025] Example 3: Component dosage (parts by weight): HTPB110, MDI11, ordinary zinc powder 35, ordinary carbon black 18, DOP10, KH5504, DBTDL0.6; ordinary zinc powder particle size 5μm, ordinary carbon black unmodified; Preparation steps: Same as the preparation steps in Example 1 above, only the amount of ingredients is adjusted according to Example 3.
[0026] Example 4: Composition and dosage (parts by weight): HTPB90, MDI9, nano zinc-aluminum alloy powder 20, BTA1, ordinary carbon black 12, DOP6, KH5502, DBTDL0.4; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%; Preparation steps: First, mix and grind nano zinc-aluminum alloy powder with BTA for 10 min to achieve particle size uniformity. Then, add HTPB, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, and DOP to a high-speed disperser. The ordinary carbon black is unmodified. Disperse at 3000 r / min for 30 min, heat to 60℃ and keep warm for 10 min to remove air bubbles. Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; Slowly add MDI at a rate of 5 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film.
[0027] Example 5: Composition and dosage (parts by weight): HTPB100, MDI10, nano zinc-aluminum alloy powder25, BTA2, ordinary carbon black15, DOP8, KH5503, DBTDL0.5; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%. Preparation steps: The preparation steps are the same as in Example 4 above, except that the amount of components is adjusted according to Example 5. The particle size and Al content of the nano zinc-aluminum alloy powder and the state of ordinary carbon black remain unchanged.
[0028] Example 6: Composition and dosage (parts by weight): HTPB110, MDI11, nano zinc-aluminum alloy powder 30, BTA3, ordinary carbon black 18, DOP10, KH5504, DBTDL0.6; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%; The preparation steps are the same as in Example 4 above, except that the amount of components is adjusted according to Example 6. The particle size and Al content of the nano zinc-aluminum alloy powder and the state of ordinary carbon black remain unchanged.
[0029] Example 7: Composition and dosage (parts by weight): KH550 modified HTPB90, MDI9, nano zinc-aluminum alloy powder 20, BTA1, ordinary carbon black 12, DOP6, KH5502, DBTDL0.4; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 90 parts by weight of HTPB, 4 parts by weight of KH550, and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. Next, the nano zinc-aluminum alloy powder is mixed and ground with BTA for 10 minutes to achieve particle size uniformity. The prepared KH550 modified HTPB, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, and DOP are added to the high-speed disperser. The ordinary carbon black is not modified. The mixture is dispersed at 3000 r / min for 30 minutes and heated to 60℃ and kept at that temperature for 10 minutes to remove air bubbles. Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; Slowly add MDI at a rate of 5 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film.
[0030] Example 8: Composition and dosage (parts by weight): KH550 modified HTPB100, MDI10, nano zinc-aluminum alloy powder25, BTA2, ordinary carbon black15, DOP8, KH5503, DBTDL0.5; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%; Preparation steps: The preparation steps are the same as in Example 7 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 100 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL; the overall component amounts are adjusted according to Example 8, and the nano zinc-aluminum alloy powder and ordinary carbon black remain unchanged.
[0031] Example 9: Composition and dosage (parts by weight): KH550 modified HTPB110, MDI11, nano zinc-aluminum alloy powder 30, BTA3, ordinary carbon black 18, DOP10, KH5504, DBTDL0.6; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%; Preparation steps: The preparation steps are the same as in Example 7 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 110 parts by weight of HTPB, 6 parts by weight of KH550, and 0.4 parts by weight of DBTDL; the overall component amounts are adjusted according to Example 9, and the nano zinc-aluminum alloy powder and ordinary carbon black remain unchanged.
[0032] Example 10: Component dosage (parts by weight): KH550 modified HTPB90, MDI10, polyether polyol 1, nano zinc-aluminum alloy powder 20, BTA1, ordinary carbon black 12, DOP6, KH5502, DBTDL0.4; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, and the polyether polyol has a number average molecular weight of 800; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 90 parts by weight of HTPB, 4 parts by weight of KH550, and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-polyether prepolymer was prepared by taking 10 parts by weight of MDI and 1 part by weight of polyether polyol, reacting at 80℃ for 1 hour, with an NCO content of 20%. Nano zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The prepared KH550 modified HTPB, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, and DOP were added to a high-speed disperser. The ordinary carbon black was not modified. The mixture was dispersed at 3000 r / min for 30 min and heated to 60℃ and held for 10 min to remove air bubbles. Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; The prepared MDI-polyether prepolymer was slowly added dropwise at a rate of 7 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free adhesive. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film.
[0033] Example 11: Component dosage (parts by weight): KH550 modified HTPB100, MDI12, polyether polyol 2, nano zinc-aluminum alloy powder 25, BTA2, ordinary carbon black 15, DOP8, KH5503, DBTDL0.5; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, and the polyether polyol has a number average molecular weight of 1000; Preparation steps: The preparation steps are the same as in Example 10 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 100 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL; when preparing MDI-polyether prepolymer, the raw material amounts are 12 parts by weight of MDI and 2 parts by weight of polyether polyol; the dropping rate is controlled at 8 mL / min when adding the prepolymer; the overall component amounts are adjusted according to Example 11.
[0034] Example 12: Component dosage (parts by weight): KH550 modified HTPB110, MDI14, polyether polyol 3, nano zinc-aluminum alloy powder 30, BTA3, ordinary carbon black 18, DOP10, KH5504, DBTDL0.6; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, and the polyether polyol has a number average molecular weight of 1200; Preparation steps: The preparation steps are the same as in Example 10 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 110 parts by weight of HTPB, 6 parts by weight of KH550, and 0.4 parts by weight of DBTDL; when preparing MDI-polyether prepolymer, the raw material amounts are 14 parts by weight of MDI and 3 parts by weight of polyether polyol; the dropping rate is controlled at 9 mL / min when adding the prepolymer; 4. The overall component amounts are adjusted according to Example 12.
[0035] Example 13: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 15, MDI 10, polyether polyol 1, nano zinc-aluminum alloy powder 20, BTA 1, ordinary carbon black 12, DOP 6, KH550 2, KH560 1, DBTDL 0.4; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, the polyether polyol has a number average molecular weight of 800, and the cashew nut phenol modified epoxy resin has an epoxy value of 0.20eq / 100g; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 80 parts by weight of HTPB, 4 parts by weight of KH550, and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-polyether prepolymer was prepared by taking 10 parts by weight of MDI and 1 part by weight of polyether polyol, reacting at 80℃ for 1 hour, with an NCO content of 20%. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. Nano zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above interpenetrating network matrix, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, and DOP were added to a high-speed disperser. The ordinary carbon black was not modified. The mixture was dispersed at 3000 r / min for 30 min and heated to 60℃ for 10 min to remove air bubbles. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-polyether prepolymer was slowly added dropwise at a rate of 7 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free adhesive. The coating substrates were Q235 steel sheets, C30 concrete test blocks, and fiberglass substrates. The pretreatment method for Q235 steel sheets was sandblasting to remove rust to Sa2.5 grade and then wiping with ethanol. The pretreatment method for C30 concrete test blocks was sandblasting the surface to expose the aggregate and then wiping with ethanol. The pretreatment method for fiberglass substrates was sanding with sandpaper to roughness and then wiping with ethanol. The coating was cured at room temperature for 24 hours to form a 0.5mm thick film.
[0036] Example 14: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 20, MDI 12, polyether polyol 2, nano zinc-aluminum alloy powder 25, BTA 2, ordinary carbon black 15, DOP 8, KH550 3, KH560 2, DBTDL 0.5; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, the polyether polyol has a number average molecular weight of 1000, and the cashew nut phenol modified epoxy resin has an epoxy value of 0.22eq / 100g; Preparation steps: The preparation steps are the same as in Example 13 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 80 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL; when preparing MDI-polyether prepolymer, the raw material amounts are 12 parts by weight of MDI and 2 parts by weight of polyether polyol; the epoxy value of cashew phenol modified epoxy resin is adjusted to 0.22 eq / 100g; the dropping rate is controlled at 8 mL / min when adding the prepolymer; the overall component amounts are adjusted according to Example 14.
[0037] Example 15: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 25, MDI 14, polyether polyol 3, nano zinc-aluminum alloy powder 30, BTA 3, ordinary carbon black 18, DOP 10, KH550 4, KH560 3, DBTDL 0.6; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, polyether polyol with a number-average molecular weight of 1200, and cashew nut phenol modified epoxy resin with an epoxy value of 0.24eq / 100g; Preparation steps: The preparation steps are the same as in Example 13 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 80 parts by weight of HTPB, 6 parts by weight of KH550, and 0.4 parts by weight of DBTDL; when preparing MDI-polyether prepolymer, the raw material amounts are 14 parts by weight of MDI and 3 parts by weight of polyether polyol; the epoxy value of cashew phenol modified epoxy resin is adjusted to 0.24 eq / 100g; the dropping rate is controlled at 9 mL / min when adding the prepolymer; the overall component amounts are adjusted according to Example 15.
[0038] Example 16: Component dosage (parts by weight): KH550 modified HTPB80, cashew phenol modified epoxy resin 15, MDI 9, PTMG 4, PCL 2, nano zinc-aluminum alloy powder 20, BTA 1, ordinary carbon black 12, DOP 6, KH550 2, KH560 1, DBTDL 0.4; nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, PTMG has a number average molecular weight of 1800, PCL has a number average molecular weight of 1300, and cashew phenol modified epoxy resin has an epoxy value of 0.20eq / 100g; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 80 parts by weight of HTPB, 4 parts by weight of KH550, and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-PTMG-PCL prepolymer was prepared by taking 9 parts by weight of MDI, 4 parts by weight of PTMG, and 2 parts by weight of PCL, reacting at 75℃ for 1.5 h, with an NCO content of 18%. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. Nano zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above interpenetrating network matrix, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, and DOP were added to a high-speed disperser. The ordinary carbon black was not modified. The mixture was dispersed at 3000 r / min for 30 min and heated to 60℃ for 10 min to remove air bubbles. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-PTMG-PCL prepolymer was slowly added dropwise at a rate of 7 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free gel. The coating substrates were Q235 steel sheets, C30 concrete test blocks, and fiberglass substrates. The pretreatment method for Q235 steel sheets was sandblasting to remove rust to Sa2.5 grade and then wiping with ethanol. The pretreatment method for C30 concrete test blocks was sandblasting the surface to expose the aggregate and then wiping with ethanol. The pretreatment method for fiberglass substrates was sanding with sandpaper to roughness and then wiping with ethanol. The coating was cured at room temperature for 24 hours to form a 0.5mm thick film.
[0039] Example 17: Component dosage (parts by weight): KH550 modified HTPB80, cashew phenol modified epoxy resin 20, MDI 10, PTMG 5, PCL 3, nano zinc-aluminum alloy powder 25, BTA 2, ordinary carbon black 15, DOP 8, KH550 3, KH560 2, DBTDL 0.5; nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, PTMG has a number average molecular weight of 2000, PCL has a number average molecular weight of 1500, and cashew phenol modified epoxy resin has an epoxy value of 0.22eq / 100g; Preparation steps: The preparation steps are the same as in Example 16 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 80 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL; when preparing MDI-PTMG-PCL prepolymer, the raw material amounts are 10 parts by weight of MDI, 5 parts by weight of PTMG, and 3 parts by weight of PCL; the epoxy value of the cashew phenol modified epoxy resin is adjusted to 0.22 eq / 100g; the dropping rate is controlled at 8 mL / min when adding the prepolymer; the overall component amounts are adjusted according to Example 17.
[0040] Example 18: Component dosage (parts by weight): KH550 modified HTPB80, cashew phenol modified epoxy resin 25, MDI 11, PTMG 6, PCL 4, nano zinc-aluminum alloy powder 30, BTA 3, ordinary carbon black 18, DOP 10, KH550 4, KH560 3, DBTDL 0.6; nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, PTMG has a number average molecular weight of 2200, PCL has a number average molecular weight of 1700, and cashew phenol modified epoxy resin has an epoxy value of 0.24eq / 100g; Preparation steps: The preparation steps are the same as in Example 16 above, except for the following adjustments: When preparing KH550 modified HTPB, the raw material amounts are 80 parts by weight of HTPB, 6 parts by weight of KH550, and 0.4 parts by weight of DBTDL; when preparing MDI-PTMG-PCL prepolymer, the raw material amounts are 11 parts by weight of MDI, 6 parts by weight of PTMG, and 4 parts by weight of PCL; the epoxy value of the cashew phenol modified epoxy resin is adjusted to 0.24 eq / 100g; the dropping rate is controlled at 9 mL / min when adding the prepolymer; the overall component amounts are adjusted according to Example 18.
[0041] Example 19: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 15, MDI 9, PTMG 4, PCL 2, nano zinc-aluminum alloy powder 20, MPEG 0.8, BTA 1, ordinary carbon black 12, DOP 6, KH550 2, KH560 1, BYK-052 0.2, DBTDL 0.4; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, PTMG with a number average molecular weight of 1800, PCL with a number average molecular weight of 1300, MPEG with a number average molecular weight of 1800, and cashew nut phenol modified epoxy resin with an epoxy value of 0.20eq / 100g; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 80 parts by weight of HTPB, 4 parts by weight of KH550, and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-PTMG-PCL prepolymer was prepared by taking 9 parts by weight of MDI, 4 parts by weight of PTMG, and 2 parts by weight of PCL, reacting at 75℃ for 1.5 h, with an NCO content of 18%. Modified nano-zinc-aluminum alloy powder was prepared by taking 20 parts by weight of nano-zinc-aluminum alloy powder and 0.8 parts by weight of MPEG, and processing them in a high-speed disperser at 5000 r / min for 20 min. MPEG was grafted onto the powder surface to provide steric hindrance. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. The modified nano-zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above-mentioned interpenetrating network matrix, the ground nano-zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, DOP, and BYK-052 were added to a high-speed disperser. The ordinary carbon black was not modified. The mixture was dispersed at 3000 r / min for 15 min. The viscosity at 25℃ dropped to 6800 mPa·s without the need for high-temperature viscosity reduction. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-PTMG-PCL prepolymer was slowly added dropwise at a rate of 7 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free gel. The coating substrates were Q235 steel sheets, C30 concrete test blocks, and fiberglass substrates. The pretreatment method for Q235 steel sheets was sandblasting to remove rust to Sa2.5 grade and then wiping with ethanol. The pretreatment method for C30 concrete test blocks was sandblasting the surface to expose the aggregate and then wiping with ethanol. The pretreatment method for fiberglass substrates was sanding with sandpaper to roughness and then wiping with ethanol. The coating was cured at room temperature for 24 hours to form a 0.5mm thick film.
[0042] Example 20: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 20, MDI 10, PTMG 5, PCL 3, nano zinc-aluminum alloy powder 25, MPEG 1, BTA 2, ordinary carbon black 15, DOP 8, KH550 3, KH560 2, BYK-052 0.3, DBTDL 0.5; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, PTMG with a number average molecular weight of 2000, PCL with a number average molecular weight of 1500, MPEG with a number average molecular weight of 2000, and cashew nut phenol modified epoxy resin with an epoxy value of 0.22eq / 100g; Preparation steps: First, KH550 modified HTPB was prepared. The preparation method was to take 80 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL, react at 80℃ for 3 hours, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-PTMG-PCL prepolymer was prepared by taking 10 parts by weight of MDI, 5 parts by weight of PTMG, and 3 parts by weight of PCL, reacting at 75℃ for 1.5 h, with an NCO content of 18%. Modified nano-zinc-aluminum alloy powder was prepared by taking 25 parts by weight of nano-zinc-aluminum alloy powder and MPEG1 by weight, and processing them in a high-speed disperser at 5000 r / min for 20 min. MPEG was grafted onto the powder surface to provide steric hindrance. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. The modified nano-zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above-mentioned interpenetrating network matrix, the ground nano-zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, DOP, and BYK-052 were added to a high-speed disperser. The ordinary carbon black was not modified. The mixture was dispersed at 3000 r / min for 15 min. The viscosity at 25℃ dropped to 6500 mPa・s without the need for high-temperature viscosity reduction. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-PTMG-PCL prepolymer was slowly added dropwise at a rate of 8 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free gel. The coating substrates were Q235 steel sheets, C30 concrete test blocks, and fiberglass substrates. The pretreatment method for Q235 steel sheets was sandblasting to remove rust to Sa2.5 grade and then wiping with ethanol. The pretreatment method for C30 concrete test blocks was sandblasting the surface to expose the aggregate and then wiping with ethanol. The pretreatment method for fiberglass substrates was sanding with sandpaper to roughness and then wiping with ethanol. The coating was cured at room temperature for 24 hours to form a 0.5mm thick film.
[0043] Example 21: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 25, MDI 11, PTMG 6, PCL 4, nano zinc-aluminum alloy powder 30, MPEG 1.2, BTA 3, ordinary carbon black 18, DOP 10, KH550 4, KH560 3, BYK-052 0.4, DBTDL 0.6; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, PTMG with a number average molecular weight of 2200, PCL with a number average molecular weight of 1700, MPEG with a number average molecular weight of 2200, and cashew nut phenol modified epoxy resin with an epoxy value of 0.24eq / 100g; Preparation steps: First, KH550 modified HTPB was prepared. The preparation method was to take 80 parts by weight of HTPB, 6 parts by weight of KH550, and 0.4 parts by weight of DBTDL, react at 80℃ for 3 hours, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-PTMG-PCL prepolymer was prepared by taking 11 parts by weight of MDI, 6 parts by weight of PTMG, and 4 parts by weight of PCL, reacting at 75℃ for 1.5 h, with an NCO content of 18%. Modified nano-zinc-aluminum alloy powder was prepared by taking 30 parts by weight of nano-zinc-aluminum alloy powder and 1.2 parts by weight of MPEG, and processing them in a high-speed disperser at 5000 r / min for 20 min. MPEG was grafted onto the powder surface to provide steric hindrance. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. The modified nano zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above interpenetrating network matrix, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, DOP, and BYK-052 were added to a high-speed disperser. The ordinary carbon black was not modified. The mixture was dispersed at 3000 r / min for 15 min. The viscosity at 25℃ dropped to 6200 mPa・s without the need for high-temperature viscosity reduction. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-PTMG-PCL prepolymer was slowly added dropwise at a rate of 9 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free gel. The coating substrates were Q235 steel sheets, C30 concrete test blocks, and fiberglass substrates. The pretreatment method for Q235 steel sheets was sandblasting to remove rust to Sa2.5 grade and then wiping with ethanol. The pretreatment method for C30 concrete test blocks was sandblasting the surface to expose the aggregate and then wiping with ethanol. The pretreatment method for fiberglass substrates was sanding with sandpaper to roughness and then wiping with ethanol. The coating was cured at room temperature for 24 hours to form a 0.5mm thick film.
[0044] Comparative Example 1: Component dosage (parts by weight): HTPB100, MDI10, ordinary zinc powder30, ordinary carbon black15, DOP8, DBTDL0.5; ordinary zinc powder particle size 5μm, ordinary carbon black unmodified; Preparation steps: Add HTPB, ordinary zinc powder, ordinary carbon black and DOP to a high-speed disperser, disperse at 3000 r / min for 30 min, heat to 60℃ and keep warm for 10 min to remove air bubbles; Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; Slowly add MDI at a rate of 5 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film. The purpose of the comparison was to verify the effect of KH550 on improving adhesion.
[0045] Comparative Example 2: Component dosage (parts by weight): HTPB100, MDI10, ordinary zinc powder30, ordinary carbon black15, DOP8, KH5503, DBTDL0.5; ordinary zinc powder particle size 5μm, ordinary carbon black unmodified; Preparation steps: Add HTPB, ordinary zinc powder, ordinary carbon black and DOP to a high-speed disperser, disperse at 3000 r / min for 30 min, heat to 60℃ and keep warm for 10 min to remove air bubbles; Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; Slowly add MDI at a rate of 5 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film. The purpose of the comparison was to verify the effect of nano zinc-aluminum alloy powder + BTA on improving salt spray resistance.
[0046] Comparative Example 3: Component dosage (parts by weight): ordinary HTPB100, MDI10, nano zinc-aluminum alloy powder25, BTA2, ordinary carbon black15, DOP8, KH5503, DBTDL0.5; the nano zinc-aluminum alloy powder has a particle size of 50nm and an Al content of 30%, and the ordinary carbon black is unmodified. Preparation steps: First, mix and grind nano zinc-aluminum alloy powder with BTA for 10 min to achieve particle size uniformity. Then, add ordinary HTPB, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black and DOP to a high-speed disperser and disperse at 3000 r / min for 30 min. Heat to 60℃ and keep warm for 10 min to remove air bubbles. Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; Slowly add MDI at a rate of 5 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film. Objective: To verify the effect of KH550-modified HTPB on improving adhesion.
[0047] Comparative Example 4: Component dosage (parts by weight): KH550 modified HTPB100, MDI12, nano zinc-aluminum alloy powder 25, BTA2, ordinary carbon black 15, DOP8, KH5503, DBTDL0.5; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, and ordinary carbon black without modification. Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 100 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. Next, the nano zinc-aluminum alloy powder is mixed and ground with BTA for 10 minutes to achieve particle size uniformity. The prepared KH550 modified HTPB, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black and DOP are added to the high-speed disperser and dispersed at 3000 r / min for 30 minutes. The temperature is raised to 60℃ and kept at 10 minutes to remove air bubbles. Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; Slowly add MDI at a rate of 8 mL / min, and stir at 2000 r / min for 25 min after the addition is complete to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The Q235 steel sheet substrate is pretreated by sandblasting to remove rust to Sa2.5 grade, then wiped with ethanol, and cured at room temperature for 24 hours to form a 0.5mm thick film. The purpose of the comparison was to verify the effect of MDI-polyether prepolymer on improving elasticity.
[0048] Comparative Example 5: Component dosage (parts by weight): KH550 modified HTPB100, MDI12, polyether polyol 2, nano zinc-aluminum alloy powder 25, BTA2, ordinary carbon black 15, DOP8, KH5503, DBTDL0.5; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, polyether polyol with a number average molecular weight of 1000, and ordinary carbon black unmodified; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 100 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-polyether prepolymer was prepared by taking 12 parts by weight of MDI and 2 parts by weight of polyether polyol, reacting at 80℃ for 1 hour, with an NCO content of 20%. Add the prepared KH550 modified HTPB, nano zinc aluminum alloy powder and BTA mixture, ordinary carbon black and DOP to the high-speed disperser. Disperse at 3000 r / min for 30 min, heat to 60℃ and keep warm for 10 min to remove air bubbles. Cool to 40℃, add KH550 and DBTDL, and stir at 1500r / min for 15min; The prepared MDI-polyether prepolymer was slowly added dropwise at a rate of 8 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free adhesive. The coating was applied to C30 concrete test blocks. The pretreatment method for C30 concrete test blocks was to sandblast the surface until the aggregate was exposed, then wipe it with ethanol, and cure it at room temperature for 24 hours to form a 0.5 mm thick film. The purpose of the comparison was to verify the effect of cashew phenol-modified epoxy resin + KH560 on improving the adhesion of non-metallic substrates.
[0049] Comparative Example 6: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut phenol modified epoxy resin 20, MDI 12, ordinary polyether polyol 8, nano zinc-aluminum alloy powder 25, BTA 2, ordinary carbon black 15, DOP 8, KH550 3, KH560 2, DBTDL 0.5; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, ordinary polyether polyol with a number average molecular weight of 1000, cashew nut phenol modified epoxy resin with an epoxy value of 0.22eq / 100g, and ordinary carbon black without modification; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 80 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-common polyether prepolymer was prepared by taking 12 parts by weight of MDI and 8 parts by weight of common polyether polyol, reacting at 75℃ for 1.5 h, with an NCO content of 18%. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. Nano-zinc-aluminum alloy powder is mixed and ground with BTA for 10 min to achieve particle size uniformity. The above-mentioned interpenetrating network matrix, the ground nano-zinc-aluminum alloy powder and BTA mixture, ordinary carbon black and DOP are added to a high-speed disperser and dispersed at 3000 r / min for 30 min. The temperature is raised to 60℃ and held for 10 min to remove air bubbles. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-common polyether prepolymer was slowly added dropwise at a rate of 8 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free adhesive. The coating is applied to Q235 steel sheets. The pretreatment of Q235 steel sheets is sandblasting to remove rust to Sa2.5 grade, followed by wiping with ethanol and curing at room temperature for 24 hours to form a 0.5mm thick film. The purpose of the comparison was to verify the effect of PTMG+PCL compound polyether on improving elasticity over a wide temperature range.
[0050] Comparative Example 7: Component dosage (parts by weight): KH550 modified HTPB80, cashew nut shell modified epoxy resin 20, MDI 10, PTMG 5, PCL 3, nano zinc-aluminum alloy powder 25, stearic acid 1, BTA 2, ordinary carbon black 15, DOP 8, KH550 3, KH560 2, DBTDL 0.5; nano zinc-aluminum alloy powder with a particle size of 50nm and an Al content of 30%, PTMG with a number average molecular weight of 2000, PCL with a number average molecular weight of 1500, cashew nut shell modified epoxy resin with an epoxy value of 0.22eq / 100g, and ordinary carbon black without modification; Preparation steps: First, prepare KH550 modified HTPB. The preparation method is to take 80 parts by weight of HTPB, 5 parts by weight of KH550, and 0.3 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. MDI-PTMG-PCL prepolymer was prepared by taking 10 parts by weight of MDI, 5 parts by weight of PTMG, and 3 parts by weight of PCL, reacting at 75℃ for 1.5 h, with an NCO content of 18%. Modified nano-zinc-aluminum alloy powder was prepared by taking 25 parts by weight of nano-zinc-aluminum alloy powder and 1 part by weight of stearic acid, and treating them in a high-speed disperser at 5000 r / min for 20 min. Modified HTPB and cashew phenol modified epoxy resin were stirred at 60℃ for 20 min to form an interpenetrating network matrix, and then KH550 and KH560 compound system were added and kept at 40℃ for 10 min. The modified nano zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above interpenetrating network matrix, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black and DOP were added to a high-speed disperser and dispersed at 3000 r / min for 15 min. The viscosity at 25℃ was 9200 mPa·s, which required high temperature viscosity reduction. Cool to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; The prepared MDI-PTMG-PCL prepolymer was slowly added dropwise at a rate of 8 mL / min. After the addition was complete, the mixture was stirred at 2000 r / min for 25 min to obtain a solvent-free gel. The coating is applied to Q235 steel sheets. The pretreatment of Q235 steel sheets is sandblasting to remove rust to Sa2.5 grade, followed by wiping with ethanol and curing at room temperature for 24 hours to form a 0.5mm thick film. The purpose of the comparison was to verify the effect of MPEG+BYK-052 on improving dispersibility, workability and water resistance.
[0051] The test methods are shown in Table 1 below:
[0052] The performance test results of the examples are shown in Tables 2 and 3 below: Table 2:
[0053] Table 3:
[0054] The comparative performance tests are shown in Table 4 below:
[0055] According to the GB / T2793-2015 standard, the VOC values of all examples were within the range of 7.6-8.3 g / L, and the VOC values of comparative examples 1-7 were also maintained in the range of 7.9-8.1 g / L, all meeting the core indicator of solvent-free coatings with VOC ≤10 g / L. This result demonstrates that while improving other properties of the adhesive through component optimization, its solvent-free characteristics remain stable, fundamentally avoiding the environmental pollution and health risks caused by solvent evaporation during construction and use of solvent-based anticorrosive adhesives. This lays an environmentally friendly foundation for subsequent performance optimization and aligns with the current development trend of environmentally friendly anticorrosive materials.
[0056] Adhesion Performance: Adhesion is crucial for ensuring a long-term stable bond between the anti-corrosion adhesive and the substrate, and for achieving its anti-corrosion effect. Test data shows that this adhesive, through its component design, achieves a dual improvement in adhesion to both metallic and non-metallic substrates. Regarding adhesion to metallic substrates (Q235 steel sheets), Comparative Example 1, without KH550, exhibited a metal adhesion of only 2.2 MPa; while Examples 1-3, with the addition of KH550, saw their metal adhesion increase to 4.8-5.3 MPa, clearly demonstrating the enhancing effect of KH550 on interfacial bonding. Further comparison shows that Comparative Example 3, using ordinary HTPB, had a metal adhesion of 5.2 MPa, while Examples 7-9, using KH550-modified HTPB, saw their metal adhesion increase to 6.8-7.3 MPa. This indicates that after modification with KH550, the molecular chains of HTPB can form stronger chemical bonds with the metal surface, further enhancing adhesion. The final example, Example 21, achieved a metal adhesion of 7.6 MPa, a 2.45-fold increase compared to Comparative Example 1, meeting the adhesion requirements for corrosion protection of high-strength metal substrates. Regarding adhesion to non-metallic substrates (C30 concrete blocks), Comparative Example 5, without the addition of cashew phenol-modified epoxy resin and KH560, showed a concrete adhesion of only 2.7 MPa. However, after introducing this compound system in Examples 13-21, the concrete adhesion increased to 5.6-6.4 MPa, with Example 21 achieving 6.4 MPa, a 1.37-fold increase compared to Comparative Example 5. This is because the polar groups of the cashew phenol-modified epoxy resin can form hydrogen bonds with the hydroxyl groups on the concrete surface, and KH560, as a silane coupling agent, can further bridge the organic adhesive and inorganic concrete. The synergistic effect of these two components achieves a significant improvement in adhesion to non-metallic substrates, making the adhesive suitable for various substrates such as metal, concrete, and fiberglass, greatly expanding its application scenarios.
[0057] Salt spray resistance: Salt spray resistance directly determines the application capability of anti-corrosion adhesives in marine and high-salt-spray industrial environments. Test data shows that this adhesive material achieves a significant improvement in salt spray resistance through component synergy. Comparative Example 2, using ordinary zinc powder without BTA, had a salt spray resistance time of only 980 hours. In Examples 4-6, after replacing ordinary zinc powder with nano-zinc-aluminum alloy powder (particle size 50nm, Al content 30%) and adding BTA, the salt spray resistance time jumped to 1450-1550 hours, an improvement of over 48%. This is because the nano-sized particles of the nano-zinc-aluminum alloy powder can form a dense protective layer, the addition of Al element can enhance the stability of the passivation film, and BTA, as a corrosion inhibitor, can further inhibit the corrosion of the metal substrate. The three together construct a basic anti-corrosion system. With further optimization of the formulation, such as the introduction of components like KH550-modified HTPB, MDI-polyether prepolymer, and cashew phenol-modified epoxy resin, the salt spray resistance time continued to improve: the salt spray resistance time of Example 12 reached 1650 hours, and the salt spray resistance times of Examples 18 and 21 both reached 1700 hours, an improvement of 73.5% compared to Comparative Example 2. This change indicates that a significant synergistic anti-corrosion effect was formed among the components—modified HTPB can improve the density of the adhesive film, the prepolymer can enhance the elasticity of the adhesive film to resist stress cracking under salt spray conditions, and cashew phenol-modified epoxy resin can improve the interfacial bonding stability. These effects together extend the salt spray erosion path and significantly enhance the long-term anti-corrosion effect of the adhesive material.
[0058] Elasticity: Elasticity is a key performance characteristic of anti-corrosion adhesives in responding to thermal expansion and contraction, vibration, and other conditions on the substrate. This adhesive achieves an effective balance of elasticity over a wide temperature range through prepolymer component optimization. Comparative Example 4, without the addition of MDI-polyether prepolymer, has an elongation at break of 285% at -40℃. Examples 10-12, after introducing MDI-polyether prepolymer, show an increase in elongation at break of 310-325% at -40℃, exceeding 10%. This is because the flexible segments of the polyether polyol maintain molecular chain mobility at low temperatures, preventing the adhesive film from becoming brittle due to low temperatures, thus meeting the application requirements in cold regions. Examples 16-18, using a compound prepolymer of PTMG (polytetrahydrofuran ether diol) and PCL (polycaprolactone diol), maintain an elongation at break of 275-285% at -40℃, while achieving a Shore A hardness of 61-64 at 80℃, demonstrating greater stability in high-temperature hardness compared to the single polyether prepolymer formulation of Examples 10-12. This is because PTMG provides excellent low-temperature elasticity, while PCL can adjust high-temperature hardness through crystallinity. The synergistic effect of the two achieves a wide-temperature performance balance of elasticity without brittleness at -40℃ and hardness without softening at 80℃, allowing the adhesive to adapt to application scenarios in different temperature environments. In addition, after introducing cashew phenol-modified epoxy resin in Examples 13-15, the elongation at break at -40℃ is 245-255%, which is lower than that of the purely elastic optimized formulation, i.e., Examples 10-12, but still meets the industrial elasticity requirements. At the same time, it significantly improves the adhesion to concrete, indicating that the formulation design achieves a performance balance between elasticity and adhesion, rather than pursuing only one indicator.
[0059] Storage stability: Storage stability directly affects the performance of the anti-corrosion adhesive, and sedimentation rate is a core indicator for evaluating storage stability. Test data shows that the adhesive effectively improved storage stability through component optimization. Comparative Examples 1 and 2, using ordinary zinc powder, achieved a sedimentation rate of 7.5-7.9%; Examples 4-6, using nano-zinc-aluminum alloy powder and adding BTA, reduced the sedimentation rate to 3.0-3.5%, a decrease of over 56%. This is because nano-sized powders have a larger specific surface area and better dispersibility than ordinary zinc powder. BTA can further improve the compatibility between the powder and the base material, thereby reducing sedimentation. Examples 19-21, using MPEG (methoxy polyethylene glycol) modified nano-zinc-aluminum alloy powder and adding BYK-052 dispersant, further reduced the sedimentation rate to 1.3-1.8%, a further reduction of 43-63% compared to Examples 4-6. Compared with Comparative Example 7, which uses stearic acid modification (requiring high temperature to reduce viscosity), Examples 19-21 can achieve low sedimentation without high temperature treatment. This shows that MPEG can provide steric hindrance through surface grafting, and BYK-052 can enhance dispersibility through charge stabilization. The two work together to solve the industry problem of easy agglomeration and sedimentation of nanoparticles, and significantly extend the storage period of the adhesive.
[0060] Application Performance: Application viscosity directly affects the ease of application of the anti-corrosion adhesive. This adhesive material gradually reduces viscosity through component optimization, thereby improving application performance. Comparative Examples 1 and 2 have viscosities of 10000-10200 mPa·s at 25°C, making application difficult. With formulation optimization, the viscosity of the examples gradually decreases: the viscosity of Example 12 at 25°C drops to 8800 mPa·s, and the viscosity of Example 18 at 25°C drops to 6600 mPa·s, which already meets the requirements of conventional application methods such as brushing and roller coating. After adding MPEG and BYK-052 to Examples 19-21, the viscosity at 25°C further decreases to 6200-6800 mPa·s, and no high-temperature viscosity reduction is required (unlike Comparative Example 7, which requires high-temperature viscosity reduction). This not only reduces application energy consumption but also avoids potential damage to the substrate from high temperatures, significantly improving application convenience and applicability.
[0061] Water resistance: The 30-day water immersion weight loss rate reflects the long-term water resistance of the anti-corrosion adhesive. Test data shows that the adhesive achieves improved water resistance through the synergistic effect of multiple components. The 30-day water immersion weight loss rate of Comparative Examples 1 and 2 was 0.32-0.36%; the 30-day water immersion weight loss rate of Examples 4-6 decreased to 0.17-0.22%, and the 30-day water immersion weight loss rate of Example 21 further decreased to 0.16%, a reduction of over 55%. This is because the dense protective layer formed by the nano-zinc-aluminum alloy powder can hinder the penetration of water molecules, KH550 modified HTPB can enhance the cross-linking density of the adhesive film, and MPEG and BYK-052 can improve interfacial compatibility. The synergistic effect of these components reduces the erosion and swelling of the adhesive film by water, ensuring the long-term waterproof and anti-corrosion effect of the adhesive, making it suitable for applications in humid and underwater environments.
[0062] The test results show that this solvent-free, salt spray resistant, highly adhesive, and corrosion-resistant elastic adhesive has achieved multi-dimensional performance breakthroughs through a technical path of core functional component selection, synergistic design, and performance balance optimization. Furthermore, this adhesive is not simply a combination of components; rather, it addresses the pain points of existing technologies, such as insufficient adhesion, poor salt spray resistance, severe powder settling, and high construction difficulty, by constructing multiple synergistic systems including KH550 modified HTPB, nano-zinc-aluminum alloy powder + BTA, MDI-PTMG-PCL prepolymer, cashew phenol modified epoxy resin + KH560, and MPEG + BYK-052. The performance improvements are significant, far exceeding the performance of the comparative example. In terms of practicality, all performance indicators are designed around actual application needs: solvent-free properties adapt to environmental protection requirements, high adhesion adapts to multiple substrates, high salt spray resistance adapts to marine / high salt environments, wide temperature range adapts to temperature fluctuation scenarios, low settling rate adapts to long-term storage, low viscosity adapts to convenient construction, and low water weight loss rate adapts to humid environments. It can be widely used in fields such as industrial equipment corrosion protection, marine engineering protection, and waterproofing and corrosion protection of building concrete, and has clear and important practical application value.
[0063] In summary, the performance test results of this solvent-free, salt spray resistant, universally adhesive, and corrosion-resistant elastic adhesive fully demonstrate its technological advancement and application feasibility, providing reliable technical support for industrial applications.
[0064] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.
Claims
1. A solvent-free, salt spray-resistant, universally adhesive, corrosion-resistant elastic adhesive, characterized in that, The ingredients are used in the following amounts by weight: KH550 modified HTPB 80, cashew phenol modified epoxy resin 15, MDI 9, PTMG 4, PCL 2, nano zinc-aluminum alloy powder 20, MPEG 0.8, BTA 1, ordinary carbon black 12, DOP 6, KH550 2, KH560 1, BYK-052 0.2, DBTDL 0.4; The nano-zinc-aluminum alloy powder has a particle size of 50 nm and an Al content of 30%. The PTMG has a number-average molecular weight of 1800, and the PCL has a number-average molecular weight of 1300; The number-average molecular weight of the MPEG is 1800; The cashew phenol-modified epoxy resin has an epoxy value of 0.20 eq / 100g; The ordinary carbon black is unmodified carbon black; The preparation method of KH550 modified HTPB is as follows: take 80 parts by weight of HTPB, 4 parts by weight of KH550, and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. The MDI, PTMG, and PCL are pre-reacted to form an MDI-PTMG-PCL prepolymer. The preparation method of the MDI-PTMG-PCL prepolymer is as follows: take 9 parts by weight of MDI, 4 parts by weight of PTMG, and 2 parts by weight of PCL, react at 75°C for 1.5 h, and the NCO content is 18%. The nano zinc-aluminum alloy powder is modified with MPEG. The modification method is as follows: take 20 parts by weight of nano zinc-aluminum alloy powder and 0.8 parts by weight of MPEG, and process them in a high-speed disperser at 5000 r / min for 20 min. MPEG is grafted onto the surface of the powder to provide steric hindrance.
2. A method for preparing a solvent-free, salt spray-resistant, highly adhesive, and corrosion-resistant elastic adhesive as described in claim 1, characterized in that, Includes the following steps: (1) First, KH550 modified HTPB is prepared. The preparation method is to take 80 parts by weight of HTPB, 4 parts by weight of KH550 and 0.2 parts by weight of DBTDL, react at 80℃ for 3h, detect the characteristic peak of Si-OC by infrared detection, and cool to 40℃ for later use. (2) Preparation of MDI-PTMG-PCL prepolymer: The preparation method is to take 9 parts by weight of MDI, 4 parts by weight of PTMG, and 2 parts by weight of PCL, react at 75℃ for 1.5h, and the NCO content is 18%; (3) Modified nano zinc-aluminum alloy powder. The modification method is to take 20 parts by weight of nano zinc-aluminum alloy powder and 0.8 parts by weight of MPEG, and process them in a high-speed disperser at 5000r / min for 20min. MPEG is grafted onto the surface of the powder to provide steric hindrance. (4) The modified HTPB and cashew phenol modified epoxy resin were stirred at 60°C for 20 min to form an interpenetrating network matrix, and the KH550 and KH560 compound system was added and kept at 40°C for 10 min. (5) The modified nano zinc-aluminum alloy powder was mixed and ground with BTA for 10 min to achieve particle size uniformity. The above interpenetrating network matrix, the ground nano zinc-aluminum alloy powder and BTA mixture, ordinary carbon black, DOP, and BYK-052 were added to the high-speed disperser. The ordinary carbon black was not modified. The dispersion was carried out at 3000 r / min for 15 min. The viscosity dropped to 6800 mPa·s at 25℃. High-temperature viscosity reduction was not required. (6) Cool down to 40°C, add DBTDL, and stir at 1500 r / min for 15 min; (7) Slowly add the prepared MDI-PTMG-PCL prepolymer, control the dropping rate to 7 mL / min, and stir at 2000 r / min for 25 min after the dropping is complete to obtain solvent-free salt spray resistant adhesive and corrosion resistant elastic adhesive.
3. An application of the solvent-free, salt spray-resistant, universally adhesive, corrosion-resistant elastic adhesive as described in claim 1, characterized in that, The solvent-free, salt spray-resistant, universally adhesive, and corrosion-resistant elastic adhesive is applied to the surface of a substrate and cured at room temperature for 24 hours to form a 0.5 mm thick film. The substrate is a Q235 steel sheet, a C30 concrete block, or a fiberglass substrate. The pretreatment method for the Q235 steel sheet is sandblasting to Sa2.5 grade and then wiping with ethanol. The pretreatment method for the C30 concrete block is sandblasting the surface to expose the aggregate and then wiping with ethanol. The pretreatment method for the fiberglass substrate is sanding to roughness and then wiping with ethanol.
Citation Information
Patent Citations
Zinc-aluminum anticorrosive paint as well as preparation method and coating process
CN109111776A
Primer-free single-component polyurethane sealant and preparation method thereof
CN111378413A